Optical glass and optical components

By controlling the composition ratio of optical glass, optical glass with low glass transition temperature and high refractive index was achieved, solving the adaptability problem of optical glass in precision pressing in the prior art and improving the performance of optical components.

CN117585898BActive Publication Date: 2026-11-17HOYA CORPORATION +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311013218.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2023-06-06
Filing Date
2023-08-10
Publication Date
2026-11-17
Estimated Expiration
2043-08-10

AI Technical Summary

Technical Problem

Existing optical glasses cannot simultaneously meet the requirements of high refractive index and low Abbe number, and their high glass transition temperature affects their suitability for precision pressing.

Method used

By controlling the composition of the optical glass, the Li2O content is ensured to be greater than 0% and within a specific range, the proportions of B2O3, SiO2, La2O3, ZnO and other components satisfy a specific relationship, the glass transition temperature Tg is less than 610℃, and the refractive index nd and Abbe number νd satisfy the relationship of equation (2).

Benefits of technology

Optical glass with low glass transition temperature and useful optical constants is provided, which is suitable for precision pressing and improves the performance of optical components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117585898B_ABST
    Figure CN117585898B_ABST
Patent Text Reader

Abstract

This invention provides optical glass with a refractive index and Abbe number satisfying a given formula and a low glass transition temperature. In the glass composition expressed as mass percent, the optical glass contains: Li₂O content greater than 0% by mass; B₂O₃ content greater than 3.00% by mass and less than 30.00% by mass; SiO₂ content greater than 0% by mass and less than 8.00% by mass; La₂O₃ content greater than 15.00% by mass and less than 55.00% by mass; ZnO content greater than 3.00% by mass and less than 30.00% by mass; TiO₂ content less than 0.60% by mass; and the total content of Li₂O and ZnO (Li₂O + ZnO). The optical glass has a content of 10.20% or more by mass, a B2O3 content to Li2O content mass ratio (B2O3 / Li2O) of 5.00 or more and 21.00 or less, a SiO2 content to Li2O content mass ratio (SiO2 / Li2O) of 10.00 or less, a glass transition temperature Tg of less than 610°C, a liquidus temperature LT of 1090°C or more, a refractive index nd and a glass transition temperature Tg satisfying the following equation (1), and a refractive index nd and an Abbe number νd satisfying the following equation (2). Equation (1): Tg < 2500*nd - 4050 Equation (2): νd > -88.355*nd + 201.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to optical glass and optical components. Background Technology

[0002] In recent years, various optical glasses have been proposed as materials for optical components (see, for example, Patent Document 1).

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 2008-201661 Summary of the Invention

[0006] The problem that the invention aims to solve

[0007] Optical glass with a refractive index and Abbe number that satisfy a given relationship is useful as a material for optical elements. For example, as a specific example of such a relationship, we can cite “Equation (2): νd>-88.355*nd+201”.

[0008] In addition, one of the desirable properties of optical glass is a low glass transition temperature (Tg). Low Tg glasses are preferred due to, for example, their excellent adaptability to precision pressing.

[0009] One embodiment of the present invention aims to provide an optical glass that satisfies the above formula (2) in terms of refractive index and Abbe number, and has a low glass transition temperature.

[0010] Problem Solving Methods

[0011] One embodiment of the present invention relates to an optical glass, wherein,

[0012] In the glass composition expressed as mass %

[0013] Li2O content exceeds 0% by mass.

[0014] The B2O3 content is above 3.00% by mass and below 30.00% by mass.

[0015] The SiO2 content is greater than 0% by mass and less than 8.00% by mass.

[0016] The La2O3 content is above 15.00% by mass and below 55.00% by mass.

[0017] The ZnO content is 3.00% by mass or more and 30.00% by mass or less.

[0018] The TiO2 content is below 0.60% by mass.

[0019] The total content of Li2O and ZnO (Li2O+ZnO) is 10.20% by mass or more.

[0020] The mass ratio of B2O3 content to Li2O content (B2O3 / Li2O) is 5.00 or higher and 21.00 or lower, and the mass ratio of SiO2 content to Li2O content (SiO2 / Li2O) is 10.00 or lower.

[0021] The glass transition temperature (Tg) of the optical glass is less than 610℃.

[0022] The liquidus temperature LT is above 1090℃.

[0023] The refractive index nd and the glass transition temperature Tg satisfy the following equation (1), and the refractive index nd and the Abbe number νd satisfy the following equation (2).

[0024] Equation (1): Tg < 2500*nd - 4050

[0025] Equation (2): νd>-88.355*nd+201.

[0026] The effects of the invention

[0027] According to one embodiment of the invention, optical glass with a low glass transition temperature and useful optical constants as a material for optical elements can be provided. Furthermore, according to another aspect of the invention, optical elements made from such optical glass can be provided. Attached Figure Description

[0028] Figure 1 A cross-sectional schematic diagram of a precision compression molding apparatus is shown. Detailed Implementation

[0029] Optical Glass

[0030] In this invention and this specification, the glass composition of the optical glass is described by mass % , cation % , or mole % .

[0031] In both mass % and mole % glass compositions, the glass composition is expressed using oxide-based glass composition. Here, "oxide-based glass composition" refers to the glass composition obtained by converting substances that exist in the glass as oxides after the glass raw material is completely decomposed during melting. In mass % glass compositions, the glass composition is expressed using mass basis (mass %), mass ratio. Hereinafter, for glass compositions expressed using mass % glass composition, "mass %" will also be simply referred to as "%". In mole % glass compositions, the glass composition is expressed using mole basis (mole %), molar ratio. Hereinafter, for glass compositions expressed using mole % glass composition, "mole %" will also be simply referred to as "%".

[0032] Regarding glass composition expressed as cation % (%, cation % represents the content and total content of cationic components), "cation %" is a value calculated as "(number of cations of interest / total number of cations in the glass composition) × 100", representing the molar percentage of the amount of cations of interest relative to the total amount of cationic components. Hereafter, for glass composition expressed as cation % (%, cation % will also be simply referred to as "%").

[0033] The cation ratio is the molar ratio of the content of each cationic component to the other, which is equal to the ratio of the content of the cationic component of interest expressed as cation %

[0034] Regarding cationic components, such as Li + Si 4+ This indicates the valence of the cation component (e.g., Li). + The valence is +1, Si 4+ The valence (+4) is a value determined by convention, similar to how Li, Si, etc., are represented as Li₂O, SiO₂, etc., using oxide references. Regarding the representation of A according to oxide references... m O n The composition (where A represents cation, O represents oxygen, and m and n are integers determined by stoichiometry) is represented by cation A as A s+ Where s = 2n / m. Therefore, for example, when analyzing and quantifying the composition of glass, it is not necessary to analyze the valence of the cationic components.

[0035] In this invention and this specification, the content of a constituent element is 0%, 0.0%, or 0.00%, or it is not present or introduced, indicating that the constituent element is substantially not contained, meaning that the content of the constituent element is below the level of impurities. Below the level of impurities means, for example, less than 0.01%. "0%" can, for example, mean "0.0%" or "0.00%".

[0036] The glass composition described in this invention and specification can be determined using methods such as ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). For example, quantitative analysis uses ICP-AES, analyzing each element separately. The analytical values ​​are then converted to oxide representations. ICP-AES-based analytical values ​​sometimes contain, for example, a measurement error of approximately ±5% of the analytical value. Therefore, the oxide representations derived from the analytical values ​​sometimes also contain an error of approximately ±5%.

[0037] For the results of quantitative analysis of glass composition, the composition expressed as mass % based on oxides can be converted into glass composition expressed as cation % by, for example, the method described below.

[0038] When a glass contains N glass components, the k-th glass component is denoted as A(k). m O n Where k is any integer greater than 1 and less than N.

[0039] A(k) represents a cation, O represents oxygen, and m and n are integers that can be determined stoichiometrically. For example, in the case of B2O3 as an oxide reference, m = 2 and n = 3, and in the case of SiO2, m = 1 and n = 2.

[0040] Next, A(k) m O n The content is set as X(k) [mass%). Here, when the atomic weight of A(k) is set as P(k) and the atomic number of oxygen O is set as Q, A(k) m O n The molecular weight R(k) in formal form is R(k) = P(k) × m + Q × n.

[0041] Furthermore, let's assume that when B = 100 / {Σ[m×X(k) / R(k)]}, the cation component A(k) s+ The content (cation %) is [X(k) / R(k)]×m×B (cation %). Here, Σ represents the sum of m×X(k) / R(K) from k = 1 to N. m varies depending on k. s is 2n / m.

[0042] Additionally, for the molecular weight R(k), round to the fourth decimal place and use the value expressed to the third decimal place for calculation. It should be noted that the molecular weights of several glass components and additives, written in oxide-based format, are shown in Table 1 below.

[0043] Table 1

[0044] oxides molecular weight oxides molecular weight <![CDATA[B2O3]]> 69.621 <![CDATA[Cs2O]]> 281.810 <![CDATA[SiO2]]> 60.084 ZnO 81.389 <![CDATA[La2O3]]> 325.809 MgO 40.304 <![CDATA[Y2O3]]> 225.810 CaO 56.077 <![CDATA[Gd2O3]]> 362.498 SrO 81.389 <![CDATA[Yb2O3]]> 394.084 BaO 153.326 <![CDATA[Nb2O5]]> 265.810 <![CDATA[Al2O3]]> 101.961 <![CDATA[TiO2]]> 79.882 <![CDATA[Ga2O3]]> 187.444 <![CDATA[WO3]]> 231.839 <![CDATA[In2O3]]> 277.634 <![CDATA[Ta2O5]]> 441.893 <![CDATA[Sc2O3]]> 137.910 <![CDATA[Bi2O3]]> 465.959 <![CDATA[HfO2]]> 210.489 <![CDATA[ZrO2]]> 123.223 <![CDATA[Lu2O3]]> 397.932 <![CDATA[Li2O]]> 29.882 <![CDATA[GeO2]]> 104.629 <![CDATA[Na2O]]> 61.979 <![CDATA[P2O5]]> 141.945 <![CDATA[K2O]]> 94.196 <![CDATA[TeO2]]> 159.599 <![CDATA[Rb2O]]> 186.935 <![CDATA[Sb2O3]]> 291.518

[0045] In this invention and this specification, the refractive index refers to the refractive index nd under helium d rays (wavelength 587.56 nm).

[0046] In this invention and this specification, the Abbe number νd is used as a value representing a property related to dispersion, and is expressed by the following mathematical formula.

[0047] νd=(nd-1) / (nF-nC)

[0048] In the above formula, nF is the refractive index under F-rays of blue hydrogen (wavelength 486.13 nm), and nC is the refractive index under C-rays of red hydrogen (656.27 nm).

[0049] The optical glass (sometimes simply referred to as "glass") described above will be explained in more detail below.

[0050] <Glass Composition>

[0051] (Li₂O, Li) + )

[0052] Li (Li₂O in glass composition expressed as mass% or mole% and Li₂O in glass composition expressed as cation%) + It is a component that can suppress the decrease in refractive index and lower the glass transition temperature, therefore, it must be contained in the above-mentioned optical glass.

[0053] In the glass composition expressed as mass % , the Li2O content is more than 0%, preferably 0.20% or more, and further preferably in the order of 0.30% or more, 0.40% or more, 0.45% or more, 0.50% or more, 0.55% or more, 0.60% or more, 0.62% or more, 0.64% or more, 0.66% or more, 0.68% or more, 0.70% or more, 0.72% or more, 0.74% or more, 0.76% or more, 0.77% or more, 0.78% or more, 0.79% or more, 0.80% or more, 0.81% or more, 0.82% or more, and 0.83% or more.

[0054] There is no particular upper limit to the Li2O content. For example, it can be below 1.80%, preferably below 1.70%, and further preferably in the order of below 1.60%, below 1.55%, below 1.50%, below 1.48%, below 1.46%, below 1.44%, below 1.42%, below 1.40%, below 1.38%, below 1.36%, below 1.34%, below 1.32%, and below 1.31%.

[0055] In the glass composition expressed as cations%, Li + The content exceeds 0%, preferably 0.50% or more, and further preferred in the order of 1.00% or more, 1.50% or more, 2.00% or more, 2.50% or more, 3.00% or more, 3.25% or more, 3.50% or more, 3.75% or more, 4.00% or more, 4.25% or more, 4.50% or more, 4.75% or more, and 5.00% or more.

[0056] Li + There is no particular upper limit to the content, for example, it can be below 12.00%, preferably below 11.00%, and further preferably in the order of below 10.50%, below 10.00%, below 9.75%, below 9.50%, below 9.25%, below 9.00%, below 8.75%, below 8.50%, below 8.25%, and below 8.00%.

[0057] In the glass composition expressed in mole % , the Li2O content is more than 0%, preferably 0.50% or more, and further preferred in the order of 1.00% or more, 1.50% or more, 2.00% or more, 2.50% or more, 3.00% or more, 3.10% or more, 3.30% or more, 3.50% or more, 3.70% or more, and 3.91% or more.

[0058] There is no particular upper limit to the Li2O content. For example, it can be 11.00% or less, preferably 10.00% or less, and further preferred in the order of 9.50% or less, 9.00% or less, 8.50% or less, 8.00% or less, 7.50% or less, 7.30% or less, 7.10% or less, 6.90% or less, 6.70% or less, and 6.51% or less.

[0059] (B2O3)

[0060] B2O3 is a network-forming component that helps maintain the thermal stability and melt permeability of glass. Therefore, in the glass composition expressed as a percentage by mass, the B2O3 content is 3.00% or more, preferably 5.00% or more, and further preferably in the order of 6.00% or more, 7.00% or more, 8.00% or more, 8.50% or more, 9.00% or more, 9.50% or more, 10.00% or more, 10.50% or more, and 10.83% or more.

[0061] B2O3 is also a component that leads to a low refractive index in glass when present in large quantities. Therefore, in the glass composition expressed as mass %, the B2O3 content is 30.00% or less, preferably 29.00% or less, and further preferably in the order of 28.00% or less, 27.00% or less, 26.00% or less, 25.00% or less, 24.00% or less, 23.00% or less, 22.00% or less, 21.00% or less, 20.00% or less, 19.00% or less, 18.00% or less, 17.00% or less, 16.00% or less, 15.50% or less, 15.00% or less, 14.50% or less, 14.00% or less, and 13.78% or less.

[0062] (SiO2)

[0063] SiO2 is also a network-forming component, which helps maintain the thermal stability and melt flowability of glass. From this perspective, in the glass composition expressed as a percentage by mass, the SiO2 content is more than 0%, preferably 0.50% or more, and further preferably in the order of 1.00% or more, 1.50% or more, 2.00% or more, 2.25% or more, 2.50% or more, 2.75% or more, 2.80% or more, 2.85% or more, 2.90% or more, 2.95% or more, 3.00% or more, 3.02% or more, 3.04% or more, and 3.06% or more.

[0064] SiO2 is also a component that leads to a low refractive index in glass when present in large quantities. Therefore, in the glass composition expressed as mass % the SiO2 content is 8.00% or less, preferably 7.50% or less, more preferably 7.00% or less, and further preferably in the order of 6.75% or less, 6.50% or less, 6.25% or less, 6.00% or less, 5.75% or less, and 5.60% or less.

[0065] (B2O3 / Li2O)

[0066] In the glass composition expressed as a percentage by mass, the mass ratio of B2O3 content to Li2O content (B2O3 / Li2O) is 5.00 or more, preferably 5.50 or more, and further preferably in the order of 6.00 or more, 6.20 or more, 6.40 or more, 6.60 or more, 6.80 or more, 7.00 or more, 7.20 or more, 7.40 or more, 7.60 or more, 7.80 or more, 8.00 or more, 8.25 or more, and 8.36 or more. Regarding the upper limit, it is 21.00 or less, preferably 20.00 or less, and further preferably in the order of 19.50 or less, 19.00 or less, 18.50 or less, 18.00 or less, 17.75 or less, 17.50 or less, 17.25 or less, 17.00 or less, 16.75 or less, and 16.54 or less.

[0067] Regarding the mass ratio (B2O3 / Li2O), from the viewpoint of lowering the glass transition temperature, the upper limit mentioned above is preferred, and from the viewpoint of suppressing the rise in glass transition temperature and maintaining thermal stability, the lower limit mentioned above is preferred.

[0068] In the glass composition expressed as cations%, B 3+ Content relative to Li + The ratio of cations in the content (B) 3+ / Li + The preferred value is 1.50 or higher, with further preferred values ​​in the order of 2.00 or higher, 2.25 or higher, 2.50 or higher, 2.75 or higher, 3.00 or higher, 3.25 or higher, 3.50 or higher, and 3.58 or higher. Regarding the upper limit, the preferred value is 9.50 or lower, with further preferred values ​​in the order of 9.00 or lower, 8.80 or lower, 8.60 or lower, 8.40 or lower, 8.20 or lower, 8.00 or lower, 7.80 or lower, 7.60 or lower, 7.40 or lower, 7.20 or lower, and 7.10 or lower.

[0069] (B 3+ / Si 4+ )

[0070] In the glass composition expressed as cations%, B 3+ Content relative to Si 4+ The ratio of cations in the content (B) 3+ / Si 4+ The preferred value is 1.25 or higher, and it is further preferred in the following order: 1.50 or higher, 1.75 or higher, 2.00 or higher, 2.25 or higher, 2.50 or higher, 2.75 or higher, 3.00 or higher, 3.10 or higher, 3.20 or higher, 3.30 or higher, 3.40 or higher, and 3.50 or higher.

[0071] In addition, the cation ratio (B 3+ / Si 4+ Preferably, the value is 11.00 or less, and further preferred in the order of 10.50 or less, 10.00 or less, 9.75 or less, 9.50 or less, 9.25 or less, 9.00 or less, 8.75 or less, 8.50 or less, 8.25 or less, 8.00 or less, 7.75 or less, 7.60 or less, 7.50 or less, 7.40 or less, and 7.30 or less.

[0072] From the perspective of maintaining the thermal stability and high refractive index characteristics of glass, the cation ratio (B... 3+ / Si 4+ The preferred range is the one described above.

[0073] In the glass composition expressed as a percentage by mass, the mass ratio of B2O3 content to SiO2 content (B2O3 / SiO2) is preferably 0.25% or more, and further preferably in the order of 0.50 or more, 0.75 or more, 1.00 or more, 1.20 or more, 1.40 or more, 1.60 or more, 1.70 or more, 1.80 or more, 1.90 or more, 2.00 or more, and 2.02 or more. Regarding the upper limit, it is preferably 9.00 or less, and further preferably in the order of 8.50 or less, 8.00 or less, 7.50 or less, 7.00 or less, 6.50 or less, 6.00 or less, 5.75 or less, 5.50 or less, 5.25 or less, 5.00 or less, 4.75 or less, 4.50 or less, and 4.23 or less.

[0074] (SiO2 / Li2O)

[0075] In the glass composition expressed as a percentage by mass, the mass ratio of SiO2 content to Li2O content (SiO2 / Li2O) is 10.00 or less, preferably 9.00 or less, and further preferably in the order of 8.50 or less, 8.00 or less, 7.50 or less, 7.00 or less, 6.75 or less, 6.50 or less, 6.25 or less, 6.00 or less, 5.75 or less, 5.50 or less, 5.25 or less, and 5.18 or less. Regarding the lower limit, it can exceed 0, preferably 0.40 or more, and further preferably in the order of 0.60 or more, 0.80 or more, 1.00 or more, 1.20 or more, 1.40 or more, 1.60 or more, 1.80 or more, 2.00 or more, 2.25 or more, 2.50 or more, and 2.68 or more.

[0076] Regarding the mass ratio (SiO2 / Li2O), from the viewpoint of lowering the glass transition temperature, the upper limit mentioned above is preferred, and from the viewpoint of suppressing the rise in glass transition temperature and maintaining thermal stability, the lower limit mentioned above is preferred.

[0077] In the glass composition expressed as cations%, Si 4+ Content relative to Li + The ratio of cations in Si 4+ / Li +The lower limit can be below 2.40, preferably in the following order: below 2.30, below 2.20, below 2.10, below 2.00, below 1.90, below 1.80, below 1.70, below 1.65, below 1.60, below 1.55, below 1.50, below 1.48, below 1.46, below 1.44, below 1.42, below 1.40, below 1.38, below 1.36, below 1.34, below 1.32, below 1.30, and below 1.29. Regarding the lower limit, it can exceed 0, preferably in the following order: above 0.25, above 0.30, above 0.35, above 0.40, above 0.50, above 0.52, above 0.54, above 0.56, above 0.58, above 0.60, above 0.62, above 0.64, and above 0.66.

[0078] (Rare earth components)

[0079] La2O3

[0080] In the glass composition expressed as mass % , the La2O3 content is 15.00% or more, preferably 17.00% or more, and further preferably in the order of 20.00% or more, 21.00% or more, 22.00% or more, 23.00% or more, 24.00% or more, 25.00% or more, 26.00% or more, 26.50% or more, 27.00% or more, 27.50% or more, 28.00% or more, and 28.35% or more.

[0081] In the glass composition expressed as mass % , the La2O3 content is 55.00% or less, preferably 50.00% or less, and further preferably in the order of 47.00% or less, 45.00% or less, 44.00% or less, 43.00% or less, 42.00% or less, 41.00% or less, 40.00% or less, 39.50% or less, 39.00% or less, 38.50% or less, 38.00% or less, 37.50% or less, and 37.22% or less.

[0082] Gd2O3

[0083] In the glass composition expressed as a percentage by mass, the Gd₂O₃ content can be 0%, 0% or more, or more than 0%, preferably in the order of 0.00% or more, 0.20% or more, 0.40% or more, 0.60% or more, and 0.80% or more. Regarding the upper limit, it is preferably 15.00% or less, and further preferably in the order of 14.75% or less, 14.50% or less, 14.25% or less, 14.00% or less, 13.85% or less, 13.75% or less, 13.50% or less, 13.25% or less, 13.00% or less, 12.75% or less, 12.55% or less, 12.25% or less, and 12.03% or less.

[0084] Y2O3

[0085] In the glass composition expressed as a percentage by mass, the Y2O3 content can be 0%, more than 0%, or more than 0%. Regarding the upper limit, it is preferably 11.00% or less, and further preferred in the order of 10.50% or less, 10.00% or less, 9.50% or less, 9.00% or less, 8.50% or less, 8.00% or less, 7.50% or less, 7.04% or less, 6.50% or less, 6.00% or less, and 5.84% or less.

[0086] Regarding rare earth elements, La, Gd, and Y are components that can maintain low dispersibility and increase the refractive index. From the viewpoint of maintaining or improving thermal stability, the contents of each rare earth oxide are preferably within the ranges mentioned above. Compared with Gd, which is also a rare earth element, Y has a smaller effect on increasing the refractive index. In addition, when the total content of rare earth elements is excessive, it tends to reduce the thermal stability of the glass. Therefore, from the viewpoint of maintaining thermal stability and high refractive index characteristics, La and / or Gd are more preferred as rare earth elements than Y.

[0087] (Lu2O3 / (La2O3+Gd2O3+Y2O3+Lu2O3))

[0088] From the viewpoint of maintaining thermal stability, a lower proportion of Lu in the total rare earth components is preferred, and Lu-free is even more preferred. Therefore, in the glass composition expressed as a percentage by mass, the mass ratio of Lu2O3 content to the total content of La2O3, Gd2O3, Y2O3, and Lu2O3 (Lu2O3 / (La2O3+Gd2O3+Y2O3+Lu2O3)) is preferably 0.50 or less, more preferably in the order of 0.40 or less, 0.30 or less, 0.20 or less, and 0.10 or less, and even more preferably, Lu-free is preferred. 3+ (Therefore, the above mass ratio is zero).

[0089] (ZnO)

[0090] In the glass composition expressed as mass % , the ZnO content is 3.00% or more, preferably 3.50% or more, and further preferably in the order of 4.00% or more, 4.50% or more, 5.00% or more, 5.25% or more, 5.50% or more, 5.75% or more, 6.00% or more, 6.25% or more, 6.50% or more, 6.75% or more, 7.00% or more, 7.25% or more, 7.53% or more, 7.75% or more, 8.00% or more, 8.25% or more, 8.50% or more, 8.75% or more, 9.00% or more, 9.10% or more, 9.20% or more, and 9.30% or more. Regarding the upper limit, it is 30.00% or less, preferably 27.00% or less, and further preferred in the order of 25.00% or less, 23.00% or less, 22.00% or less, 21.00% or less, 20.00% or less, 19.50% or less, 19.00% or less, 18.50% or less, 17.00% or less, 16.75% or less, 16.50% or less, 16.25% or less, 16.00% or less, 15.75% or less, and 15.65% or less.

[0091] Zn is a component that suppresses the decrease in refractive index, lowers the glass transition temperature, and improves meltability. On the other hand, when it is present in excess, the liquidus temperature increases, and the thermal stability of the glass decreases. From these perspectives, the ZnO content is preferably within the range described above.

[0092] (Li₂O+ZnO)

[0093] From the viewpoint of achieving a low Tg, the total content of Li2O and ZnO (Li2O+ZnO) in the glass composition expressed as mass% is 10.20% or more, preferably 10.22% or more, 10.30% or more, 10.40% or more, and further preferably in the order of 10.60% or more and 10.79% or more. Regarding the upper limit, from the viewpoint of the thermal stability of the glass, it is preferably 21.00% or less, and further preferably in the order of 20.00% or less, 19.50% or less, 19.00% or less, 18.50% or less, 18.00% or less, 17.75% or less, 17.50% or less, 17.25% or less, 17.00% or less, and 16.79% or less.

[0094] (TiO2)

[0095] Ti is a component that increases the refractive index and improves dispersion. However, if excessive Ti is introduced, it reacts with the forming surface of the mold during pressing, tending to deteriorate the surface quality of the glass, and sometimes the coloration of the glass becomes stronger. Furthermore, from the viewpoint of suppressing the deterioration of the release film (described later), it is preferable to have no Ti or very little Ti. From these viewpoints, in the glass composition expressed as a percentage by mass, the TiO2 content is 0.60% or less, preferably 0.40% or less, more preferably 0.30%, 0.20%, or 0.10% or less, and even more preferably 0% (i.e., not contained).

[0096] (Ta2O5)

[0097] Ta is a component that maintains high refractive index, low dispersion, and thermal stability. Therefore, in the glass composition expressed as mass % , the Ta2O5 content is preferably 7.00% or more, and further preferred in the order of 7.50% or more, 8.00% or more, 8.50% or more, 8.75% or more, 9.00% or more, 9.25% or more, 9.50% or more, 9.75% or more, 10.00% or more, 10.25% or more, and 10.43% or more. There is no particular limitation on the upper limit; for example, it can be 19.00% or less, preferably 18.00% or less, and further preferred in the order of 17.50% or less, 17.00% or less, 16.50% or less, 16.00% or less, 15.75% or less, 15.50% or less, 15.25% or less, 15.00% or less, and 14.92% or less.

[0098] (Nb2O5)

[0099] Nitrogen (Nb) is a component that increases the refractive index of glass; however, excessive Nb content tends to reduce the thermal stability of the glass. In the glass composition expressed as a percentage by mass, the Nb₂O₅ content can be 0%, 0% or more, or more than 0%, preferably in the order of 0% or more, 0.10% or more, 0.20% or more, 0.30% or more, 0.40% or more, 0.50% or more, and 0.60% or more. Regarding the upper limit, it is preferably 9.00% or less, and further preferably in the order of 8.00% or less, 7.50% or less, 7.00% or less, 6.50% or less, 6.00% or less, 5.80% or less, 5.60% or less, 5.40% or less, and 5.24% or less.

[0100] (ZrO2)

[0101] In the glass composition expressed as a percentage by mass, the ZrO2 content can be 0%, 0% or more, or more than 0%, preferably in the order of 0.00% or more, 0.50% or more, 1.00% or more, 1.20% or more, 1.40% or more, 1.60% or more, 1.80% or more, and 1.90% or more. Regarding the upper limit, it is preferably 10.00% or less, and further preferably in the order of 9.00% or less, 8.50% or less, 8.00% or less, 7.50% or less, 7.00% or less, 6.80% or less, 6.60% or less, 6.40% or less, 6.20% or less, 6.00% or less, and 5.90% or less. By introducing Zr into the glass, the effect of improving the thermal stability of the glass can be obtained without reducing the refractive index of the glass; therefore, the introduction of Zr is preferred.

[0102] (WO3)

[0103] In the glass composition expressed as a percentage by mass, the WO3 content can be 0%, 0% or more, or more than 0%, preferably in the order of 0% or more, 1.00% or more, 2.00% or more, 2.50% or more, 3.00% or more, 3.50% or more, 4.00% or more, 4.20% or more, 4.40% or more, 4.60% or more, 4.80% or more, and 4.93% or more. Regarding the upper limit, it is preferably 21.00% or less, preferably in the order of 20.00% or less, 19.00% or less, 18.50% or less, 18.00% or less, 17.80% or less, 17.60% or less, 17.40% or less, 17.20% or less, 17.00% or less, 16.80% or less, and 16.66% or less. WO3 is a component that improves the thermal stability and meltability of glass and increases its refractive index. On the other hand, when a large amount is included, the dispersion becomes higher and the adaptability to precision pressing decreases; therefore, fewer inclusions are preferred.

[0104] (Nb2O5+TiO2+WO3) / (SiO2+B2O3)

[0105] In the glass composition expressed as a percentage by mass, the mass ratio of the total content of Nb₂O₅, TiO₂, and WO₃ to the total content of SiO₂ and B₂O₃ (Nb₂O₅+TiO₂+WO₃) / (SiO₂+B₂O₃) is preferably 0.40 or more, and further preferred in the order of 0.45 or more, 0.50 or more, 0.56 or more, 0.57 or more, 0.58 or more, 0.59 or more, 0.60 or more, 0.61 or more, 0.62 or more, and 0.63 or more. Regarding the upper limit, it is preferably 1.60 or less, and further preferred in the order of 1.40 or less, 1.35 or less, 1.30 or less, 1.28 or less, 1.26 or less, 1.24 or less, 1.22 or less, 1.20 or less, 1.19 or less, 1.18 or less, 1.17 or less, 1.16 or less, 1.15 or less, and 1.14 or less.

[0106] Regarding the mass ratio (Nb2O5+TiO2+WO3) / (SiO2+B2O3), from the viewpoint of maintaining the high refractive index characteristics of the glass, the lower limit mentioned above is preferred, and from the viewpoint of maintaining thermal stability, the upper limit mentioned above is preferred.

[0107] (ZnO / WO3)

[0108] In the glass composition expressed as a percentage by mass, the mass ratio of ZnO content to WO3 content (ZnO / WO3) is preferably 0.10 or more, and further preferably in the order of 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, 0.60 or more, 0.63 or more, 0.67 or more, 0.70 or more, 0.73 or more, and 0.76 or more. Regarding the upper limit, it is preferably 5.00 or less, and further preferably in the order of 4.80 or less, 4.60 or less, 4.40 or less, 4.20 or less, 4.00 or less, 3.80 or less, 3.60 or less, 3.40 or less, 3.20 or less, 3.00 or less, 2.80 or less, 2.60 or less, and 2.46 or less.

[0109] Regarding the mass ratio (ZnO / WO3), from the viewpoint of lowering the glass transition temperature and maintaining low dispersion, the lower limit mentioned above is preferred, and from the viewpoint of maintaining the high refractive index characteristics of the glass, the upper limit mentioned above is preferred.

[0110] (Sb2O3)

[0111] Sb is a component that functions as a clarifying agent. From the viewpoints of suppressing damage to the forming surface of the pressing die during precision pressing and suppressing glass coloration, a lower addition amount is preferred. Regarding the Sb₂O₃ content, in the glass composition expressed as a percentage by mass, the preferred values ​​are 0% or more, 0.01% or more, and 0.02% or more, expressed as an additive proportion (Sb₂O₃ content when the total mass of the glass components excluding Sb₂O₃ is set to 100% by mass). Furthermore, the preferred values ​​are 1.00% or less, 0.90% or less, 0.80% or less, 0.70% or less, 0.60% or less, and 0.50% or less.

[0112] (Anionic component)

[0113] The aforementioned optical glass can be oxide glass, which may contain O 2- As an anionic component. In this invention and this specification, the content of anionic components in a glass composition expressed as anion% is expressed as anion%. Here, "anion%" refers to the value calculated according to "(number of anions of interest / total number of anions in the glass composition) × 100", which is the molar percentage of the amount of anions of interest relative to the total amount of anionic components. In a glass composition expressed as anion%, O 2- The preferred content is 95.0% or more of anions, further preferred in the order of 97.0% or more of anions, 98.0% or more of anions, 99.0% or more of anions, 99.5% or more of anions, and 100% of anions. Considering the ease of volatilization during glass melting, F... - The content is preferably 0.1% or less of anions, more preferably 0% of anions (i.e., not containing F). For the results of quantitative analysis of the glass composition, the composition expressed in mass % according to oxides can be converted into the glass composition expressed in anion % by the method described above for converting the glass composition to cation %.

[0114] <Properties of Glass>

[0115] (Glass transition temperature Tg)

[0116] The aforementioned optical glass, by having the aforementioned glass composition, is able to have a low glass transition temperature (Tg). For example, from the viewpoint of suppressing the deterioration of the release film during precision molding and suppressing the consumption of molding dies, low Tg glass is preferred. The Tg of the aforementioned optical glass is below 610°C, preferably in the order of 608°C or less, 606°C or less, 604°C or less, 602°C or less, 600°C or less, 598°C or less, 596°C or less, 594°C or less, 592°C or less, and 590°C or less. The lower limit of Tg is not particularly limited, for example, it can be 530°C or more, preferably in the order of 540°C or more, 550°C or more, 555°C or more, 560°C or more, 565°C or more, and 570°C or more. The glass transition temperature (Tg) can be determined by the method described later.

[0117] (Equation (1))

[0118] In the above optical glass, the refractive index nd and the glass transition temperature Tg satisfy the following equation (1).

[0119] Equation (1): Tg < 2500*nd - 4050

[0120] By satisfying equation (1), the aforementioned optical glass can balance high refractive index characteristics and moldability. Generally speaking, there is a tendency for higher refractive index to have higher Tg. In contrast, equation (1) indicates that although the refractive index is high, the Tg is low.

[0121] The aforementioned optical glass preferably satisfies the following formula (1-1), more preferably satisfies the following formula (1-2), even more preferably satisfies the following formula (1-3), even more preferably satisfies the following formula (1-4), and even more preferably satisfies the following formula (1-5).

[0122] Equation (1-1): Tg < 2500*nd - 4060

[0123] Equation (1-2): Tg < 2500*nd - 4070

[0124] Equation (1-3): Tg < 2500*nd - 4080

[0125] Equation (1-4): Tg < 2500*nd - 4090

[0126] Equation (1-5): Tg < 2500*nd - 4100

[0127] (Equation (2))

[0128] In the above optical glass, the refractive index nd and Abbe number νd satisfy the following equation (2).

[0129] Equation (2): νd>-88.355*nd+201

[0130] Optical glass that satisfies the above equation (2) exhibits low dispersion at a given refractive index and is useful as a material for optical elements.

[0131] (Refractive index nd)

[0132] As long as equations (1) and (2) above are satisfied, the refractive index nd of the optical glass is not particularly limited. High refractive index glass is useful as a material for optical components. Therefore, the refractive index nd of the optical glass is preferably 1.8600 or higher, and is further preferred in the order of 1.8620 or higher, 1.8640 or higher, 1.8660 or higher, 1.8680 or higher, 1.8700 or higher, 1.8720 or higher, 1.8740 or higher, and 1.8760 or higher. Regarding the upper limit, it is preferably 1.9000 or lower, and is further preferred in the order of 1.8980 or lower, 1.8960 or lower, 1.8940 or lower, 1.8920 or lower, 1.8900 or lower, 1.8880 or lower, and 1.8860 or lower.

[0133] (Abbe number νd)

[0134] As long as equation (2) above is satisfied, the Abbe number νd of the optical glass is not particularly limited. Glass exhibiting low dispersion is useful as a material for optical elements. Therefore, the Abbe number νd of the optical glass is preferably 34.0 or higher, and is further preferred in the order of 34.20 or higher, 34.40 or higher, 34.60 or higher, 34.80 or higher, 35.00 or higher, 35.10 or higher, 35.20 or higher, 35.30 or higher, 35.40 or higher, 35.50 or higher, 35.60 or higher, 35.70 or higher, 35.80 or higher, 35.90 or higher, 36.00 or higher, 36.10 or higher, and 36.20 or higher. Regarding the upper limit, it is preferably below 40.0, and further preferred in the order of below 39.50, below 39.00, below 38.80, below 38.60, below 38.40, below 38.20, below 38.00, below 37.90, below 37.80, and below 37.76.

[0135] When considering glass as a material for optical elements, increasing the refractive index of the glass is equivalent to expanding the degrees of freedom possessed by the glass. From the viewpoint of expanding these degrees of freedom, increasing the refractive index is preferable. On the other hand, if dispersion is maintained and the refractive index is increased, there is a tendency for the stability of the glass to decrease. From these viewpoints, the Abbe number νd is preferably within the range described above.

[0136] (Liquid phase temperature LT)

[0137] As described above, the optical glass does not contain Ti, or contains a small amount of Ti. The optical glass described above, composed of glass that does not contain Ti, or contains a small amount of Ti, and has the desired Tg and optical constants described above, has a liquidus temperature LT of 1090°C or higher. The liquidus temperature LT can also be 1100°C or higher, 1110°C or higher, or 1120°C or higher. Regarding the upper limit, from the viewpoint of maintaining viscosity during molding, 1230°C or lower is preferred, and further preferred in the order of 1220°C or lower, 1210°C or lower, 1200°C or lower, 1190°C or lower, and 1180°C or lower.

[0138] In this invention and this specification, the liquid phase temperature LT is determined by the following method.

[0139] Place 5-8 cc of glass into a platinum crucible and heat in the furnace at an atmosphere temperature T for 2 hours until it reaches a molten state. Remove the glass from the furnace and allow it to cool to room temperature. Set the room temperature to a range of 20°C-30°C. Observe the glass using an optical microscope (100x magnification) to determine whether crystals have precipitated within the cooled glass.

[0140] For different temperatures (T) (in 10°C intervals), the presence or absence of crystallization was determined using the method described above. The lowest temperature at which no crystallization was observed was taken as the liquidus temperature.

[0141] (proportion)

[0142] From the viewpoint of lightweighting optical components, a low specific gravity of the optical glass is preferred. The specific gravity of the aforementioned optical glass is preferably 5.75 g / cc or less, and further preferred in the order of 5.70 g / cc or less, 5.65 g / cc or less, and 5.58 g / cc or less. However, the specific gravity of the aforementioned optical glass can be, for example, 5.10 g / cc or more; the lower the specific gravity, the more preferred, therefore, there is no particular limitation on the lower limit. In this invention and this specification, the specific gravity is set as a value measured by the Archimedes method.

[0143] (shading degree λ5, λ) 70 , λ 80 )

[0144] Regarding the light transmittance of glass, specifically the suppression of the long-wavelength absorption at the short-wavelength side, this can be achieved based on the tinting degree λ5, λ 70 and λ 80 The evaluation is based on one or more of the following: Colorimetric λ5 refers to the wavelength from the ultraviolet to the visible region where the spectral transmittance (including surface reflection loss) of a 10mm thick glass reaches 5%. 70 This indicates the wavelength at which the spectral transmittance reaches 70%, as measured by the method described for λ5. 80This indicates the wavelength at which the spectral transmittance reaches 80%, as measured by the method described for λ5. λ5 and λ6 are shown in the table below. 70 and λ 80 The values ​​were measured in the wavelength range of 250–700 nm. The spectral transmittance T (%) of the glass in this invention and specification can be expressed as follows: For a glass sample having two mutually parallel planes after optical polishing, the intensity of light incident perpendicularly to one of these planes is set as I. in And the intensity of the light that passes through the glass sample and is emitted from the other side is set as I. out At that time, T(%) = I out / I in ×100 represents the value.

[0145] Based on chromaticity λ5, λ 70 and λ 80 The absorption end of the short-wavelength side of the spectral transmittance can be quantitatively evaluated. When bonding lenses together using a UV-curable adhesive to create a bonding lens, the following operation can be performed: UV light is irradiated through the optical element onto the adhesive, causing the adhesive to cure. From the viewpoint of efficiently curing the UV-curable adhesive, it is preferable that the absorption end of the short-wavelength side of the spectral transmittance is in a short wavelength range. As an indicator for quantitatively evaluating this short-wavelength absorption end, chromaticity λ5, λ... 70 and λ 80 One or more of them.

[0146] The aforementioned optical glass preferably exhibits a wavelength λ5 of 380 nm or less. λ5 is further preferred in the order of 370 nm or less, 360 nm or less, and 350 nm or less. Shorter wavelengths of λ5 are more preferred, but there is no particular limitation on the lower limit.

[0147] The aforementioned optical glass is preferably capable of displaying a wavelength below 430 nm. 70 . λ 70 Further preferred nanometers are selected in the order of 420nm or less, 410nm or less, 400nm or less, and 395nm or less. 70 Shorter wavelengths are preferred, and there is no specific lower limit.

[0148] The aforementioned optical glass is preferably capable of displaying a wavelength below 510 nm. 80 . λ 80 Further optimization is performed in the order of 500nm or below, 490nm or below, 480nm or below, and 470nm or below. 80 Shorter wavelengths are preferred, and there is no specific lower limit.

[0149] <Methods of Glass Manufacturing>

[0150] The aforementioned optical glass can be obtained as follows: oxides, carbonates, sulfates, nitrates, hydroxides, etc., used as raw materials are weighed and mixed to obtain the desired glass composition. These are then thoroughly mixed to form a mixed batch, heated and melted in a melting vessel, and subjected to degassing and stirring to produce a homogeneous, bubble-free molten glass. This molten glass is then shaped to obtain the optical glass. Specifically, a known melting method can be used for its production.

[0151] [Glass raw materials for compression molding, methods for manufacturing the same, and methods for manufacturing glass molded bodies]

[0152] According to embodiments of the present invention, glass raw materials for pressing and molding made of the above-described optical glass, glass molded bodies made of the above-described optical glass, and methods for manufacturing the same can be provided.

[0153] Glass raw materials for pressing and molding refer to glass blocks that are heated and pressed into shape.

[0154] Examples of glass raw materials for compression molding include glass blocks with a mass comparable to that of the compressed product, such as glass raw materials (glass droplets for compression molding) used for compression molding of preforms for precision compression molding and blanks for optical components.

[0155] Glass raw materials for pressing and molding can be manufactured through a process of processing glass molded bodies. Glass molded bodies can be manufactured by heating and melting glass raw materials as described above, and then molding the resulting molten glass. Examples of processing methods for glass molded bodies include cutting, grinding, and polishing.

[0156] [Optical component blanks and their manufacturing methods]

[0157] According to one aspect of the present invention, an optical element blank made of the aforementioned optical glass can be provided. The optical element blank is a glass molded body having a shape approximating the shape of the optical element to be manufactured. The optical element blank can be manufactured by methods such as molding the glass into a shape that includes machining allowances to be removed during processing. For example, the optical element blank can be manufactured by a method of pressing and molding by heating and softening the glass raw material for pressing (reheat pressing method); or by pressing and molding by feeding a block of molten glass to a pressing mold using a known method (direct pressing method).

[0158] Optical components and their manufacturing methods

[0159] According to one aspect of the present invention, an optical element made of the aforementioned optical glass can be provided. Examples of optical elements include spherical lenses, aspherical lenses, prisms, diffraction gratings, etc. Examples of lens shapes include biconvex lenses, plano-convex lenses, biconcave lenses, plano-concave lenses, convex meniscus lenses, concave meniscus lenses, and various other shapes.

[0160] To prevent the glass from melting and sticking to the forming surface of the molding die during precision pressing and to ensure good glass stretching along the forming surface, a release film is preferably applied to the surface of the preform for precision pressing. Such release films are known. The aforementioned optical glass is a low-Tg glass with a glass transition temperature within the range described above, and it contains no Ti or only a small amount of Ti. Precision pressing preforms made from such glass are preferred from the viewpoint of suppressing the deterioration of the release film. As an example of a release film, a carbon-containing film can be cited. The carbon-containing film can be, for example, a film in which carbon is the main component (when the elemental content in the film is expressed in atomic percent, the carbon content is greater than the content of other elements). As a method for forming a carbon-containing film, known methods such as vacuum evaporation, sputtering, and ion plating using carbon raw materials, or known methods such as thermal decomposition of materials such as hydrocarbons, can be used.

[0161] Figure 1 A cross-sectional schematic diagram of a precision compression molding apparatus is shown. Precision compression molding can be performed, for example, as described below.

[0162] A preform (hereinafter simply referred to as "preform") 4 for precision pressing is placed between the lower mold 2 and the upper mold 1 constituting the pressing mold. Then, a nitrogen atmosphere is created inside the quartz tube 11, and a heater (not shown) is energized to heat the inside of the quartz tube 11. The temperature inside the pressing mold is set to such that the glass to be formed displays, for example, 10°C. 6 ~10 10 At a viscosity of dPa·s, while maintaining this temperature, the push rod 13 is lowered to press against the upper mold 1, applying pressure to the preform placed within the molding die. After pressurization, the pressure is released, and the pressed glass molded article is slowly cooled while maintaining contact with the lower mold 2 and the upper mold 1 until the viscosity of the glass reaches, for example, 10 dPa·s. 12 The glass is heated to a temperature above dPa·s, then rapidly cooled to room temperature, and the molded glass is removed from the mold. This yields an optical element. It should be noted that... Figure 1 In the mold, retaining member 10 holds the lower mold 2 and shell mold 3, and support rod 9 supports the upper mold 1, lower mold 2, shell mold 3, and retaining member 10, and is subjected to pressure based on push rod 13. A thermocouple 14 is inserted inside the lower mold 2 to monitor the temperature inside the pressing mold.

[0163] Another method for manufacturing optical elements is to produce optical elements by machining optical element blanks. Examples of machining include cutting, slitting, rough grinding, fine grinding, and polishing. Such manufacturing methods are suitable for manufacturing spherical lenses, prisms, and the like.

[0164] Example

[0165] The present invention will now be described in more detail with reference to the embodiments. However, the present invention is not limited to the embodiments shown.

[0166] [Examples No. 1 to No. 197]

[0167] To achieve the glass composition shown in the table below, appropriate phosphates, fluorides, nitrates, sulfates, carbonates, hydroxides, oxides, and boric acids were used as raw materials for introducing each component. The raw materials were weighed and thoroughly mixed to prepare the formulation. In the table below, "cat%" represents "cation%", "wt%" represents "mass%", "mol%" represents "mol%", and the Sb₂O₃ content is expressed as an external proportion. Additionally, for example, "B 3+ / Si 4+ "(cat%)" indicates the percentage of B in the glass composition represented by cations. 3+ Content relative to Si 4+ The cation ratio, "B2O3 / SiO2 (wt%)", indicates the mass ratio of B2O3 content to SiO2 content in the glass composition, expressed as a percentage by mass. The same applies to the descriptions of various cation ratios and mass ratios in the tables below.

[0168] The raw materials were placed in a platinum crucible and heated in a furnace set at 1250–1350°C for 120 minutes. The molten glass was stirred and homogenized, then poured into a preheated mold. After natural cooling to near the glass transition temperature, it was immediately placed in an annealing furnace and held at approximately the glass transition temperature for about 30 minutes. Then, it was slowly cooled at a rate of -30°C / hour for 4 hours, and finally allowed to cool naturally to room temperature in the furnace. This yielded the optical glasses of Examples No. 1 to No. 197 shown in the table below. Regarding the anionic composition of each optical glass shown in the table below, O… 2- The content is 100% anion.

[0169] <Physical Property Evaluation>

[0170] The various physical properties of the optical glasses shown in the following table were determined using the following methods.

[0171] (1) Refractive index nd Abbe number νd

[0172] The refractive index nd and Abbe number νd of each optical glass were measured using the refractive index measurement method standard of the Japan Optical Glass Manufacturers Association.

[0173] For each optical glass, the calculated values ​​on the right side of equation (1) and equation (2) are shown in the following table. If each equation is satisfied, it is indicated as "○" in the "Judgment" column.

[0174] (2) Glass transition temperature Tg

[0175] The glass was thoroughly pulverized in a mortar and pestle as a sample. A platinum cell was used as the sample container. The glass transition temperature Tg was determined using a differential scanning calorimeter (DSC3300SA) manufactured by NETZSCH JAPAN, with the heating rate set to 10℃ / min.

[0176] (3) Specific gravity

[0177] The specific gravity was determined using the Archimedes method.

[0178] (4) Liquid phase temperature LT

[0179] The liquid phase temperature LT was determined using the method described above.

[0180] (5) Shading degree λ5, λ 70 , λ 80

[0181] The spectrophotometric transmittance T (%) was determined using a spectrophotometer on a glass sample with a thickness of 10 ± 0.1 mm and two opposing optically polished planes. The wavelength (nm) at which T reaches 5% was defined as λ5, and the wavelength (nm) at which T reaches 70% was defined as λ. 70 Let λ be the wavelength (nm) at which T reaches 80%. 80 .

[0182] The results are shown in the table below.

[0183]

[0184]

[0185]

[0186]

[0187]

[0188]

[0189]

[0190]

[0191]

[0192]

[0193]

[0194]

[0195]

[0196]

[0197]

[0198]

[0199]

[0200]

[0201]

[0202]

[0203]

[0204]

[0205]

[0206]

[0207]

[0208]

[0209]

[0210]

[0211]

[0212]

[0213]

[0214]

[0215]

[0216]

[0217]

[0218]

[0219]

[0220]

[0221]

[0222] Fabrication of preforms for precision pressing

[0223] For each embodiment in the above embodiments, in order to achieve the glass composition shown in the table above, the corresponding nitrates, sulfates, carbonates, hydroxides, oxides, boric acids, etc. are used as raw materials for introducing each component. The raw materials are weighed and thoroughly mixed to prepare the blending raw materials.

[0224] As a comparative example 1, the glass composition of Example 10 shown in Table 1 of Patent Document 1 (Japanese Patent Application Publication No. 2008-201661) was prepared by using the corresponding nitrates, sulfates, carbonates, hydroxides, oxides, boric acids, etc. as raw materials for introducing each component, weighing the raw materials, and mixing them thoroughly.

[0225] As a comparative example 2, in the manner of glass composition shown in Table 1 of Patent Document 1 (Japanese Patent Application Publication No. 2008-201661), corresponding nitrates, sulfates, carbonates, hydroxides, oxides, boric acids, etc. were used as raw materials for introducing each component. The raw materials were weighed and thoroughly mixed to prepare a blended raw material.

[0226] An example of preform fabrication (Example 1) will be described. Raw materials were placed in a platinum crucible and heated to melt. The clarified and homogenized molten glass was then allowed to flow out at a controlled flow rate through a platinum alloy pipe at a temperature adjusted to a stable flow range without causing devitrification. The molten glass was separated into blocks of the desired preform mass using a drip-feeding or drop-cutting method. The separated molten glass blocks were received in a mold with a gas ejector at the bottom. While the glass blocks floated due to gas ejection from the gas ejector, a preform for precision pressing was formed. By adjusting and setting the separation interval of the molten glass blocks, a flat, spherical preform was obtained.

[0227] As another example of preform fabrication (Fabrication Example 2), the following method is used: after the homogeneous molten glass obtained by melting the raw materials is cast into a mold and shaped, the strain of the obtained molded body is removed by annealing, and it is cut or diced into a given size and shape to produce multiple glass sheets. The glass sheets are polished to make the surface smooth, and a preform made of glass of a given quality is produced.

[0228] For the above embodiments and comparative examples, a preform for precision pressing was manufactured by manufacturing example 2.

[0229] [Deterioration Evaluation Experiment of Release Film]

[0230] In the above embodiments and comparative examples, a carbon-containing film was coated on the surface of the fabricated preform, and heating was performed in a nitrogen atmosphere. Specifically, after evacuating the furnace, nitrogen was introduced at approximately 0.2 MPa to bring the glass to a pressure of 2.5 MPa. 10 Heating was performed for 360 seconds at a temperature with a viscosity of approximately poise. Heating was carried out at a rate of 25°C / min from room temperature, and cooling was carried out at a rate of 20°C / min.

[0231] After the above heating, the surface of the preform was measured by SEM-EDX (Scanning Electron Microscope-Energy Dispersive X-ray Spectrometry) at an accelerating voltage of 3 to 25 kV to confirm the presence or absence of carbon, thereby evaluating whether a carbon-containing film remained on the surface of each preform.

[0232] The results of the above experiments showed that a carbon-containing film remained on the surface of the preform in all the above embodiments. In contrast, no carbon-containing film was found on the surface of the preform in Comparative Examples 1 and 2. The glass constituting the preform of Comparative Example 1 was a glass with a TiO2 content of 0.83% by mass (refer to Table 1 of Patent Document 1 (Japanese Unexamined Patent Application Publication No. 2008-201661)). The glass of the preform constituting Comparative Example 2 had a glass transition temperature of 610°C (refer to Table 1 of Patent Document 1 (Japanese Unexamined Patent Application Publication No. 2008-201661)).

[0233] Based on the above results, it can be confirmed that glass with a TiO2 content of less than 0.6% by mass and a glass transition temperature of less than 610°C, as in the above embodiments, can prevent the deterioration of the release film.

[0234] To confirm the correlation between the above experiments and the adaptability to precision pressing, a carbon-containing film was coated on the surface of the preforms produced in the above embodiments and comparative examples. The preforms were then introduced into a SiC pressing mold containing upper and lower molds and a shell mold, with a carbon-containing release film on the molding surface. The molding mold and the preforms were heated together in a nitrogen atmosphere to soften the preforms and then precision pressed to produce an aspherical biconvex lens with a diameter of 30 mm and a thickness of 4 mm in the optical axis direction.

[0235] In the above embodiments, even after more than 150 shots, no deterioration of the release film was observed during precision pressing, indicating good mass production capability. In contrast, in the above comparative example, significant deterioration of the release film was observed during 100 shots of precision pressing, resulting in mold breakage, poor lens shape / appearance, and other issues, leading to poor mass production capability.

[0236] The results above confirm that the glass produced by the above embodiments can achieve excellent mass production performance through precision pressing. Furthermore, the glass according to the above embodiments can also be used to manufacture large-diameter lenses exceeding φ30mm, lenses with a wall thickness exceeding 4mm along the optical axis (more preferably lenses with a maximum wall thickness exceeding 5mm), and lenses with complex shapes, with high mass production performance.

[0237] Finally, the above implementation methods are summarized.

[0238] [1] An optical glass, wherein,

[0239] In the glass composition expressed as mass %

[0240] Li2O content exceeds 0% by mass.

[0241] The B2O3 content is above 3.00% by mass and below 30.00% by mass.

[0242] The SiO2 content is greater than 0% by mass and less than 8.00% by mass.

[0243] The La2O3 content is above 15.00% by mass and below 55.00% by mass.

[0244] The ZnO content is 3.00% by mass or more and 30.00% by mass or less.

[0245] The TiO2 content is below 0.60% by mass.

[0246] The total content of Li2O and ZnO (Li2O+ZnO) is 10.20% by mass or more.

[0247] The mass ratio of B2O3 content to Li2O content (B2O3 / Li2O) is 5.00 or higher and 21.00 or lower, and the mass ratio of SiO2 content to Li2O content (SiO2 / Li2O) is 10.00 or lower.

[0248] The glass transition temperature (Tg) of the optical glass is below 610℃.

[0249] The liquidus temperature LT is above 1090℃.

[0250] The refractive index nd and the glass transition temperature Tg satisfy the following equation (1), and the refractive index nd and the Abbe number νd satisfy the following equation (2).

[0251] Equation (1): Tg < 2500*nd - 4050

[0252] Equation (2): νd>-88.355*nd+201.

[0253] [2] According to the optical glass described in [1], wherein,

[0254] In the glass composition expressed as cations%, B 3+ Content relative to Si 4+ The ratio of cations in the content (B) 3+ / Si 4+ The value is above 1.25 and below 11.00.

[0255] [3] The optical glass according to [1] or [2], wherein,

[0256] In the glass composition expressed as mass % (Nb2O5, TiO2, and WO3), the mass ratio of the total content of Nb2O5, TiO2, and WO3 to the total content of SiO2 and B2O3 (Nb2O5+TiO2+WO3) / (SiO2+B2O3) is 0.40 or more and 1.60 or less.

[0257] [4] The optical glass according to any one of [1] to [3], wherein,

[0258] In the glass composition expressed as % by mass, the mass ratio of ZnO content to WO3 content (ZnO / WO3) is 0.10 or more and 5.00 or less.

[0259] [5] The optical glass according to any one of [1] to [4], wherein,

[0260] In the glass composition expressed as mass % (Lu2O3 content relative to the total content of La2O3, Gd2O3, Y2O3 and Lu2O3) (Lu2O3 / (La2O3+Gd2O3+Y2O3+Lu2O3)), the mass ratio of Lu2O3 content to the total content of La2O3, Gd2O3, Y2O3 and Lu2O3 is 0.50 or less.

[0261] [6] The optical glass according to any one of [1] to [5], wherein,

[0262] In the glass composition expressed as cations%, Li + The content is 0.50% or more of cationic.

[0263] [7] The optical glass according to any one of [1] to [6] has a refractive index nd of 1.8600 or higher.

[0264] [8] The optical glass according to any one of [1] to [7] has an Abbe number νd of 34.0 or more and 40.0 or less.

[0265] [9] The optical glass according to claim 1, wherein,

[0266] In the glass composition expressed as mass %

[0267] The mass ratio of the total content of Nb2O5, TiO2, and WO3 to the total content of SiO2 and B2O3 (Nb2O5+TiO2+WO3) / (SiO2+B2O3) is greater than or equal to 0.40 and less than or equal to 1.60.

[0268] The mass ratio of ZnO content to WO3 content (ZnO / WO3) is greater than 0.10 and less than 5.00.

[0269] The mass ratio of Lu2O3 content to the total content of La2O3, Gd2O3, Y2O3, and Lu2O3 (Lu2O3 / (La2O3+Gd2O3+Y2O3+Lu2O3)) is less than 0.50.

[0270] In the glass composition expressed as cations%,

[0271] B 3+ Content relative to Si 4+ The ratio of cations in the content (B) 3+ / Si 4+ For values ​​between 1.25 and 11.00, Li + The content is 0.50% or more of cationic content.

[0272] The optical glass has a refractive index nd of 1.8600 or higher, and

[0273] The Abbe number νd is above 34.0 and below 40.0.

[0274]

[10] An optical element made of any one of the optical glass described in [1] to [9].

[0275] It should be understood that all the embodiments disclosed herein are exemplary and do not constitute a limitation. The scope of the invention is defined by the claims, not the foregoing description, and is intended to include all modifications within the meaning and scope of the claims.

[0276] For example, by adjusting the composition as described in the specification, an optical glass according to one aspect of the present invention can be obtained from the glass composition exemplified above.

[0277] In addition, any combination of two or more items exemplified in the specification or described as a preferred range is of course possible.

Claims

1. An optical glass, wherein, In the glass composition expressed as a percentage by mass, Li2O content exceeds 0% by mass. The B2O3 content is above 3.00% by mass and below 30.00% by mass. The SiO2 content is greater than 0% by mass and less than 8.00% by mass. The La2O3 content is above 15.00% by mass and below 55.00% by mass. The ZnO content is above 3.00% by mass and below 30.00% by mass. The TiO2 content is below 0.60% by mass. The total content of Li2O and ZnO (Li2O+ZnO) is 10.20% by mass or more. The mass ratio of B2O3 content to Li2O content (B2O3 / Li2O) is greater than 5.00 and less than 21.

00. The mass ratio of SiO2 content to Li2O content (SiO2 / Li2O) is below 10.

00. The mass ratio of the total content of Nb2O5, TiO2, and WO3 to the total content of SiO2 and B2O3 (Nb2O5+TiO2+WO3) / (SiO2+B2O3) is 0.56 or higher and 1.60 or lower. The glass transition temperature (Tg) of the optical glass is below 610℃. The liquidus temperature LT is above 1090℃. The refractive index nd and the glass transition temperature Tg satisfy the following equation (1), and the refractive index nd and the Abbe number νd satisfy the following equation (2). Equation (1): Tg < 2500*nd - 4050 Equation (2): νd>-88.355*nd+201.

2. An optical glass, wherein, In the glass composition expressed as a percentage by mass, Li2O content exceeds 0% by mass. The B2O3 content is above 3.00% by mass and below 30.00% by mass. The SiO2 content is greater than 0% by mass and less than 8.00% by mass. The La2O3 content is above 15.00% by mass and below 55.00% by mass. The ZnO content is above 3.00% by mass and below 30.00% by mass. The TiO2 content is below 0.60% by mass. The total content of Li2O and ZnO (Li2O+ZnO) is 10.20% by mass or more. The mass ratio of B2O3 content to Li2O content (B2O3 / Li2O) is greater than 5.00 and less than 21.

00. The mass ratio of SiO2 content to Li2O content (SiO2 / Li2O) is below 10.

00. The mass ratio of ZnO content to WO3 content (ZnO / WO3) is greater than 0.10 and less than 2.

46. The glass transition temperature (Tg) of the optical glass is below 610℃. The liquidus temperature LT is above 1090℃. The refractive index nd and the glass transition temperature Tg satisfy the following equation (1), and the refractive index nd and the Abbe number νd satisfy the following equation (2). Equation (1): Tg < 2500*nd - 4050 Equation (2): νd>-88.355*nd+201.

3. An optical glass, wherein, In the glass composition expressed as a percentage by mass, Li2O content exceeds 0% by mass. The B2O3 content is above 3.00% by mass and below 30.00% by mass. The SiO2 content is greater than 0% by mass and less than 8.00% by mass. The La2O3 content is above 15.00% by mass and below 55.00% by mass. The ZnO content is above 3.00% by mass and below 30.00% by mass. The TiO2 content is below 0.60% by mass. The WO3 content is 7.27% by mass or higher. The total content of Li2O and ZnO (Li2O+ZnO) is 10.20% by mass or more. The mass ratio of B2O3 content to Li2O content (B2O3 / Li2O) is greater than 5.00 and less than 21.

00. The mass ratio of SiO2 content to Li2O content (SiO2 / Li2O) is below 10.

00. The mass ratio of the total content of Nb2O5, TiO2, and WO3 to the total content of SiO2 and B2O3 (Nb2O5+TiO2+WO3) / (SiO2+B2O3) is greater than or equal to 0.40 and less than or equal to 1.

60. The glass transition temperature (Tg) of the optical glass is below 610℃. The liquidus temperature LT is above 1090℃. The refractive index nd and the glass transition temperature Tg satisfy the following equation (1), and the refractive index nd and the Abbe number νd satisfy the following equation (2). Equation (1): Tg < 2500*nd - 4050 Equation (2): νd>-88.355*nd+201.

4. An optical glass, wherein, In the glass composition expressed as a percentage by mass, Li2O content exceeds 0% by mass. The B2O3 content is above 3.00% by mass and below 30.00% by mass. The SiO2 content is greater than 0% by mass and less than 8.00% by mass. The La2O3 content is above 15.00% by mass and below 55.00% by mass. The ZnO content is above 3.00% by mass and below 30.00% by mass. The TiO2 content is below 0.60% by mass. The WO3 content is 7.27% by mass or higher. The total content of Li2O and ZnO (Li2O+ZnO) is 10.20% by mass or more. The mass ratio of B2O3 content to Li2O content (B2O3 / Li2O) is greater than 5.00 and less than 21.

00. The mass ratio of SiO2 content to Li2O content (SiO2 / Li2O) is below 10.

00. The mass ratio of ZnO content to WO3 content (ZnO / WO3) is greater than 0.10 and less than 5.

00. The glass transition temperature (Tg) of the optical glass is below 610℃. The liquidus temperature LT is above 1090℃. The refractive index nd and the glass transition temperature Tg satisfy the following equation (1), and the refractive index nd and the Abbe number νd satisfy the following equation (2). Equation (1): Tg < 2500*nd - 4050 Equation (2): νd>-88.355*nd+201.

5. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as cations%, B 3+ Content relative to Si 4+ The ratio of cations in the content (B) 3+ / Si 4+ The value is above 1.25 and below 11.

00.

6. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass % (Lu2O3 content relative to the total content of La2O3, Gd2O3, Y2O3 and Lu2O3) (Lu2O3 / (La2O3+Gd2O3+Y2O3+Lu2O3)), the mass ratio of Lu2O3 content to the total content of La2O3, Gd2O3, Y2O3 and Lu2O3 is less than 0.

50.

7. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as cations%, Li + The content is 0.50% or more of cations.

8. The optical glass according to any one of claims 1 to 4, wherein the refractive index nd is 1.8600 or higher.

9. The optical glass according to any one of claims 1 to 4, wherein the Abbe number νd is 34.0 or more and 40.0 or less.

10. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as a percentage by mass, The mass ratio of the total content of Nb2O5, TiO2, and WO3 to the total content of SiO2 and B2O3 (Nb2O5+TiO2+WO3) / (SiO2+B2O3) is 0.56 or higher and 1.60 or lower. The mass ratio of ZnO content to WO3 content (ZnO / WO3) is greater than 0.10 and less than 2.

46. The mass ratio of Lu2O3 content to the total content of La2O3, Gd2O3, Y2O3, and Lu2O3 (Lu2O3 / (La2O3+Gd2O3+Y2O3+Lu2O3)) is less than 0.

50. In the glass composition expressed as cations%, B 3+ Content relative to Si 4+ The ratio of cations in the content (B) 3+ / Si 4+ () is above 1.25 and below 11.00, Li + The content is 0.50% or more of cations. The optical glass has a refractive index nd of 1.8600 or higher, and The Abbe number νd is above 34.0 and below 40.

0.

11. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the Li2O content is 0.20% or more, 0.45% or more, or 0.62% or more.

12. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the B2O3 content is 6.00% by mass or more, or 10.50% by mass or more.

13. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the B2O3 content is less than 20.00% by mass or less than 13.78% by mass.

14. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the SiO2 content is 2.50% by mass or more, or 3.06% by mass or more.

15. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the SiO2 content is less than 7.00% by mass or more than 5.75% by mass.

16. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as a percentage by mass, the mass ratio of B2O3 content to Li2O content (B2O3 / Li2O) is 6.00 or more or 7.40 or more.

17. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as a percentage by mass, the mass ratio of B2O3 content to Li2O content (B2O3 / Li2O) is 19.50 or less or 17.50 or less.

18. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as cations%, B 3+ Content relative to Si 4+ The ratio of cations in the content (B) 3+ / Si 4+ The value is 1.75 or higher, or 3.30 or higher.

19. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as cations%, B 3+ Content relative to Si 4+ The ratio of cations in the content (B) 3+ / Si 4+ The value is below 9.75 or below 7.

50.

20. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as a percentage by mass, the mass ratio of B2O3 content to SiO2 content (B2O3 / SiO2) is 0.50 or more or 2.00 or more.

21. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as a percentage by mass, the mass ratio of B2O3 content to SiO2 content (B2O3 / SiO2) is 7.50 or less or 4.50 or less.

22. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the La2O3 content is 23.00% or more or 28.35% or more.

23. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the La2O3 content is less than 45.00% by mass or less than 38.00% by mass.

24. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the Gd2O3 content is less than 14.00% by mass.

25. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the ZnO content is 5.75% by mass or more, or 9.30% by mass or more.

26. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the ZnO content is less than 21.00% by mass or less than 15.65% by mass.

27. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the total content of Li2O and ZnO (Li2O+ZnO) is 10.40% by mass or more.

28. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the total content of Li2O and ZnO (Li2O+ZnO) is less than 17.00% by mass.

29. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the Nb2O5 content is less than 6.00% by mass.

30. The optical glass according to any one of claims 2 to 4, wherein, In the glass composition expressed as mass % (Nb2O5, TiO2, and WO3), the mass ratio of the total content of Nb2O5, TiO2, and WO3 to the total content of SiO2 and B2O3 (Nb2O5+TiO2+WO3) / (SiO2+B2O3) is 0.56 or more or 0.63 or more.

31. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as mass%, the mass ratio of the total content of Nb2O5, TiO2 and WO3 to the total content of SiO2 and B2O3 (Nb2O5+TiO2+WO3) / (SiO2+B2O3) is less than 1.30 or less than 1.

15.

32. The optical glass according to any one of claims 1 to 4, wherein, In the glass composition expressed as a percentage by mass, the mass ratio of ZnO content to WO3 content (ZnO / WO3) is 0.70 or higher.

33. The optical glass according to any one of claims 1, 3 to 4, wherein, In the glass composition expressed as a percentage by mass, the mass ratio of ZnO content to WO3 content (ZnO / WO3) is less than 2.

60.

34. The optical glass according to any one of claims 1 to 4, wherein the liquidus temperature LT is below 1180°C.

35. An optical element made of any one of the optical glass claims 1 to 34.

Citation Information

Patent Citations

  • Optical glass, preform for precision press-molding, optical element, and methods for manufacturing the same

    JP2008201661A

  • Optical glass for pressure forming

    CN101423328A

  • Optical glass and optical element formed from optical glass

    CN114315130A

  • Optical glass for mold press molding

    JP2009102215A

  • Optical glass

    JP2013256438A