A sodium ion battery and a formation method thereof
Through a combination of five steps of charging and standing, the formation process of sodium-ion batteries is optimized, which solves the problems of inconsistent SEI film thickness and high internal resistance, improves battery performance and production efficiency, and achieves the formation of high-quality SEI films. and battery performance improvements.
Patent Information
- Application Number
- CN202410034411.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-09
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-01-09
AI Technical Summary
The existing sodium-ion battery formation process results in inconsistent SEI film thickness, increased internal resistance, excessive gas generation, and high risk of sodium precipitation at the interface, resulting in low first-efficiency battery capacity, poor cycle performance and storage performance, low production efficiency, and high cost.
The five step charging method is adopted, combined with standing at room temperature and high temperature, and the charging current, SOC value and standing time are adjusted to shorten the total formation time and optimize the formation process of the SEI film.
It improves the quality of the SEI film and battery performance, shortens the formation time, reduces production costs, enhances the conductivity of sodium ions and battery cycle performance, and improves high-temperature storage performance.
Smart Images

Figure CN117855647B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and more specifically to the technical field of sodium ion batteries and formation methods thereof. Background Art
[0002] Sodium-ion batteries are considered to be the secondary batteries that will replace lithium-ion batteries and be widely used in the field of energy storage in the future due to their advantages such as low cost, good safety performance, good low-temperature performance, and long cycle life. At present, in the production and manufacturing of sodium-ion batteries, in order to ensure the formation of a better and more stable SEI film, the battery formation adopts a method of using a small rate current in the early stage and then charging in a step-by-step manner to 100% SOC. This makes the entire formation cycle longer, the thickness consistency of the formed SEI film is poor, the internal resistance increases significantly, and more gas is generated during the formation process, resulting in an increased risk of sodium precipitation on the interface. The final manufactured battery has a low initial capacity, poor cycle performance and storage performance. In addition, the longer production cycle of the formation process also reduces production efficiency and increases manufacturing costs. Therefore, how to optimize the formation process and improve the performance and production efficiency of sodium-ion batteries is a technical problem that needs to be solved urgently. Summary of the invention
[0003] The purpose of the present invention is to solve the above technical problems and provide a sodium ion battery and a formation method thereof, which aims to reduce the total formation time of the sodium ion battery and improve the quality of SIE film formation and battery performance.
[0004] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:
[0005] The first aspect of the present invention provides a sodium ion battery formation method, wherein after the sodium ion battery core is filled with liquid and left to stand at room temperature and at high temperature for a set time, the battery is charged five times in a step-by-step manner at a formation pressure and a formation temperature, and the five-step charging comprises the following steps:
[0006] Step H1, charging the sodium ion battery with a constant current continuously according to a first charging condition to reach a first formation stage; the first charging condition is to reach a first charging current, and the first formation stage is when the SOC value of the sodium ion battery reaches a first SOC;
[0007] Step H2, leaving the mixture to stand for a first preset time;
[0008] Step H3, after the battery is left to stand for a first preset time, the sodium ion battery is continuously charged with a constant current according to a second charging condition to reach a second formation stage; the second charging condition is to reach a second charging current; the second formation stage is when the SOC value of the sodium ion battery reaches a second SOC;
[0009] Step H4, leaving it alone for a second preset time;
[0010] Step H5, after standing for a second preset time, the sodium ion battery is continuously charged at a constant current according to a third charging condition to reach a third formation stage; the third charging condition is to reach a third charging current; the third formation stage is when the SOC value of the sodium ion battery reaches a third SOC;
[0011] Step H6, leaving it alone for a third preset time;
[0012] Step H7, after standing for a third preset time, continuously charging the sodium ion battery with a constant current according to a fourth charging condition to reach a fourth formation stage; the fourth charging condition is to reach a fourth charging current; the fourth formation stage is when the SOC value of the sodium ion battery reaches a fourth SOC;
[0013] Step H8, leaving it alone for a fourth preset time period;
[0014] Step H9, after standing for a fourth preset time period, continuously charging the sodium ion battery with a constant current according to a fifth charging condition to reach a fifth formation stage; the fifth charging condition is to reach a fifth charging current; the fifth formation stage is when the SOC value of the sodium ion battery reaches a fifth SOC;
[0015] After the fifth preset time, the transformation is completed.
[0016] Specifically, the formation process of sodium-ion batteries aims to form a high-quality SEI film, and the quality of the SEI film is closely related to factors such as temperature, charging rate, charging time, and charging depth in the formation process. In theory, during the first formation of a sodium-ion battery, the first layer to be formed between the main material and the electrolyte of the sodium-ion battery is an inorganic layer. The formation of the inorganic layer is a two-electron reaction process, which makes the inorganic layer dense and can effectively isolate the direct contact between the electrolyte and the main material, thereby preventing the electrolyte from further reduction and decomposition.
[0017] In this scheme, after the sodium-ion battery is filled with liquid at room temperature and then left at high temperature for a set time, the sodium-ion battery is charged in a step-by-step manner five times at the formation pressure and formation temperature. This shortens the total formation time of the sodium-ion battery, while improving the quality of SIE film formation and the performance of the ion battery.
[0018] In one embodiment, the room temperature standing temperature is 25±5° C., and the room temperature standing time is 6 to 8 hours.
[0019] Specifically, the room temperature standing temperature is 25±5°C, such as 20°C, 25°C or 30°C, etc.; the standing time is 6 to 8h, such as 6h, 7h or 8h, etc.
[0020] In one embodiment, the high temperature standing temperature is 45±5° C., and the high temperature standing time is 8 to 16 hours.
[0021] Specifically, the high temperature standing temperature is 45±5°C, for example, 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C or 50°C; the high temperature standing time is 8 to 16h, for example, 8h, 12h or 16h.
[0022] Among them, during the standing process, the preferred combination of room temperature and high temperature standing temperature and time is: room temperature standing temperature is 25°C, room temperature standing time is 6 hours, high temperature standing temperature is 45°C, and high temperature standing time is 12 hours.
[0023] In one embodiment, the formation pressure is 300-600 kgf.
[0024] Specifically, the forming pressure is 300 to 600 kgf, for example, 300 kgf, 400 kgf, 500 kgf, or 600 kgf.
[0025] In one embodiment, the formation temperature is 30-45°C.
[0026] Specifically, the formation temperature is 30 to 45°C, for example, 30°C, 35°C, 40°C, or 50°C, and the preferred formation temperature is 30°C.
[0027] In one embodiment, in step H1, the first charging current is 0.01C to 0.02C; in step H3, the second charging current is 0.02C to 0.03C; in step H5, the third charging current is 0.03C to 0.05C; in step H7, the fourth charging current is 0.1C to 0.15C; in step H9, the fifth charging current is 0.33C to 0.5C.
[0028] Specifically, the preferred combination of the first charging current to the fifth charging current is: the first charging current is 0.01C, the second charging current is 0.02C, the third charging current is 0.05C, the fourth charging current is 0.10C, and the fifth charging current is 0.33C.
[0029] In one embodiment, in step H1, the first SOC is 1.0% to 2.0%; in step H3, the second SOC is 2.0% to 3.0%; in step H5, the third SOC is 3.0% to 5.0%; in step H7, the fourth SOC is 20.0% to 30.0%; in step H9, the fifth SOC is 15.0% to 20.0%.
[0030] Specifically, a very small current is used in the initial stage of formation, followed by step-by-step charging. Each stage is combined with lower SOC control. This not only can obtain a high-quality SEI film, but also can greatly shorten the formation time and reduce production costs. At the same time, it can also be used for various types of sodium-ion batteries, and has the advantages of strong versatility and good formation effect.
[0031] In one embodiment, the first SOC is 1%, the second SOC is 2%, the third SOC is 5%, the fourth SOC is 20%, and the fifth SOC is 15%.
[0032] Specifically, the preferred combination of the first SOC to the fifth SOC is: the first SOC is 1%, the second SOC is 2%, the third SOC is 5%, the fourth SOC is 20%, and the fifth SOC is 15%.
[0033] In one embodiment, in step H2, the first preset time length is 2 to 5 minutes; in step H4, the second preset time length is 1 to 5 minutes; in step H6, the third preset time length is 1 to 5 minutes; in step H8, the fourth preset time length is 1 to 5 minutes.
[0034] Specifically, by briefly letting the sodium-ion battery rest after each charging stage, the stability of the sodium-ion battery performance can be ensured, thereby improving the consistency of the sodium-ion battery performance.
[0035] The preferred combination of the first preset time length to the fifth preset time length is: the first preset time length is 2 minutes, the second preset time length is 1 minute, the third preset time length is 1 minute, and the fourth preset time length is 1 minute.
[0036] A second aspect of the present invention provides a sodium ion battery prepared by the above-mentioned sodium ion battery formation method.
[0037] The beneficial effects of the present invention are as follows:
[0038] The present invention is reasonably designed. When forming a sodium ion battery, a step-by-step charging method is adopted for formation, which mainly has the following gain effects:
[0039] 1. It reduces the total charging time of formation and reduces the overall charging depth of the battery (the battery state of charge SOC is the charging depth), reduces the gas production during the battery formation process, and increases the uniform contact area between the internal diaphragm and the negative electrode of the battery, thereby enhancing the conductivity of sodium ions.
[0040] 2. In the first, second and third formation charging stages, the charging time of small current is shortened, the thickness of the inorganic layer formed on the negative electrode interface is reduced, the rate of exchange between sodium ions and electrons is increased, and the sodium ion transmission capacity of the SEI interface film is enhanced.
[0041] 3. In the fourth and fifth formation charging stages, by increasing the high rate charging, a porous organic layer is formed, in which the electrolyte can be stored, thus promoting the transmission rate of sodium ions.
[0042] 4. In the formation method provided by the present invention, a high-quality SEI film can be formed without subjecting the sodium ion battery to vacuum negative pressure, hot pressing, voltage limitation and other means of formation, so that the battery has a small internal resistance, high energy density, high battery capacity and first efficiency, and low cycle inflation rate, thereby improving the battery cycle performance and high-temperature storage performance.
[0043] 5. The formation method provided by the present invention has a short formation time, greatly reduces the production cost, can be used for various types of sodium ion batteries, and has the advantages of strong versatility and good formation effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 The present invention is a schematic flow diagram of a sodium ion battery formation method.
[0045] Figure 2 This is a diagram of the negative electrode plate interface of a sodium ion battery after being fully charged and disassembled after being formed using the sodium ion battery formation method provided in Example 1 of the present invention.
[0046] Figure 3 This is a voltage-current-time diagram of a sodium ion battery after formation using the sodium ion battery formation method provided in Example 1 of the present invention.
[0047] Figure 4 This is a graph showing the change in internal resistance of a sodium ion battery after being formed using the sodium ion battery formation method provided in Example 1 of the present invention.
[0048] Figure 5 It is a high and low temperature performance curve of a sodium ion battery formed by the sodium ion battery formation method provided in Example 1 of the present invention.
[0049] Figure 6 It is a cycle performance curve diagram of a sodium ion battery formed by the sodium ion battery formation method provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0050] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0051] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0052] Example 1
[0053] like Figure 1 As shown, this embodiment provides a formation method of a sodium ion battery, comprising the following steps:
[0054] The first step is to select a sodium ion battery with good appearance, completed liquid injection, and left standing at room temperature or high temperature without being formed;
[0055] The second step is to charge the sodium ion battery with a current of 0.01C (current 0.13A). During the charging process, the SOC value is monitored by controlling the charging time. When the SOC value reaches 1% (capacity 0.13Ah), that is, charging for 60 minutes, the charging is stopped.
[0056] Step 3: Let stand for 2 minutes;
[0057] Step 4: After standing for 2 minutes, the sodium ion battery is charged at a current of 0.02C (current 0.26A). The SOC value is monitored by controlling the charging time during the charging process. When the SOC value reaches 2% (capacity 0.26Ah), that is, charging for 60 minutes, the charging is stopped.
[0058] Step 5: Let stand for 1 minute;
[0059] Step 6. After standing for 1 minute, continue to charge the sodium ion battery at a current of 0.05C (current 0.65A). During the charging process, the SOC value is monitored by controlling the charging time. When the SOC value reaches 5% (capacity 0.65Ah), that is, charging for 60 minutes, stop charging.
[0060] Step 7: Let stand for 1 minute;
[0061] Step 8. After standing for 1 minute, the sodium ion battery is charged at a current of 0.1C (current 1.3A). The SOC value is monitored by controlling the charging time during the charging process. When the SOC value reaches 20% (capacity 2.6Ah), that is, charging for 120 minutes, the charging is stopped.
[0062] Step 9: Let stand for 1 minute;
[0063] Step 10. After standing for 1 minute, the sodium ion battery is charged at a current of 0.33C (current 4.29A). The SOC value is monitored by controlling the charging time during the charging process. When the SOC value reaches 15% (capacity 1.56Ah), that is, charging for 22 minutes, the charging is stopped.
[0064] Step 9: Complete the formation of the sodium ion battery.
[0065] After the formation of the sodium ion battery is completed, it is disassembled after full charge and capacity division and the interface of the negative electrode is observed. In addition, the internal resistance change, high and low temperature performance and cycle performance of the subsequent process are tested. The interface of the negative electrode is shown in 2, and the voltage, current and time are shown in Figure 3 As shown, high and low temperature performance Figure 5 As shown, the cycle performance is Figure 6 shown.
[0066] Compared with the currently commonly used formation full charge method (charging to 100%), the total formation time of Example 1 of the present invention is greatly reduced compared with the formation full charge method, and the sodium ion battery formed by the sodium ion battery formation method implemented by the present invention has a good interface, a small change in internal resistance, and the high and low temperature performance and the cycle performance are not affected, that is, the sodium ion battery has good stability.
[0067] By adopting the sodium ion battery formation method disclosed in the embodiment of the present invention to carry out formation, the formation time can be effectively shortened, the production cost can be reduced, and it can be adopted for various types of sodium ion batteries, has strong versatility, and the sodium ion battery has stable performance and good formation effect.
[0068] Example 2
[0069] like Figure 1 As shown, this embodiment provides a formation method of a sodium ion battery, comprising the following steps:
[0070] The first step is to select a sodium ion battery with good appearance, completed liquid injection, and left standing at room temperature or high temperature without being formed;
[0071] The second step is to charge the sodium ion battery with a current of 0.02C. During the charging process, the SOC value is monitored by controlling the charging time. When the SOC value reaches 2%, that is, charging for 60 minutes, the charging is stopped.
[0072] Step 3: Let stand for 5 minutes;
[0073] Step 4: After standing for 5 minutes, continue to charge the sodium ion battery at a current of 0.03. During the charging process, the SOC value is monitored by controlling the charging time. When the SOC value reaches 3%, that is, charging for 60 minutes, stop charging.
[0074] Step 5: Let stand for 5 minutes;
[0075] Step 6. After standing for 5 minutes, continue to charge the sodium ion battery at a current of 0.05C. During the charging process, the SOC value is monitored by controlling the charging time. When the SOC value reaches 5%, that is, charging for 60 minutes, stop charging.
[0076] Step 7: Let stand for 5 minutes;
[0077] Step 8. After standing for 5 minutes, the sodium ion battery is charged at a current of 0.15C. The SOC value is monitored by controlling the charging time during the charging process. When the SOC value reaches 30%, that is, charging for 120 minutes, the charging is stopped.
[0078] Step 9: Let stand for 5 minutes;
[0079] Step 10: After standing for 5 minutes, the sodium ion battery is charged at a current of 0.5C. The SOC value is monitored by controlling the charging time during the charging process. When the SOC value reaches 20%, that is, charging for 22 minutes, the charging is stopped.
[0080] Step 9: Complete the formation of the sodium ion battery.
[0081] Specifically, after the formation of the sodium ion battery is completed, it is disassembled after full charge and capacity division and the interface of the negative electrode is observed. In addition, the internal resistance change, high and low temperature performance and cycle performance of the subsequent process are tested. Among them, the interface of the negative electrode, voltage and current time, high and low temperature performance, and cycle performance are similar to those of Example 1, and will not be repeated here.
[0082] Compared with the currently commonly used formation full charge method (charging to 100%), the total formation time of Example 2 of the present invention is greatly reduced compared with the formation full charge method, and the sodium ion battery formed by the sodium ion battery formation method implemented by the present invention has a good interface, a small change in internal resistance, and high and low temperature performance and cycle performance are not affected, that is, the sodium ion battery has good stability.
[0083] Example 3
[0084] like Figure 1 As shown, this embodiment provides a formation method of a sodium ion battery, comprising the following steps:
[0085] The first step is to select a sodium ion battery with good appearance, completed liquid injection, and left standing at room temperature or high temperature without being formed;
[0086] The second step is to charge the sodium ion battery with a current of 0.015C. During the charging process, the SOC value is monitored by controlling the charging time. When the SOC value reaches 1.5%, that is, charging for 60 minutes, the charging is stopped.
[0087] Step 3: Let stand for 3 minutes;
[0088] Step 4: After standing for 3 minutes, continue to charge the sodium ion battery at a current of 0.025. During the charging process, the SOC value is monitored by controlling the charging time. When the SOC value reaches 2.5%, that is, charging for 60 minutes, stop charging.
[0089] Step 5: Let stand for 3 minutes;
[0090] Step 6. After standing for 3 minutes, continue to charge the sodium ion battery at a current of 0.04C. During the charging process, the SOC value is monitored by controlling the charging time. When the SOC value reaches 4%, that is, charging for 60 minutes, stop charging.
[0091] Step 7: Let stand for 2 minutes;
[0092] Step 8. After standing for 2 minutes, the sodium ion battery is charged at a current of 0.12C. The SOC value is monitored by controlling the charging time during the charging process. When the SOC value reaches 25%, that is, charging for 120 minutes, the charging is stopped.
[0093] Step 9: Let stand for 3 minutes;
[0094] Step 10: After standing for 3 minutes, the sodium ion battery is charged at a current of 0.42C. The SOC value is monitored by controlling the charging time during the charging process. When the SOC value reaches 18%, that is, charging for 22 minutes, the charging is stopped.
[0095] Step 9: Complete the formation of the sodium ion battery.
[0096] Specifically, after the formation of the sodium ion battery is completed, it is disassembled after full charge and capacity division and the interface of the negative electrode is observed. In addition, the internal resistance change, high and low temperature performance and cycle performance of the subsequent process are tested. Among them, the interface of the negative electrode, voltage and current time, high and low temperature performance, and cycle performance are similar to those of Example 1, and will not be repeated here.
[0097] Compared with the currently commonly used formation full charge method (charging to 100%), the total formation time of Example 3 of the present invention is greatly reduced compared with the formation full charge method, and the sodium ion battery formed by the sodium ion battery formation method implemented by the present invention has a good interface, a small change in internal resistance, and the high and low temperature performance and the cycle performance are not affected, that is, the sodium ion battery has good stability.
Claims
1. A sodium ion battery formation method, characterized in that: After the sodium ion battery is filled and left to stand at room temperature and at high temperature for a set time, the battery is charged five times in a step-by-step manner at the formation pressure and formation temperature. The five-step charging includes the following steps: Step H1, charging the sodium ion battery with a constant current continuously according to a first charging condition to reach a first formation stage; the first charging condition is to reach a first charging current, the first charging current is 0.01C to 0.02C, and the first formation stage is when the SOC value of the sodium ion battery reaches a first SOC; Step H2, standing for a first preset time, the first preset time being 2 to 5 minutes; Step H3, after the sodium ion battery is left to stand for a first preset time, the sodium ion battery is continuously charged with a constant current according to a second charging condition to reach a second formation stage; the second charging condition is to reach a second charging current, and the second charging current is 0.02C to 0.03C; the second formation stage is when the SOC value of the sodium ion battery reaches a second SOC; Step H4, standing for a second preset time, the second preset time being 1 to 5 minutes; Step H5, after standing for a second preset time, continuously charging the sodium ion battery with a constant current according to a third charging condition to reach a third formation stage; the third charging condition is to reach a third charging current, and the third charging current is 0.03C to 0.05C; The third formation stage is when the SOC value of the sodium ion battery reaches the third SOC; Step H6: let stand for a third preset time, the third preset time being 1 to 5 minutes; Step H7, after standing for a third preset time, the sodium ion battery is continuously charged at a constant current according to a fourth charging condition to reach a fourth formation stage; the fourth charging condition is to reach a fourth charging current, and the fourth charging current is 0.1C to 0.15C; the fourth formation stage is when the SOC value of the sodium ion battery reaches a fourth SOC; Step H8, leaving the mixture to stand for a fourth preset time period, the fourth preset time period being 1 to 5 minutes; Step H9, after standing for a fourth preset time period, continuously charging the sodium ion battery with a constant current according to a fifth charging condition to reach a fifth formation stage; the fifth charging condition is to reach a fifth charging current, and the fifth charging current is 0.33C to 0.5C; the fifth formation stage is when the SOC value of the sodium ion battery reaches a fifth SOC; After the fifth preset time, the transformation is completed.
2. A sodium ion battery formation method according to claim 1, characterized in that: The room temperature static temperature is 25±5℃, and the room temperature static time is 6 to 8h.
3. A sodium ion battery formation method according to claim 1, characterized in that: The high temperature standing temperature is 45±5℃, and the high temperature standing time is 8 to 16 hours.
4. A sodium ion battery formation method according to claim 1, characterized in that: The forming pressure is 300-600kgf.
5. A sodium ion battery formation method according to claim 1, characterized in that: The formation temperature is 30-45°C.
6. A sodium ion battery formation method according to claim 1, characterized in that: In step H1, the first SOC is 1.0% to 2.0%; In step H3, the second SOC is 2.0% to 3.0%; In step H5, the third SOC is 3.0% to 5.0%; In step H7, the fourth SOC is 20.0% to 30.0%; In step H9, the fifth SOC is 15.0% to 20.0%.
7. A sodium ion battery formation method according to claim 6, characterized in that: The first SOC is 1%, the second SOC is 2%, the third SOC is 5%, the fourth SOC is 20%, and the fifth SOC is 15%.
8. A sodium ion battery, characterized in that: The battery is prepared by a sodium ion battery formation method as claimed in any one of claims 1 to 7.