A negative electrode, a battery, its preparation method and application
By setting pores and grooves in the active material layer of the negative electrode and optimizing the electrolyte composition, the problem of poor battery wettability under high voltage density was solved, and a battery with high energy density and high and low temperature performance was achieved.
Patent Information
- Application Number
- CN202311780889.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-22
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-22
AI Technical Summary
How to improve the wettability of the negative electrode and electrolyte under high actual density to ensure that the battery has high energy density, good liquid retention capacity and excellent high and low temperature cycle life.
Pores are formed on the surface of the active material layer of the negative electrode. By adjusting parameters such as the depth, volume fraction, and angle of the pores, combined with the viscosity and composition ratio of the electrolyte, the wettability between the negative electrode and the electrolyte is optimized, forming a rapid lithium-ion diffusion channel.
Under high density, the energy density and liquid retention capacity of the battery are improved, ensuring the stability and cycle life of the battery in high and low temperature environments.
Smart Images

Figure CN117832384B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery technology, and in particular to a negative electrode, a battery, a method for preparing the same, and their applications. Background Technology
[0002] Lithium-ion batteries are a common type of rechargeable battery widely used in mobile devices, electric vehicles, and renewable energy storage systems. They store and release electrical energy through an electrochemical reaction between lithium ions at the positive and negative electrodes. The main components of a lithium-ion battery include the positive electrode, negative electrode, electrolyte, and separator. The positive electrode is typically made of lithium compounds (such as lithium manganese oxide, lithium cobalt oxide, or lithium iron phosphate), while the negative electrode often uses graphite materials. The electrolyte is a conductive solution or polymer film used for ion conduction. The separator isolates the positive and negative electrodes to prevent short circuits. The working principle of a lithium-ion battery is that lithium ions repeatedly insert and extract between the positive and negative electrodes during charging and discharging. When the battery is charging, lithium ions are released from the positive electrode, move through the electrolyte to the negative electrode, and insert into it. When the battery discharges, lithium ions are extracted from the negative electrode and move back to the positive electrode. This insertion and extraction process is reversible, allowing lithium-ion batteries to be charged and discharged multiple times. Lithium-ion batteries have many advantages, such as high energy density, long cycle life, low self-discharge rate, and minimal memory effect. They are also lighter, easier to maintain, and have higher voltage stability than other types of rechargeable batteries.
[0003] As market demands for battery performance gradually increase, high-performance lithium-ion batteries not only need to possess high energy density but also excellent long cycle life. One common measure to improve the energy density of lithium-ion batteries is to increase the compaction density of the positive and negative electrodes. However, increasing the compaction density has a significant negative impact on the liquid absorption capacity and time of the electrodes and separator. Insufficient liquid absorption by the cell can lead to adverse phenomena such as rapid liquid degradation during later cycles.
[0004] To improve electrolyte wetting, methods such as high-temperature settling after electrolyte injection, vacuum settling, or complex formation processes are commonly used. Furthermore, some battery manufacturers address the difficulty of electrolyte absorption by electrodes and separators by reducing electrolyte viscosity and adding novel wetting agents, thereby increasing the amount of electrolyte absorbed by the electrodes and separator in the cell and reducing the absorption time. Increasing the content of low-melting-point, low-viscosity solvents in the electrolyte improves electrode wetting, but deteriorates the battery's high-temperature performance. Conversely, increasing electrolyte viscosity results in better high-temperature performance but weaker penetration, leading to insufficient wetting and ultimately rendering the product unusable.
[0005] Therefore, how to ensure that the electrode and electrolyte have suitable wettability and improve the electrolyte retention and high and low temperature cycle life of the battery have become urgent technical problems to be solved. Summary of the Invention
[0006] The first technical problem to be solved by this invention is:
[0007] A negative electrode is provided.
[0008] The second technical problem to be solved by this invention is:
[0009] A battery is provided.
[0010] To solve the first technical problem, the technical solution adopted by the present invention is as follows:
[0011] A negative electrode, the structure of which includes:
[0012] current collector;
[0013] An active material layer is disposed on the surface of the current collector;
[0014] The number of active material layers is greater than or equal to 1, and at least one active material layer has a hole groove on its surface;
[0015] The depth H of the groove and the thickness T of the active material layer satisfy the following relationship:
[0016] 1 / 3T < H ≤ 2 / 3T;
[0017] The compaction density of the active material layer is P, and P satisfies the following relationship: 1.55 ≤ P ≤ 1.75 g / cm³ 3 .
[0018] According to embodiments of the present invention, one of the technical solutions has at least one of the following advantages or beneficial effects:
[0019] This invention, while ensuring high energy density in the active material layer, further balances the wettability between the negative electrode and the electrolyte, ensuring that the battery not only has high energy density benefits, but also has good liquid retention capacity and excellent high and low temperature cycle life.
[0020] Specifically:
[0021] High-density active material layers can effectively improve battery energy density, but high density reduces the gaps in the active material layer, increasing the difficulty of electrolyte wetting and leading to poor wetting and reduced battery liquid retention. Therefore, this invention incorporates grooves in the active material layer on the negative electrode surface to facilitate electrolyte flow, improve wetting, promote liquid retention, and create channels for rapid lithium-ion diffusion, effectively alleviating the wetting and lithium plating problems associated with high-density electrodes. Furthermore, by adjusting the groove depth H and the active material layer thickness T, electrolyte flow is controlled, balancing the wetting between the negative electrode and the electrolyte, ensuring high battery energy density, good liquid retention, and excellent high and low temperature cycle life.
[0022] According to one embodiment of the present invention, the active material layer is disposed on the upper and / or lower surface of the current collector.
[0023] According to one embodiment of the present invention, the volume fraction of the pores in the active material layer is η, where η satisfies the following relationship: 1% ≤ η ≤ 5%. The present invention defines the presence of pores in the active material layer on the surface of the negative electrode to facilitate electrolyte flow and improve wetting. However, if the volume fraction of the pores in the negative electrode is too high, it will affect the N / P ratio of the positive and negative electrodes; if the volume fraction is too low, electrolyte wetting will be unsatisfactory, and the lithium-ion transport path will be obstructed. Therefore, it is necessary to strictly limit the volume fraction of the pores in the active material layer.
[0024] According to one embodiment of the present invention, the perforation width of the pores in the active material layer is R, and R satisfies the following relationship: 50≤R≤140μm.
[0025] According to one embodiment of the present invention, the spacing between the pores in the active material layer is L, and L satisfies the following relationship: 1.0≤L≤2.5mm.
[0026] According to one embodiment of the present invention, the angle between the perforated groove and the negative electrode plate in the reactive material layer is θ, where θ satisfies the following relationship: 85°≤θ≤95°. The angle between the perforated groove and the negative electrode plate, the spacing between the perforated grooves, the perforation width of the perforated grooves, the volume fraction of the perforated grooves, and the depth H of the perforated grooves all affect the regulation of electrolyte flow by the perforated grooves, thereby affecting the electrolyte retention stability.
[0027] According to one embodiment of the present invention, the material of the negative electrode includes at least one of graphite and graphite mixed with silicon carbon.
[0028] To solve the second technical problem, the technical solution adopted by the present invention is as follows:
[0029] A battery includes a positive electrode, a separator, an electrolyte, and the negative electrode.
[0030] According to one embodiment of the present invention, the electrolyte comprises a non-aqueous solvent, a lithium salt, and an additive, wherein the non-aqueous solvent comprises a first organic solvent and a second organic solvent, the first organic solvent having a mass fraction of W1 in the electrolyte, wherein W1 satisfies the following relationship: 30 wt.% ≤ W1 ≤ 45 wt.%; the second organic solvent having a mass fraction of W2 in the electrolyte, wherein W2 satisfies the following relationship: 15 wt.% ≤ W2 ≤ 40 wt.%, and W2 ≤ W1 ≤ 3W2.
[0031] According to one embodiment of the present invention, the viscosity of the electrolyte is ω, where ω satisfies the following relationship: 0.4 ≤ ω ≤ 2 mPa·s. The viscosity ω of the electrolyte is the viscosity of the electrolyte at 25°C. Too low an electrolyte viscosity will deteriorate high-temperature performance, while increased electrolyte viscosity is detrimental to low-temperature performance and will also affect the battery's wetting effect and liquid retention stability. By setting the ratio of the first solvent to the second solvent in the present invention to control the electrolyte viscosity, combined with the pore effect of the negative electrode sheet, wetting is ensured while appropriately increasing the electrolyte viscosity and liquid retention stability, thus balancing the high and low temperature performance of the battery. Therefore, the present invention reduces the requirements of high compaction density on the electrolyte's penetration capacity, broadens the selection of solvents and additives and the ratio window, and significantly improves the overall performance of the battery.
[0032] According to one embodiment of the present invention, the negative electrode sheet has a compaction density of P, and includes an active material layer with pores and grooves. The volume fraction of the pores and grooves is η, and P, η, W1, and ω satisfy the following relationship: 2.8 ≤ (P*ω) / (10*=*W1) ≤ 50. To ensure stable liquid retention between the negative electrode sheet and the electrolyte, and to consider the high and low temperature performance of the battery, the compaction density of the negative electrode sheet, the volume fraction of the pores and grooves, and the electrolyte solvent need to satisfy the above relationship. When the compaction density is high, there are fewer gaps between the substances in the active material layer, making it extremely difficult to wet the electrolyte and maintain liquid retention stability. Low electrolyte viscosity is beneficial for electrolyte wetting, but at high temperatures, the reactivity of the substances in the active material layer is also enhanced, increasing side reactions with the electrolyte, and generating more byproducts and heat, posing a significant safety risk. The presence of pores and grooves on the electrode surface helps the electrode to have good liquid retention stability and also provides a path for rapid lithium-ion transport. Therefore, by creating grooves on the surface of the electrode under high voltage density, the viscosity of the electrolyte can be appropriately increased, giving the electrode good electrolyte retention stability and excellent performance at high or low temperatures.
[0033] According to one embodiment of the present invention, the pressure relief compaction density of the negative electrode is β, and the pressure relief compaction density β, the compaction density P of the negative electrode, and the viscosity ω of the electrolyte satisfy the following relationship: 0.05≤ω*(P-β) / P≤0.23. Satisfying the above relationship further improves the electrolyte retention stability of the negative electrode. Furthermore, in the above relationship, the various substances in the active material layer have good contact, and the presence of pores in the active material layer on the anode surface can further reduce lithium-ion transport obstacles, helping to reduce heat generation during battery charging and discharging, and improving the high and low temperature performance of the battery.
[0034] According to one embodiment of the present invention, the first organic solvent includes at least one of carbonate organic solvents and carboxylic acid ester organic solvents; the second organic solvent includes at least one of sulfur solvents, fluorinated solvents, sulfone solvents and nitrile solvents.
[0035] According to one embodiment of the present invention, the first organic solvent includes at least one selected from ethylene carbonate, propylene carbonate, γ-butyrolactone L, dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate.
[0036] According to one embodiment of the present invention, the mass fraction of the first organic solvent in the electrolyte is W1, and 30 wt.% ≤ W1 ≤ 45 wt.%.
[0037] According to one embodiment of the present invention, the second organic solvent includes at least one selected from CF3SO2N(CH2CH3)(CH3), CF3SO2N(CH2CH3)2, CF3SO2N(CH3)2, CF3CF2SO2N(CH3)2, sulfite ester, butenyl sulfite ester, methoxyethyl methyl sulfone, tetramethylene sulfone, succinate, pentanolyl nitrile, dioxolane fluoride, pyrrolidine, piperidine, and ammonium solvents.
[0038] According to one embodiment of the present invention, the second organic solvent has a mass fraction of W2 in the electrolyte, and 15 wt.% ≤ W2 ≤ 40 wt.%.
[0039] According to one embodiment of the present invention, the electrolyte in the battery further includes a lithium salt, wherein the lithium salt includes at least one of LiFSI, LiTFSI, LiBOB, and LiPO2F2.
[0040] According to one embodiment of the present invention, the lithium salt has a mass fraction of 10-20 wt.% in the electrolyte.
[0041] According to one embodiment of the present invention, the electrolyte in the battery further includes an additive, the additive comprising at least one selected from 1,3-propanesulfonate lactone, 1,3-propenesulfonate lactone, 1,3,6-hexanetrionitrile, 1,3-propanesulfonate lactone, vinyl sulfate, and 1,2-bis(cyanoethoxy)ethane.
[0042] According to one embodiment of the present invention, the additive has a mass percentage of 10-20 wt.% in the electrolyte.
[0043] According to one embodiment of the present invention, the material of the positive electrode includes at least one of lithium cobalt oxide, ternary materials, and lithium-rich materials.
[0044] According to one embodiment of the present invention, the material of the diaphragm includes at least one of polyethylene, polypropylene and polyvinylidene fluoride.
[0045] Other features and advantages of the invention will be set forth in the description which follows, and will be apparent in part from the description, or may be learned by practicing the invention. Attached Figure Description
[0046] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:
[0047] Figure 1 This is a schematic diagram of the structure of the active material layer in Example 1. Detailed Implementation
[0048] In the description of this invention, the use of terms such as "first," "second," etc., is for the purpose of distinguishing technical features only and should not be construed as indicating or implying relative importance, or implicitly indicating the number of technical features indicated, or implicitly indicating the order of the technical features indicated.
[0049] In the description of this invention, it should be understood that the orientation descriptions, such as up, down, etc., are based on the orientation or positional relationship shown in the embodiments, and are only for the purpose of facilitating the description of this invention and simplifying the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this invention.
[0050] The terms "preferred," "more preferably," etc., used in this invention refer to embodiments of the invention that provide certain beneficial effects under certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. Furthermore, the description of one or more preferred embodiments does not imply that other embodiments are unavailable, nor is it intended to exclude other embodiments from the scope of this invention.
[0051] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.
[0052] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of the present invention.
[0053] Unless otherwise specified, the reagents, methods and equipment used in this invention are all conventional reagents, methods and equipment in this technical field.
[0054] In the examples and comparative examples, the first organic solvent was ethylene carbonate, the second organic solvent was methoxyethyl methyl sulfone, the lithium salt was LiPO2F2, and the additive was 1,3-propenesulfonate lactone.
[0055] In the examples and comparative examples, the viscosity ω of the electrolyte is the viscosity of the electrolyte at 25°C.
[0056] Example 1
[0057] A negative electrode sheet, the structure of which includes:
[0058] current collector;
[0059] An active material layer is disposed on the surface of the current collector; a schematic diagram of the structure of the active material layer is shown below. Figure 1 As shown;
[0060] The number of the above-mentioned active material layers is 1, and the surface of the active material layer is provided with grooves;
[0061] The depth H of the aforementioned grooves and the thickness T of the aforementioned active material layer satisfy the following relationship:
[0062] 1 / 3T < H ≤ 2 / 3T;
[0063] The compaction density of the above-mentioned active material layer is P, and P is 1.6 g / cm³. 3 .
[0064] The volume fraction of the pores in the above-mentioned active material layer is η, where η is 1%.
[0065] A battery includes a positive electrode, a separator, an electrolyte, and the aforementioned negative electrode.
[0066] The above-mentioned method for preparing the positive electrode includes the following steps:
[0067] The active material LiCoO2, conductive agent acetylene black, conductive carbon nanotubes, and binder polyvinylidene fluoride (PVDF) were fully dispersed and uniformly coated onto an aluminum current collector in an N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold-pressed into strips to obtain the positive electrode sheet.
[0068] The method for preparing the above-mentioned diaphragm includes the following steps:
[0069] A ceramic mixture is coated onto the PE surface to serve as a release membrane.
[0070] The preparation process of the above-mentioned negative electrode includes the following steps:
[0071] A negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05), and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) were mixed in a weight ratio of 97.7:1.1:1.2 to prepare a negative electrode active material slurry. This slurry was then uniformly coated onto a composite current collector and compacted to a density of 1.6 g / cm³. 3 Cold pressing and slitting; using laser drilling equipment to create holes on the surface of the active material layer, with a hole volume ratio of 1%, to obtain the negative electrode sheet.
[0072] The preparation process of the above electrolyte includes the following steps:
[0073] An electrolyte is prepared by mixing and dissolving 40 wt.% of a first organic solvent, 30 wt.% of a second organic solvent, 15 wt.% of a lithium salt, and 15 wt.% of an additive.
[0074] The viscosity of the electrolyte is 0.806 mPa·s.
[0075] The manufacturing process of the above-mentioned battery includes the following steps:
[0076] The above-mentioned positive electrode sheet, separator, and negative electrode sheet are wound to form a bare cell, which is then packaged and injected with electrolyte to produce a finished battery.
[0077] Example 2
[0078] The difference between Example 2 and Example 1 lies in the volume fraction of the perforations. Specifically, the volume fraction of the perforations in Example 1 is 1%, while the volume fraction of the perforations in Example 2 is 3%.
[0079] A negative electrode sheet, the structure of which includes:
[0080] current collector;
[0081] An active material layer is disposed on the surface of the current collector;
[0082] The number of the above-mentioned active material layers is 1, and the surface of the active material layer is provided with grooves;
[0083] The depth H of the aforementioned grooves and the thickness T of the aforementioned active material layer satisfy the following relationship:
[0084] 1 / 3T < H ≤ 2 / 3T;
[0085] The compaction density of the above-mentioned active material layer is P, and P is 1.6 g / cm³. 3 .
[0086] The volume fraction of the pores in the above-mentioned active material layer is η, where η is 3%.
[0087] A battery includes a positive electrode, a separator, an electrolyte, and the aforementioned negative electrode.
[0088] The above-mentioned method for preparing the positive electrode includes the following steps:
[0089] The active material LiCoO2, conductive agent acetylene black, conductive carbon nanotubes, and binder polyvinylidene fluoride (PVDF) were fully dispersed and uniformly coated onto an aluminum current collector in an N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold-pressed into strips to obtain the positive electrode sheet.
[0090] The method for preparing the above-mentioned diaphragm includes the following steps:
[0091] A ceramic mixture is coated onto the PE surface to serve as a release membrane.
[0092] The preparation process of the above-mentioned negative electrode includes the following steps:
[0093] A negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05), and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) were mixed in a weight ratio of 97.7:1.1:1.2 to prepare a negative electrode active material slurry. This slurry was then uniformly coated onto a composite current collector and compacted to a density of 1.6 g / cm³. 3 Cold pressing and slitting; using laser drilling equipment to create holes on the surface of the active material layer, with a hole volume ratio of 3%, to obtain the negative electrode sheet.
[0094] The preparation process of the above electrolyte includes the following steps:
[0095] An electrolyte is prepared by mixing and dissolving 40 wt.% of a first organic solvent, 30 wt.% of a second organic solvent, 15 wt.% of a lithium salt, and 15 wt.% of an additive.
[0096] The viscosity of the electrolyte is 0.806 mPa·s.
[0097] The manufacturing process of the above-mentioned battery includes the following steps:
[0098] The above-mentioned positive electrode sheet, separator, and negative electrode sheet are wound to form a bare cell, which is then packaged and injected with electrolyte to produce a finished battery.
[0099] Example 3
[0100] The difference between Example 3 and Example 1 includes the different volume fractions of the perforations. Specifically, the volume fraction of the perforations in Example 1 is 1%, while the volume fraction of the perforations in Example 3 is 5%.
[0101] A negative electrode sheet, the structure of which includes:
[0102] current collector;
[0103] An active material layer is disposed on the surface of the current collector;
[0104] The number of the above-mentioned active material layers is 1, and the surface of the active material layer is provided with grooves;
[0105] The depth H of the aforementioned grooves and the thickness T of the aforementioned active material layer satisfy the following relationship:
[0106] 1 / 3T < H ≤ 2 / 3T;
[0107] The compaction density of the above-mentioned active material layer is P, and P is 1.6 g / cm³. 3 .
[0108] The volume fraction of the pores in the above-mentioned active material layer is η, where η is 5%.
[0109] A battery includes a positive electrode, a separator, an electrolyte, and the aforementioned negative electrode.
[0110] The above-mentioned method for preparing the positive electrode includes the following steps:
[0111] The active material LiCoO2, conductive agent acetylene black, conductive carbon nanotubes, and binder polyvinylidene fluoride (PVDF) were fully dispersed and uniformly coated onto an aluminum current collector in an N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold-pressed into strips to obtain the positive electrode sheet.
[0112] The method for preparing the above-mentioned diaphragm includes the following steps:
[0113] A ceramic mixture is coated onto the PE surface to serve as a release membrane.
[0114] The preparation process of the above-mentioned negative electrode includes the following steps:
[0115] A negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05), and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) were mixed in a weight ratio of 97.7:1.1:1.2 to prepare a negative electrode active material slurry. This slurry was then uniformly coated onto a composite current collector and compacted to a density of 1.6 g / cm³. 3 Cold pressing and slitting; using laser drilling equipment to create holes on the surface of the active material layer, with a hole volume ratio of 5%, to obtain the negative electrode sheet.
[0116] The preparation process of the above electrolyte includes the following steps:
[0117] An electrolyte is prepared by mixing and dissolving 40 wt.% of a first organic solvent, 30 wt.% of a second organic solvent, 15 wt.% of a lithium salt, and 15 wt.% of an additive.
[0118] The viscosity of the electrolyte is 0.806 mPa·s.
[0119] The manufacturing process of the above-mentioned battery includes the following steps:
[0120] The above-mentioned positive electrode sheet, separator, and negative electrode sheet are wound to form a bare cell, which is then packaged and injected with electrolyte to produce a finished battery.
[0121] Example 4
[0122] The difference between Example 4 and Example 2 is that the compaction density is different. Specifically, the compaction density of Example 2 is 1.6 g / cm³. 3 Example 4 shows a compaction density of 1.55 g / cm³. 3 .
[0123] A negative electrode sheet, the structure of which includes:
[0124] current collector;
[0125] An active material layer is disposed on the surface of the current collector;
[0126] The number of the above-mentioned active material layers is 1, and the surface of the active material layer is provided with grooves;
[0127] The depth H of the aforementioned grooves and the thickness T of the aforementioned active material layer satisfy the following relationship:
[0128] 1 / 3T < H ≤ 2 / 3T;
[0129] The compaction density of the above-mentioned active material layer is P, and P is 1.55 g / cm³. 3 .
[0130] The volume fraction of the pores in the above-mentioned active material layer is η, where η is 3%.
[0131] A battery includes a positive electrode, a separator, an electrolyte, and the aforementioned negative electrode.
[0132] The above-mentioned method for preparing the positive electrode includes the following steps:
[0133] The active material LiCoO2, conductive agent acetylene black, conductive carbon nanotubes, and binder polyvinylidene fluoride (PVDF) were fully dispersed and uniformly coated onto an aluminum current collector in an N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold-pressed into strips to obtain the positive electrode sheet.
[0134] The method for preparing the above-mentioned diaphragm includes the following steps:
[0135] A ceramic mixture is coated onto the PE surface to serve as a release membrane.
[0136] The preparation process of the above-mentioned negative electrode includes the following steps:
[0137] A negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05), and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) were mixed in a weight ratio of 97.7:1.1:1.2 to prepare a negative electrode active material slurry. This slurry was then uniformly coated onto a composite current collector and compacted to a density of 1.55 g / cm³. 3 Cold pressing and slitting; using laser drilling equipment to create holes on the surface of the active material layer, with a hole volume ratio of 3%, to obtain the negative electrode sheet.
[0138] The preparation process of the above electrolyte includes the following steps:
[0139] An electrolyte is prepared by mixing and dissolving 40 wt.% of a first organic solvent, 30 wt.% of a second organic solvent, 15 wt.% of a lithium salt, and 15 wt.% of an additive.
[0140] The viscosity of the electrolyte is 0.806 mPa·s.
[0141] The manufacturing process of the above-mentioned battery includes the following steps:
[0142] The above-mentioned positive electrode sheet, separator, and negative electrode sheet are wound to form a bare cell, which is then packaged and injected with electrolyte to produce a finished battery.
[0143] Example 5
[0144] The difference between Example 5 and Example 2 is that the compaction density is different. Specifically, the compaction density of Example 2 is 1.6 g / cm³. 3 Example 5 shows a compaction density of 1.65 g / cm³. 3 .
[0145] A negative electrode sheet, the structure of which includes:
[0146] current collector;
[0147] An active material layer is disposed on the surface of the current collector;
[0148] The number of the above-mentioned active material layers is 1, and the surface of the active material layer is provided with grooves;
[0149] The depth H of the aforementioned grooves and the thickness T of the aforementioned active material layer satisfy the following relationship:
[0150] 1 / 3T < H ≤ 2 / 3T;
[0151] The compaction density of the above-mentioned active material layer is P, and P is 1.65 g / cm³. 3 .
[0152] The volume fraction of the pores in the above-mentioned active material layer is η, where η is 3%.
[0153] A battery includes a positive electrode, a separator, an electrolyte, and the aforementioned negative electrode.
[0154] The above-mentioned method for preparing the positive electrode includes the following steps:
[0155] The active material LiCoO2, conductive agent acetylene black, conductive carbon nanotubes, and binder polyvinylidene fluoride (PVDF) were fully dispersed and uniformly coated onto an aluminum current collector in an N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold-pressed into strips to obtain the positive electrode sheet.
[0156] The method for preparing the above-mentioned diaphragm includes the following steps:
[0157] A ceramic mixture is coated onto the PE surface to serve as a release membrane.
[0158] The preparation process of the above-mentioned negative electrode includes the following steps:
[0159] A negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05), and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) were mixed in a weight ratio of 97.7:1.1:1.2 to prepare a negative electrode active material slurry. This slurry was then uniformly coated onto a composite current collector and compacted to a density of 1.65 g / cm³. 3 Cold pressing and slitting; using laser drilling equipment to create holes on the surface of the active material layer, with a hole volume ratio of 3%, to obtain the negative electrode sheet.
[0160] The preparation process of the above electrolyte includes the following steps:
[0161] An electrolyte is prepared by mixing and dissolving 40 wt.% of a first organic solvent, 30 wt.% of a second organic solvent, 15 wt.% of a lithium salt, and 15 wt.% of an additive.
[0162] The viscosity of the electrolyte is 0.806 mPa·s.
[0163] The manufacturing process of the above-mentioned battery includes the following steps:
[0164] The above-mentioned positive electrode sheet, separator, and negative electrode sheet are wound to form a bare cell, which is then packaged and injected with electrolyte to produce a finished battery.
[0165] Example 6
[0166] The difference between Example 6 and Example 2 is that the compaction density is different. Specifically, the compaction density of Example 2 is 1.6 g / cm³. 3 Example 6 shows a compaction density of 1.70 g / cm³. 3 .
[0167] A negative electrode sheet, the structure of which includes:
[0168] current collector;
[0169] An active material layer is disposed on the surface of the current collector;
[0170] The number of the above-mentioned active material layers is 1, and the surface of the active material layer is provided with grooves;
[0171] The depth H of the aforementioned grooves and the thickness T of the aforementioned active material layer satisfy the following relationship:
[0172] 1 / 3T < H ≤ 2 / 3T;
[0173] The compaction density of the above-mentioned active material layer is P, and P is 1.70 g / cm³. 3 .
[0174] The volume fraction of the pores in the above-mentioned active material layer is η, where η is 3%.
[0175] A battery includes a positive electrode, a separator, an electrolyte, and the aforementioned negative electrode.
[0176] The above-mentioned method for preparing the positive electrode includes the following steps:
[0177] The active material LiCoO2, conductive agent acetylene black, conductive carbon nanotubes, and binder polyvinylidene fluoride (PVDF) were fully dispersed and uniformly coated onto an aluminum current collector in an N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold-pressed into strips to obtain the positive electrode sheet.
[0178] The method for preparing the above-mentioned diaphragm includes the following steps:
[0179] A ceramic mixture is coated onto the PE surface to serve as a release membrane.
[0180] The preparation process of the above-mentioned negative electrode includes the following steps:
[0181] A negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05), and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) were mixed in a weight ratio of 97.7:1.1:1.2 to prepare a negative electrode active material slurry. This slurry was then uniformly coated onto a composite current collector and compacted to a density of 1.7 g / cm³. 3 Cold pressing and slitting; using laser drilling equipment to create holes on the surface of the active material layer, with a hole volume ratio of 3%, to obtain the negative electrode sheet.
[0182] The preparation process of the above electrolyte includes the following steps:
[0183] An electrolyte is prepared by mixing and dissolving 40 wt.% of a first organic solvent, 30 wt.% of a second organic solvent, 15 wt.% of a lithium salt, and 15 wt.% of an additive.
[0184] The viscosity of the electrolyte is 0.806 mPa·s.
[0185] The manufacturing process of the above-mentioned battery includes the following steps:
[0186] The above-mentioned positive electrode sheet, separator, and negative electrode sheet are wound to form a bare cell, which is then packaged and injected with electrolyte to produce a finished battery.
[0187] Example 7
[0188] The difference between Example 7 and Example 2 includes the compaction density. Specifically, the compaction density of Example 2 is 1.6 g / cm³. 3 Example 7 shows a compaction density of 1.75 g / cm³. 3 .
[0189] A negative electrode sheet, the structure of which includes:
[0190] current collector;
[0191] An active material layer is disposed on the surface of the current collector;
[0192] The number of the above-mentioned active material layers is 1, and the surface of the active material layer is provided with grooves;
[0193] The depth H of the aforementioned grooves and the thickness T of the aforementioned active material layer satisfy the following relationship:
[0194] 1 / 3T < H ≤ 2 / 3T;
[0195] The compaction density of the above-mentioned active material layer is P, and P is 1.75 g / cm³. 3 .
[0196] The volume fraction of the pores in the above-mentioned active material layer is η, where η is 3%.
[0197] A battery includes a positive electrode, a separator, an electrolyte, and the aforementioned negative electrode.
[0198] The above-mentioned method for preparing the positive electrode includes the following steps:
[0199] The active material LiCoO2, conductive agent acetylene black, conductive carbon nanotubes, and binder polyvinylidene fluoride (PVDF) were fully dispersed and uniformly coated onto an aluminum current collector in an N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold-pressed into strips to obtain the positive electrode sheet.
[0200] The method for preparing the above-mentioned diaphragm includes the following steps:
[0201] A ceramic mixture is coated onto the PE surface to serve as a release membrane.
[0202] The preparation process of the above-mentioned negative electrode includes the following steps:
[0203] A negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05), and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) were mixed in a weight ratio of 97.7:1.1:1.2 to prepare a negative electrode active material slurry. This slurry was then uniformly coated onto a composite current collector and compacted to a density of 1.75 g / cm³. 3 Cold pressing and slitting; using laser drilling equipment to create holes on the surface of the active material layer, with a hole volume ratio of 3%, to obtain the negative electrode sheet.
[0204] The preparation process of the above electrolyte includes the following steps:
[0205] An electrolyte is prepared by mixing and dissolving 40 wt.% of a first organic solvent, 30 wt.% of a second organic solvent, 15 wt.% of a lithium salt, and 15 wt.% of an additive.
[0206] The viscosity of the electrolyte is 0.806 mPa·s.
[0207] The manufacturing process of the above-mentioned battery includes the following steps:
[0208] The above-mentioned positive electrode sheet, separator, and negative electrode sheet are wound to form a bare cell, which is then packaged and injected with electrolyte to produce a finished battery.
[0209] Example 8
[0210] The differences between Example 8 and Example 5 include: the amount of the first organic solvent, the amount of the second organic solvent, the lithium salt concentration, the additive concentration, and the electrolyte viscosity. Specifically, in Example 5, the amount of the first organic solvent is 40 wt%, the amount of the second organic solvent is 30 wt%, the lithium salt concentration is 15 wt%, the additive concentration is 15 wt%, and the electrolyte viscosity is 0.806 mPa·s; in Example 8, the amount of the first organic solvent is 45 wt%, the amount of the second organic solvent is 40 wt%, the lithium salt concentration is 10 wt%, the additive concentration is 5 wt%, and the electrolyte viscosity is 0.400 mPa·s.
[0211] A negative electrode sheet, the structure of which includes:
[0212] current collector;
[0213] An active material layer is disposed on the surface of the current collector;
[0214] The number of the above-mentioned active material layers is 1, and the surface of the active material layer is provided with grooves;
[0215] The depth H of the aforementioned grooves and the thickness T of the aforementioned active material layer satisfy the following relationship:
[0216] 1 / 3T < H ≤ 2 / 3T;
[0217] The compaction density of the above-mentioned active material layer is P, and P is 1.65 g / cm³. 3 .
[0218] The volume fraction of the pores in the above-mentioned active material layer is η, where η is 3%.
[0219] A battery includes a positive electrode, a separator, an electrolyte, and the aforementioned negative electrode.
[0220] The above-mentioned method for preparing the positive electrode includes the following steps:
[0221] The active material LiCoO2, conductive agent acetylene black, conductive carbon nanotubes, and binder polyvinylidene fluoride (PVDF) were fully dispersed and uniformly coated onto an aluminum current collector in an N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold-pressed into strips to obtain the positive electrode sheet.
[0222] The method for preparing the above-mentioned diaphragm includes the following steps:
[0223] A ceramic mixture is coated onto the PE surface to serve as a release membrane.
[0224] The preparation process of the above-mentioned negative electrode includes the following steps:
[0225] A negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05), and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) were mixed in a weight ratio of 97.7:1.1:1.2 to prepare a negative electrode active material slurry. This slurry was then uniformly coated onto a composite current collector and compacted to a density of 1.65 g / cm³. 3 Cold pressing and slitting; using laser drilling equipment to create holes on the surface of the active material layer, with a hole volume ratio of 3%, to obtain the negative electrode sheet.
[0226] The preparation process of the above electrolyte includes the following steps:
[0227] An electrolyte is prepared by mixing and dissolving 45 wt.% of a first organic solvent, 40 wt.% of a second organic solvent, 10 wt.% of a lithium salt, and 5 wt.% of an additive.
[0228] The viscosity of the electrolyte is 0.400 mPa·s.
[0229] The manufacturing process of the above-mentioned battery includes the following steps:
[0230] The above-mentioned positive electrode sheet, separator, and negative electrode sheet are wound to form a bare cell, which is then packaged and injected with electrolyte to produce a finished battery.
[0231] Example 9
[0232] The differences between Example 9 and Example 5 include: different amounts of the first organic solvent, lithium salt concentration, additive concentration, and electrolyte viscosity. Specifically, in Example 5, the amount of the first organic solvent was 40 wt%, the lithium salt concentration was 15 wt%, the additive concentration was 15 wt%, and the electrolyte viscosity was 0.806 mPa·s; in Example 9, the amount of the first organic solvent was 30 wt%, the lithium salt concentration was 20 wt%, the additive concentration was 20 wt%, and the electrolyte viscosity was 2.000 mPa·s.
[0233] A negative electrode sheet, the structure of which includes:
[0234] current collector;
[0235] An active material layer is disposed on the surface of the current collector;
[0236] The number of the above-mentioned active material layers is 1, and the surface of the active material layer is provided with grooves;
[0237] The depth H of the aforementioned grooves and the thickness T of the aforementioned active material layer satisfy the following relationship:
[0238] 1 / 3T < H ≤ 2 / 3T;
[0239] The compaction density of the above-mentioned active material layer is P, and P is 1.65 g / cm³.3 .
[0240] The volume fraction of the pores in the above-mentioned active material layer is η, where η is 3%.
[0241] A battery includes a positive electrode, a separator, an electrolyte, and the aforementioned negative electrode.
[0242] The above-mentioned method for preparing the positive electrode includes the following steps:
[0243] The active material LiCoO2, conductive agent acetylene black, conductive carbon nanotubes, and binder polyvinylidene fluoride (PVDF) were fully dispersed and uniformly coated onto an aluminum current collector in an N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold-pressed into strips to obtain the positive electrode sheet.
[0244] The method for preparing the above-mentioned diaphragm includes the following steps:
[0245] A ceramic mixture is coated onto the PE surface to serve as a release membrane.
[0246] The preparation process of the above-mentioned negative electrode includes the following steps:
[0247] A negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05), and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) were mixed in a weight ratio of 97.7:1.1:1.2 to prepare a negative electrode active material slurry. This slurry was then uniformly coated onto a composite current collector and compacted to a density of 1.65 g / cm³. 3 Cold pressing and slitting; using laser drilling equipment to create holes on the surface of the active material layer, with a hole volume ratio of 3%, to obtain the negative electrode sheet.
[0248] The preparation process of the above electrolyte includes the following steps:
[0249] An electrolyte is prepared by mixing and dissolving 30 wt.% of a first organic solvent, 30 wt.% of a second organic solvent, 20 wt.% of a lithium salt, and 20 wt.% of an additive.
[0250] The viscosity of the electrolyte is 2.000 mPa·s.
[0251] The manufacturing process of the above-mentioned battery includes the following steps:
[0252] The above-mentioned positive electrode sheet, separator, and negative electrode sheet are wound to form a bare cell, which is then packaged and injected with electrolyte to produce a finished battery.
[0253] Example 10
[0254] The differences between Example 10 and Example 9 include the different amounts of the first organic solvent, the second organic solvent, and the electrolyte viscosity. Specifically, in Example 9, the amount of the first organic solvent was 30 wt%, the amount of the second organic solvent was 30 wt%, and the electrolyte viscosity was 2.000 mPa·s; in Example 10, the amount of the first organic solvent was 45 wt%, the amount of the second organic solvent was 15 wt%, and the electrolyte viscosity was 1.379 mPa·s.
[0255] A negative electrode sheet, the structure of which includes:
[0256] current collector;
[0257] An active material layer is disposed on the surface of the current collector;
[0258] The number of the above-mentioned active material layers is 1, and the surface of the active material layer is provided with grooves;
[0259] The depth H of the aforementioned grooves and the thickness T of the aforementioned active material layer satisfy the following relationship:
[0260] 1 / 3T < H ≤ 2 / 3T;
[0261] The compaction density of the above-mentioned active material layer is P, and P is 1.65 g / cm³. 3 .
[0262] The volume fraction of the pores in the above-mentioned active material layer is η, where η is 3%.
[0263] A battery includes a positive electrode, a separator, an electrolyte, and the aforementioned negative electrode.
[0264] The above-mentioned method for preparing the positive electrode includes the following steps:
[0265] The active material LiCoO2, conductive agent acetylene black, conductive carbon nanotubes, and binder polyvinylidene fluoride (PVDF) were fully dispersed and uniformly coated onto an aluminum current collector in an N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold-pressed into strips to obtain the positive electrode sheet.
[0266] The method for preparing the above-mentioned diaphragm includes the following steps:
[0267] A ceramic mixture is coated onto the PE surface to serve as a release membrane.
[0268] The preparation process of the above-mentioned negative electrode includes the following steps:
[0269] A negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05), and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) were mixed in a weight ratio of 97.7:1.1:1.2 to prepare a negative electrode active material slurry. This slurry was then uniformly coated onto a composite current collector and compacted to a density of 1.65 g / cm³. 3 Cold pressing and slitting; using laser drilling equipment to create holes on the surface of the active material layer, with a hole volume ratio of 3%, to obtain the negative electrode sheet.
[0270] The preparation process of the above electrolyte includes the following steps:
[0271] An electrolyte is prepared by mixing and dissolving 45 wt.% of a first organic solvent, 15 wt.% of a second organic solvent, 20 wt.% of a lithium salt, and 20 wt.% of an additive.
[0272] The viscosity of the electrolyte is 1.379 mPa·s.
[0273] The manufacturing process of the above-mentioned battery includes the following steps:
[0274] The above-mentioned positive electrode sheet, separator, and negative electrode sheet are wound to form a bare cell, which is then packaged and injected with electrolyte to produce a finished battery.
[0275] Example 11
[0276] The difference between Example 11 and Example 10 includes the difference in pressure relief compaction density. Specifically, the pressure relief compaction density of Example 10 is 1.44 g / cm³. 3 The depressurization compaction density of Example 11 is 1.48 g / cm³. 3 .
[0277] A negative electrode sheet, the structure of which includes:
[0278] current collector;
[0279] An active material layer is disposed on the surface of the current collector;
[0280] The number of the above-mentioned active material layers is 1, and the surface of the active material layer is provided with grooves;
[0281] The depth H of the aforementioned grooves and the thickness T of the aforementioned active material layer satisfy the following relationship:
[0282] 1 / 3T < H ≤ 2 / 3T;
[0283] The compaction density of the above-mentioned active material layer is P, and P is 1.65 g / cm³. 3 .
[0284] The volume fraction of the pores in the above-mentioned active material layer is η, where η is 3%.
[0285] A battery includes a positive electrode, a separator, an electrolyte, and the aforementioned negative electrode.
[0286] The above-mentioned method for preparing the positive electrode includes the following steps:
[0287] The active material LiCoO2, conductive agent acetylene black, conductive carbon nanotubes, and binder polyvinylidene fluoride (PVDF) were fully dispersed and uniformly coated onto an aluminum current collector in an N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold-pressed into strips to obtain the positive electrode sheet.
[0288] The method for preparing the above-mentioned diaphragm includes the following steps:
[0289] A ceramic mixture is coated onto the PE surface to serve as a release membrane.
[0290] The preparation process of the above-mentioned negative electrode includes the following steps:
[0291] A negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05), and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) were mixed in a weight ratio of 97.7:1.1:1.2 to prepare a negative electrode active material slurry. This slurry was then uniformly coated onto a composite current collector and compacted to a density of 1.65 g / cm³. 3 Cold pressing and slitting; using laser drilling equipment to create holes on the surface of the active material layer, with a hole volume ratio of 3%, to obtain the negative electrode sheet.
[0292] The preparation process of the above electrolyte includes the following steps:
[0293] An electrolyte is prepared by mixing and dissolving 45 wt.% of a first organic solvent, 15 wt.% of a second organic solvent, 20 wt.% of a lithium salt, and 20 wt.% of an additive.
[0294] The viscosity of the electrolyte is 1.379 mPa·s.
[0295] The manufacturing process of the above-mentioned battery includes the following steps:
[0296] The above-mentioned positive electrode sheet, separator, and negative electrode sheet are wound to form a bare cell, which is then packaged and injected with electrolyte to produce a finished battery.
[0297] Example 12
[0298] The difference between Example 12 and Example 10 includes the difference in the volume fraction of the pores / grooves. Specifically, the volume fraction of the pores / grooves in Example 10 is 3%, while the volume fraction in Example 12 is 1%.
[0299] A negative electrode sheet, the structure of which includes:
[0300] current collector;
[0301] An active material layer is disposed on the surface of the current collector;
[0302] The number of the above-mentioned active material layers is 1, and the surface of the active material layer is provided with grooves;
[0303] The depth H of the aforementioned grooves and the thickness T of the aforementioned active material layer satisfy the following relationship:
[0304] 1 / 3T < H ≤ 2 / 3T;
[0305] The compaction density of the above-mentioned active material layer is P, and P is 1.65 g / cm³. 3 .
[0306] The volume fraction of the pores in the above-mentioned active material layer is η, where η is 1%.
[0307] A battery includes a positive electrode, a separator, an electrolyte, and the aforementioned negative electrode.
[0308] The above-mentioned method for preparing the positive electrode includes the following steps:
[0309] The active material LiCoO2, conductive agent acetylene black, conductive carbon nanotubes, and binder polyvinylidene fluoride (PVDF) were fully dispersed and uniformly coated onto an aluminum current collector in an N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold-pressed into strips to obtain the positive electrode sheet.
[0310] The method for preparing the above-mentioned diaphragm includes the following steps:
[0311] A ceramic mixture is coated onto the PE surface to serve as a release membrane.
[0312] The preparation process of the above-mentioned negative electrode includes the following steps:
[0313] A negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05), and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) were mixed in a weight ratio of 97.7:1.1:1.2 to prepare a negative electrode active material slurry. This slurry was then uniformly coated onto a composite current collector and compacted to a density of 1.65 g / cm³. 3 Cold pressing and slitting; using laser drilling equipment to create holes on the surface of the active material layer, with a hole volume ratio of 1%, to obtain the negative electrode sheet.
[0314] The preparation process of the above electrolyte includes the following steps:
[0315] An electrolyte is prepared by mixing and dissolving 45 wt.% of a first organic solvent, 15 wt.% of a second organic solvent, 20 wt.% of a lithium salt, and 20 wt.% of an additive.
[0316] The viscosity of the electrolyte is 1.379 mPa·s.
[0317] The manufacturing process of the above-mentioned battery includes the following steps:
[0318] The above-mentioned positive electrode sheet, separator, and negative electrode sheet are wound to form a bare cell, which is then packaged and injected with electrolyte to produce a finished battery.
[0319] Example 13
[0320] The difference between Example 13 and Example 7 lies in the mass percentage of the first organic solvent, the lithium salt concentration, the additive concentration, and the electrolyte viscosity. Specifically, in Example 7, the mass percentage of the first organic solvent is 40 wt.%, the lithium salt concentration is 15 wt.%, the additive concentration is 15 wt.%, and the electrolyte viscosity is 0.806 wt.%; in Example 13, the mass percentage of the first organic solvent is 30 wt.%, the lithium salt concentration is 20 wt.%, the additive concentration is 20 wt.%, and the electrolyte viscosity is 2.000 mPa·s.
[0321] A negative electrode sheet, the structure of which includes:
[0322] current collector;
[0323] An active material layer is disposed on the surface of the current collector;
[0324] The number of the above-mentioned active material layers is 1, and the surface of the active material layer is provided with grooves;
[0325] The depth H of the aforementioned grooves and the thickness T of the aforementioned active material layer satisfy the following relationship:
[0326] 1 / 3T < H ≤ 2 / 3T;
[0327] The compaction density of the above-mentioned active material layer is P, and P is 1.75 g / cm³. 3 .
[0328] The volume fraction of the pores in the above-mentioned active material layer is η, where η is 3%.
[0329] A battery includes a positive electrode, a separator, an electrolyte, and the aforementioned negative electrode.
[0330] The above-mentioned method for preparing the positive electrode includes the following steps:
[0331] The active material LiCoO2, conductive agent acetylene black, conductive carbon nanotubes, and binder polyvinylidene fluoride (PVDF) were fully dispersed and uniformly coated onto an aluminum current collector in an N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold-pressed into strips to obtain the positive electrode sheet.
[0332] The method for preparing the above-mentioned diaphragm includes the following steps:
[0333] A ceramic mixture is coated onto the PE surface to serve as a release membrane.
[0334] The preparation process of the above-mentioned negative electrode includes the following steps:
[0335] A negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05), and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) were mixed in a weight ratio of 97.7:1.1:1.2 to prepare a negative electrode active material slurry. This slurry was then uniformly coated onto a composite current collector and compacted to a density of 1.75 g / cm³. 3 Cold pressing and slitting; using laser drilling equipment to create holes on the surface of the active material layer, with a hole volume ratio of 3%, to obtain the negative electrode sheet.
[0336] The preparation process of the above electrolyte includes the following steps:
[0337] An electrolyte is prepared by mixing and dissolving 30 wt.% of a first organic solvent, 30 wt.% of a second organic solvent, 20 wt.% of a lithium salt, and 20 wt.% of an additive.
[0338] The viscosity of the electrolyte is 2.000 mPa·s.
[0339] The manufacturing process of the above-mentioned battery includes the following steps:
[0340] The above-mentioned positive electrode sheet, separator, and negative electrode sheet are wound to form a bare cell, which is then packaged and injected with electrolyte to produce a finished battery.
[0341] Comparative Example 1
[0342] The difference between Comparative Example 1 and Example 5 includes that there are no pores or grooves in the active material layer in Comparative Example 1.
[0343] Comparative Example 2
[0344] The differences between Comparative Example 2 and Example 9 include the different amounts of the first organic solvent, the second organic solvent, and the electrolyte viscosity. Specifically, in Example 9, the amount of the first organic solvent was 30 wt%, the amount of the second organic solvent was 30 wt%, and the electrolyte viscosity was 2.000 mPa·s; in Comparative Example 2, the amount of the first organic solvent was 25 wt%, the amount of the second organic solvent was 35 wt%, and the electrolyte viscosity was 2.291 mPa·s.
[0345] Comparative Example 3
[0346] The difference between Comparative Example 3 and Example 5 includes the difference in pressure relief compaction density. Specifically, the pressure relief compaction density of Example 5 is 1.44 g / cm³. 3 The depressurized compaction density of Comparative Example 3 is 1.60 g / cm³. 3 .
[0347] Comparative Example 4
[0348] The difference between Comparative Example 4 and Example 5 includes the difference in the cavity volume fraction. Specifically, the cavity volume fraction of Example 5 is 3%, while that of Comparative Example 4 is 6%.
[0349] The parameter settings for Examples 1-13 and Comparative Examples 1-4 are shown in Table 1-2.
[0350] Table 1
[0351]
[0352] In Table 1, the values of the first organic solvent W1, the second organic solvent W2, the lithium salt concentration, and the additive concentration mainly affect the electrolyte viscosity ω.
[0353] Table 2
[0354]
[0355] The parameters recorded in Table 2 are mainly the parameters of the orifice and groove, which affect the orifice and groove volume fraction η in Table 1. When the parameters in Table 2 are adjusted, the corresponding orifice and groove volume fraction η in Table 1 will be affected.
[0356] Using the parameters listed in Table 1, calculate whether P, η, W1, and ω satisfy the following relationship: 2.8 ≤ (P*ω) / (10*η*W1) ≤ 50; and calculate whether β, P, and ω satisfy the following relationship: 0.05 ≤ ω*(P-β) / P ≤ 0.23. The calculation results are shown in Table 3.
[0357] Table 3
[0358]
[0359]
[0360] As can be seen from Table 3, Examples 12, Comparative Examples 1 and 2 do not satisfy 2.8≤(P*ω) / (10*η*W1)≤50; Examples 13, Comparative Examples 1, 2 and 3 do not satisfy 0.05≤ω*(P-β) / P≤0.23.
[0361] Performance testing:
[0362] The batteries prepared in Examples 1-13 and Comparative Examples 1-4 were subjected to the following tests, and the test results are shown in Table 4.
[0363] Pressure-relief compaction density: Weigh 1.00g ± 0.05g of negative electrode active material powder, then place the sample in a powder compaction density meter and test at a pressure of 5 tons. The pressure-relief compaction density is β, the mass of the negative electrode active material is M, the force-bearing area of the negative electrode active material is S, and the thickness of the powder sample after pressure relief is H. The formula for calculating the pressure-relief compaction density is as follows: β = M / (S × H).
[0364] Electrolyte retention range: After vacuum drying for a period of time, electrolyte is injected into the battery, and the initial injection volume is recorded. After a period of electrolyte immersion treatment, excess electrolyte is extracted from the battery, and the amount extracted is recorded. Therefore, electrolyte retention = injected volume - extracted volume, with a value taken from 100 batteries.
[0365] Loop testing method:
[0366] In an environment of 25℃ / 45℃, perform cyclic testing according to the following method: charging mode: 3.5C CC to 4.25V, 2.8C CC to 4.35V, CV to 1.8C, 1.8C CC to 4.4V, CV to 1.5C, 1.5C CC to 4.5V, CV to 1.2C, 1.2C CC to 4.55V, CV to 0.26C; discharging mode: 0.7C DC to 3.0V.
[0367] 500-week capacity retention = discharge capacity in week 500 / discharge capacity in week 1 * 100%;
[0368] 300-week capacity retention = discharge capacity in week 300 / discharge capacity in week 1 * 100%;
[0369] -10℃ Low Temperature Discharge Test: At 25℃, charge to 4.5V at 0.5C, cut-off current 0.02C, rest for 5 minutes, discharge to 3.0V at 0.2C; then charge to 4.5V at 0.5C, cut-off current 0.02C; set the test temperature to -10℃, rest for 120 minutes, discharge to 3.0V at 0.2C.
[0370] Low-temperature discharge capacity ratio = -10℃ discharge capacity / 25℃ discharge capacity * 100%.
[0371] Table 4
[0372]
[0373]
[0374] As can be seen from Examples 1-10, when the battery parameters P, ω, η, W1, and β satisfy the relationships 2.8 ≤ (P*ω) / (10*η*W1) ≤ 50 and 0.05 ≤ ω*(P-β) / P ≤ 0.23, and all parameters are within the range of this application, the battery can have a more stable electrolyte retention capacity, and at the same time, the battery has better high and low temperature performance. This expands the selection window for electrolyte types, ensuring good electrolyte retention stability and taking into account both high and low temperature comprehensive performance. If the parameters do not meet the above relationship range, the electrolyte retention is unstable, and the high and low temperature performance is also poor.
[0375] As can be seen from Examples 1-10 and Comparative Examples 1-4, the presence of grooves on the electrode surface is beneficial for the electrode to have good electrolyte retention stability, while also providing a path for rapid lithium-ion transport. Therefore, under high actual density, the presence of grooves on the electrode surface can appropriately increase the electrolyte viscosity, giving the electrode good electrolyte retention stability and excellent performance at high or low temperatures. Without grooves, the stability and average value of electrolyte retention decrease significantly, and the high and low temperature performance degrades severely. If the groove volume fraction of the negative electrode is too high, it will affect the N / P ratio of the positive and negative electrodes, significantly reducing the high and low temperature cycle life. A high groove volume fraction results in a greater reduction in active material and more free electrolyte stored in the grooves. When vacuuming out excess electrolyte, the electrolyte loss is significant, and it also leads to unstable electrolyte retention.
[0376] As can be seen from Examples 1-10 and Comparative Example 2, low viscosity results in poor high-temperature performance. This is mainly because low viscosity leads to increased side reactions at high temperatures. If the viscosity is too high, the electrolyte viscosity is too large, lithium-ion conduction is hindered, lithium deposition is easy, wettability is poor, and the stability of liquid retention is affected, as well as low-temperature discharge and high-low temperature cycling performance.
[0377] As can be seen from Examples 1-10 and Comparative Example 3, the depressurized compaction density is between 1.37 and 1.52 g / cm³. 3 Within the specified range, the contact between substances in the active material layers is good, the structure of the active material is stable, and the gaps between particles are fixed, which helps to improve the stability of electrolyte retention. This, combined with compaction density and electrolyte viscosity, further enhances the stability of electrolyte retention and high / low temperature cycling performance. However, when the pressure relief and compaction are too high, the structural stability of the active material is lower, and the electrolyte retention stability and high / low temperature performance also decrease.
[0378] As can be seen from Examples 1-12, if the parameters P, ω, η, and W1 are within the range of this application, but do not satisfy the relationship 2.8 ≤ (P*ω) / (10*η*W1) ≤ 50, the electrolyte retention stability and high and low temperature cycling performance will also decrease. The parameters P, ω, η, and W1 need to cooperate with each other to improve the electrolyte retention stability and improve the high and low temperature cycling performance.
[0379] As can be seen from Examples 1 to 13, if the parameters P, ω, and β are within the range of this application, but do not satisfy the relationship: 0.05≤ω*(P-β) / P≤0.23, the electrolyte retention stability and high and low temperature cycling performance will also decrease. The parameters P, ω, and β need to cooperate with each other to improve the electrolyte retention stability and improve the high and low temperature cycling performance.
[0380] In this design, the porous grooves on the active layer of the anode not only facilitate electrolyte flow, effectively improving the wettability of the high-voltage solid electrode and reducing its permeation requirements, but also broaden the selection and proportioning options for solvents and additives. Furthermore, they create channels for rapid lithium-ion transport, mitigating lithium-ion deposition caused by the low porosity of the high-voltage solid electrode. By appropriately adjusting the solvent ratio of the electrolyte based on the pore volume fraction of the anode active material layer, the overall performance of the battery can be improved while maintaining wettability, thus meeting market demands.
[0381] The above are merely embodiments of the present invention and do not limit the patent scope of the present invention. Any equivalent modifications made based on the content of the present invention specification, or direct or indirect applications in related technical fields, are similarly included within the patent protection scope of the present invention.
Claims
1. A battery, characterized in that: It includes a positive electrode, a separator, an electrolyte, and a negative electrode, wherein the structure of the negative electrode includes: current collector; An active material layer is disposed on the surface of the current collector; The number of active material layers is greater than or equal to 1, and at least one active material layer has a hole groove on its surface; The depth H of the groove and the thickness T of the active material layer satisfy the following relationship: 1 / 3T < H ≤ 2 / 3T; The compacted density of the active material layer is P, P satisfies the following relationship: 1.55≤P≤1.75 g / cm 3 ; The compaction density of the active material layer of the negative electrode is P. The negative electrode includes an active material layer with pores and grooves. The volume fraction of the pores and grooves is η. The viscosity of the electrolyte is ω. P, η, W1, and ω satisfy the following relationship: 2.8 ≤ (P ω) / (10 η W1)≤50; The volume fraction of the pores in the active material layer is η, where η satisfies the following relationship: 1% ≤ η ≤ 5%; The electrolyte comprises a non-aqueous solvent, a lithium salt, and additives. The non-aqueous solvent includes a first organic solvent and a second organic solvent. The first organic solvent has a mass fraction of W1 in the electrolyte, where W1 satisfies the following relationship: 30 wt.% ≤ W1 ≤ 45 wt.%. The second organic solvent has a mass fraction of W2 in the electrolyte, where W2 satisfies the following relationship: 15 wt.% ≤ W2 ≤ 40 wt.%, and W2 ≤ W1 ≤ 3W2. ω satisfies the following relationship: 0.4 ≤ ω ≤ 2 mPa•s; The pressure relief compaction density of the negative electrode is β, where 1.37 ≤ β ≤ 1.52 g / cm³. 3 The test pressure was 5 tons.
2. The battery according to claim 1, characterized in that: The perforation width of the grooves in the active material layer is R, and R satisfies the following relationship: 50≤R≤140μm.
3. The battery according to claim 1, characterized in that: The spacing between the pores in the active material layer is L, and L satisfies the following relationship: 1.0≤L≤2.5mm.
4. The battery according to claim 1, characterized in that: The angle between the pores and the negative electrode in the active material layer is θ, and θ satisfies the following relationship: 85°≤θ≤95°.
5. The battery according to claim 1, characterized in that: The following relationship exists between the pressure relief compaction density β of the negative electrode, the compaction density P of the active material layer, and the viscosity ω of the electrolyte: 0.05 ≤ ω (P- β ) / P≤0.
23.
6. The battery according to claim 1, characterized in that: The first organic solvent includes at least one of carbonate organic solvents and carboxylic acid ester organic solvents; the second organic solvent includes at least one of sulfur solvents, fluorinated solvents, sulfone solvents and nitrile solvents.
Citation Information
Patent Citations
Composite negative plate and preparation method thereof, and secondary battery
CN113644231A
Lithium secondary battery
CN113711408A