Batteries and electrical devices
By introducing positive electrode active materials containing Al and ceramic coatings into lithium-ion batteries, the battery design was optimized, resolving the contradiction between battery energy density and thermal stability in EVTOLs. This achieved a balance between high energy density and high thermal box failure temperature, meeting the usage requirements of EVTOLs.
Patent Information
- Application Number
- CN202410038452.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-10
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-01-10
AI Technical Summary
Existing lithium-ion batteries cannot simultaneously meet the requirements of high energy density and high heatbox failure temperature in electric vertical takeoff and landing (EVTOL) aircraft, affecting range and safety performance.
By introducing an Al-containing positive electrode active material into the positive electrode sheet and coating a ceramic coating on the separator, the relationship 0.3≤1000*(9a+t)/c^2≤0.58 is satisfied, so as to regulate the coordinated effect of Al content, ceramic coating thickness and positive electrode film layer density and optimize battery design.
While ensuring battery energy density, it significantly increases the battery's thermal failure temperature, improves battery safety performance, meets EVTOL's usage requirements, and saves R&D time and costs.
Smart Images

Figure BDA0004658961140000121 
Figure BDA0004658961140000131
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and more specifically, to a battery and an electrical device. Background Technology
[0002] Electric vertical takeoff and landing (EVTOL) aircraft have attracted widespread attention due to their advantages such as low energy consumption, zero pollution, low noise, and high comfort. They can be applied to various scenarios including regional passenger transport, freight transport, and emergency medical services, and have broad market prospects. Currently, batteries such as lithium-ion batteries are the best choice for powering EVTOLs.
[0003] One of the main challenges facing EVTOL is battery technology. During flight, aircraft have extremely high requirements for battery energy density and safety performance. Battery energy density determines the flight range, while safety performance determines the probability of an accident. Among these, hot box testing is an important means of evaluating battery thermal stability, and the hot box failure temperature is a crucial indicator of battery safety performance.
[0004] Therefore, improving the battery thermal failure temperature while maintaining battery energy density is an important condition for promoting the large-scale application of lithium-ion batteries in EVTOL. Summary of the Invention
[0005] In view of this, the present invention aims to at least partially solve one of the technical problems in the related art. To this end, the present invention provides a battery and an electrical device that, while ensuring battery energy density, can also increase the battery thermal failure temperature, thus meeting the requirements of electrical devices such as EVTOL.
[0006] To solve the above-mentioned technical problems, this application is implemented as follows:
[0007] According to one aspect of this application, an embodiment of this application provides a battery, which includes a positive electrode, a negative electrode, an electrolyte, and a separator disposed between the positive electrode and the negative electrode.
[0008] The positive electrode sheet includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector, the positive electrode film layer including a positive electrode active material, the positive electrode active material containing Al element;
[0009] The separator includes a separator substrate and a coating disposed on at least one surface of the separator substrate, the coating including a ceramic coating;
[0010] The battery satisfies: 0.3≤1000*(9a+t) / c^2≤0.58;
[0011] Where a is the mass percentage of Al element in the positive electrode active material, in %;
[0012] t represents the thickness of the ceramic coating, in μm;
[0013] c is the areal density of the positive electrode film, in g / m³. 2 .
[0014] In addition, the battery according to this application may also have the following additional technical features:
[0015] In some of these embodiments, the battery satisfies: 0.32 ≤ 1000*(9a+t) / c^2 ≤ 0.55;
[0016] Optionally, the battery satisfies: 0.34≤1000*(9a+t) / c^2≤0.52.
[0017] In some embodiments, the mass percentage 'a' of Al element in the positive electrode active material is 0.2% to 0.6%; optionally, the mass percentage 'a' of Al element in the positive electrode active material is 0.3% to 0.5%.
[0018] In some embodiments, the thickness t of the ceramic coating is 4 μm to 8 μm; optionally, the thickness t of the ceramic coating is 5 μm to 7 μm.
[0019] In some embodiments, the areal density c of the positive electrode film is 115 g / m². 2 ~190g / m 2 Optionally, the areal density c of the positive electrode film is 150 g / m². 2 ~190g / m 2 .
[0020] In some embodiments, the positive electrode active material comprises a lithium-containing transition metal oxide, the general chemical formula of which is:
[0021] Li d Ni x Co y Mn z Al f M n O2;
[0022] Wherein, 1.0≤d≤1.2, 0.8≤x<1, 0.01≤y≤0.15, 0.01≤z≤0.15, 0.001≤f≤0.10, 0≤n≤0.05, x+y+z+f+n=1;
[0023] The M includes at least one of Ti, Cr, B, K, Mg, Zn, Sn, Si, P, Mo, Zr, Fe, V, Ba, Sr, Nb, W, or Cu; optionally, the M includes at least one of Ti, Mg, Zn, Nb, Zr, or Sr.
[0024] Optionally, f satisfies: 0.007≤f≤0.022.
[0025] In some embodiments, the ceramic particles in the ceramic coating include at least one of alumina, silicon oxide, titanium oxide, zirconium oxide, barium titanate, yttrium-doped zirconium oxide, gadolinium-doped cerium oxide, lithium aluminate, lithium lanthanum titanate, lithium aluminum titanium phosphate, lithium lanthanum zirconate, or lithium lanthanum zirconate tantalate.
[0026] Optionally, the membrane substrate includes at least one of polyethylene, polypropylene, poly(p-phenylene terephthalamide), polyethylene terephthalate, polyacrylonitrile, polytetrafluoroethylene, polyamide, or polyimide.
[0027] In some embodiments, the ceramic particles have a particle size of 0.8 μm to 1.2 μm;
[0028] Optionally, the thickness of the diaphragm substrate is 5 μm to 15 μm.
[0029] In some embodiments, the thickness of the positive current collector is 3 μm to 50 μm; optionally, the thickness of the positive current collector is 5 μm to 30 μm.
[0030] Optionally, the mass percentage of the positive electrode active material in the positive electrode film layer is 94% to 98%.
[0031] According to another aspect of this application, embodiments of this application provide an electrical device that includes a battery selected from the foregoing.
[0032] Implementing the technical solution of the present invention has at least the following beneficial effects:
[0033] In this embodiment, the battery uses a positive electrode active material containing Al (aluminum) and a separator with a ceramic coating. Given the potential correlation between the Al content in the positive electrode active material, the thickness of the ceramic coating, and the areal density of the positive electrode film on the battery's energy density and thermal failure temperature, extensive research has led to the development of an important empirical formula related to cell design. Specifically, when the battery satisfies the relationship 0.3 ≤ 1000*(9a+t) / c^2 ≤ 0.58, it can balance the coordinating effects of the Al content in the positive electrode active material, the thickness of the ceramic coating, and the areal density of the positive electrode film. This allows for both ensuring battery energy density and improving the thermal failure temperature (enhancing safety performance), meeting the requirements of electrical devices such as EVTOLs. Furthermore, based on the relationship provided by this invention, using this empirical formula as a guide during cell design can avoid numerous DOE experiments, saving battery development time and costs, and resulting in a battery with both excellent energy density and a high thermal failure temperature.
[0034] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Detailed Implementation
[0035] The present application will be further described below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the present application.
[0036] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges or individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0037] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0038] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0039] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0040] Given the increasingly stringent requirements placed on the energy density and safety performance of existing electrical devices' power systems, such as batteries, there is a need to optimize these aspects. This application provides a battery, also known as a rechargeable battery or accumulator, which is a battery that can be recharged to activate its active materials and continue to be used after discharge. The battery includes a positive electrode and a separator. The positive electrode includes a positive current collector and a positive electrode film layer, and the positive active material in the positive electrode contains Al. The separator includes a ceramic coating.
[0041] This application investigates the relationship between the Al content in the positive electrode active material, the areal density of the positive electrode film, and the thickness of the ceramic coating, optimizing the entire battery system to improve the battery's energy density and thermal stability. This allows the battery to maintain a high thermal failure temperature while achieving excellent energy density, thus optimizing the combination of energy density and thermal stability. Specific technical solutions are described below.
[0042] In some embodiments, this application provides a battery, which includes a positive electrode, a negative electrode, an electrolyte, and a separator disposed between the positive electrode and the negative electrode.
[0043] The positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector. The positive electrode film layer includes a positive electrode active material, and the positive electrode active material contains Al element.
[0044] The separator includes a separator substrate and a coating disposed on at least one surface of the separator substrate, the coating including a ceramic coating;
[0045] The battery satisfies: 0.3≤1000*(9a+t) / c^2≤0.58;
[0046] Where a is the mass percentage of Al element in the positive electrode active material, in %;
[0047] t represents the thickness of the ceramic coating, in μm;
[0048] c is the areal density of the positive electrode film, in g / m². 2 .
[0049] The mass percentage of Al in the above-mentioned positive electrode active material refers to the mass content of Al, which is a, based on the total mass of the positive electrode active material, that is, the mass of Al relative to the total mass of the positive electrode active material.
[0050] This application is able to simultaneously optimize and improve the energy density and thermal stability of the battery for the following reasons:
[0051] The content (doping amount) of Al in the positive electrode active material has a significant impact on the energy density and thermal stability of the battery cell. On the one hand, a higher Al doping amount can improve the structural stability of positive electrode active materials, such as the layered structure of nickel-cobalt-manganese. In other words, Al can stabilize the positive electrode structure and suppress the decomposition of the layered structure at high temperatures, which leads to excessive heat generation. Furthermore, Al doping can also suppress the surface stability of the positive electrode material, inhibiting the reaction and heat generation between the positive electrode material and the electrolyte at high temperatures. Therefore, a higher Al doping amount can significantly improve the stability of the positive electrode at high temperatures, reduce heat generation, and thus increase the cell's thermal failure temperature. Increasing the Al content can improve the battery's thermal stability. On the other hand, Al plays a stabilizing role in the positive electrode material and does not undergo valence state changes during charging and discharging. Therefore, doped Al does not contribute to capacity; the specific capacity of the material decreases with increasing Al doping amount. Thus, excessive Al doping will correspondingly lead to a decrease in the cell's energy density. Therefore, it is necessary to keep the Al content in the positive electrode active material within a certain range to better improve the cell's thermal failure temperature, i.e., improve the battery's thermal stability, while ensuring the battery's energy density.
[0052] The areal density of the positive electrode film layer in the positive electrode sheet has a significant impact on the energy density and thermal stability of the battery cell. On the one hand, increasing the areal density of the positive electrode film layer can reduce the proportion of the positive electrode current collector, such as foil, in the battery cell, thereby increasing the proportion of the positive electrode active material and improving the energy density. In other words, increasing the areal density of the positive electrode film layer helps to improve the energy density of the battery. On the other hand, the positive electrode current collector, such as foil, is more stable than the positive electrode active material at high temperatures. It can also play a good role in heat dissipation during high-temperature processes, which can suppress the heat spread and thermal runaway caused by local overheating. Therefore, the lower the areal density of the positive electrode film layer, the higher the thermal stability of the battery cell and the higher the thermal box failure temperature. In other words, reducing the areal density of the positive electrode film layer helps to increase the thermal box failure temperature and improve the thermal stability of the battery. Therefore, it is necessary to control the areal density of the positive electrode film layer within a suitable range, so as to ensure the battery energy density while preventing the battery thermal box failure temperature from becoming too low. That is, it is possible to improve the thermal box failure temperature of the battery cell and improve the thermal stability of the battery while ensuring the battery energy density.
[0053] The separator substrate in a battery separator is typically made of polymer materials. Due to the poor thermal stability of polymer-based membranes, they shrink or soften and deform above 130°C. Damage to the separator can lead to direct contact between the positive and negative electrodes, causing a short circuit and generating significant heat, potentially resulting in thermal runaway. Therefore, a coating, including a ceramic coating, is usually applied to the surface of the polymer separator substrate. Materials used in ceramic coatings typically possess high thermal stability, not decomposing or deforming below 200°C, thus significantly enhancing the mechanical strength of the separator at high temperatures. Therefore, a thicker ceramic coating can increase the cell failure temperature, meaning that increasing the ceramic coating thickness improves the battery's thermal stability. However, on the other hand, reducing the separator thickness is currently one direction for improving cell energy density. An excessively thick coating can reduce the space in the cell thickness direction, decreasing the proportion of active material and resulting in excessively low energy density. Therefore, reducing the ceramic coating thickness helps to improve the battery's energy density. Therefore, it is necessary to control the ceramic thickness of the separator within a suitable range so as to ensure the battery energy density while preventing the battery thermal box failure temperature from being too low. In other words, it is possible to improve the cell thermal box failure temperature and enhance the battery thermal stability while ensuring the battery energy density.
[0054] Therefore, for batteries, the content of Al in the positive electrode active material, the areal density of the positive electrode film, and the thickness of the ceramic coating all have a significant impact on the battery's energy density and thermal failure temperature (thermal stability), and there is a certain contradiction between improving energy density and thermal safety. Based on this, the inventors of this application unexpectedly discovered after extensive research that, although the content of Al in the positive electrode active material, the areal density of the positive electrode film, and the thickness of the ceramic coating do affect the battery's energy density and thermal failure temperature, their influence has certain limitations and correlations. Only when the formula 0.3≤1000*(9a+t) / c^2≤0.58 is satisfied can the battery cell achieve both high energy density and high thermal failure temperature, thus obtaining a battery that combines high energy density and improved thermal stability.
[0055] Therefore, this application satisfies the above conditions by controlling the relationship between the Al content in the positive electrode active material, the areal density of the positive electrode film, and the thickness of the ceramic coating, namely, 0.3 ≤ 1000*(9a+t) / c^2 ≤ 0.58. This comprehensively controls high energy density and good thermal box failure temperature, thereby ensuring battery energy density while improving battery thermal box failure temperature (improving safety performance), meeting the requirements of electrical devices such as EVTOLs. Furthermore, based on the relationship provided by this invention, using the above empirical formula as a guide during cell design can avoid numerous DOE experiments, saving battery development time and costs, and enabling the designed battery to possess both excellent energy density and a high thermal box failure temperature.
[0056] When the value of 1000*(9a+t) / c^2 is too low, such as less than 0.3, it will reduce the thermal box failure temperature. For example, poor stability of the positive electrode active material will lead to a low thermal box failure temperature; or the proportion of positive electrode current collector such as foil is too high, which reduces the thermal stability and heat dissipation capacity of the positive electrode sheet, resulting in a lower thermal box failure temperature; or the thickness of the ceramic coating is too thin, the coating has low mechanical strength at high temperature, and shrinkage and damage will cause short circuit between the positive and negative electrodes, generating heat, which will result in a low thermal box failure temperature.
[0057] When the value of 1000*(9a+t) / c^2 is too high, such as greater than 0.58, it will reduce the energy density of the battery. For example, it will affect the specific capacity of the material, resulting in a decrease in the energy density of the battery; or the proportion of the positive electrode current collector, such as foil, is too high, resulting in a decrease in the energy density of the battery; or the thickness of the ceramic coating is too thick, occupying too much space in the thickness direction, resulting in a decrease in the energy density of the cell.
[0058] The aforementioned batteries can be, for example, lithium-ion batteries, sodium-ion batteries, magnesium-ion batteries, potassium-ion batteries, etc., but are not limited to these. In this invention, the batteries can be manufactured into batteries with different structures as needed, without any particular limitation. As examples, the battery structures of this application include, but are not limited to, pouch batteries, square hard-shell batteries, or cylindrical hard-shell batteries. That is, the battery can be cylindrical, flat, cuboid, or other shapes.
[0059] It should be noted that, in the specific implementation, lithium-ion batteries are used as an example to explain this application, but the batteries in this application are not limited to lithium-ion batteries.
[0060] Through in-depth research, the inventors have discovered that, in addition to meeting the above-mentioned design conditions, the battery of this application can further improve its energy density, thermal safety, etc., if it can also optionally meet one or more of the following conditions.
[0061] In some embodiments, the battery satisfies: 0.32≤1000*(9a+t) / c^2≤0.55;
[0062] In some embodiments, the battery satisfies: 0.34≤1000*(9a+t) / c^2≤0.52.
[0063] As an example, the value of 1000*(9a+t) / c^2 can be any point value within the range of 0.3, 0.32, 0.34, 0.35, 0.36, 0.38, 0.4, 0.42, 0.43, 0.44, 0.45, 0.46, 0.48, 0.5, 0.51, 0.52, 0.54, 0.55, 0.56, 0.58, or any combination of two values.
[0064] By ensuring that the battery meets the above conditions, its thermal stability can be further improved, which in turn improves its safety performance, while maintaining a high energy density.
[0065] In some embodiments, the mass percentage 'a' of Al element in the positive electrode active material is 0.2% to 0.6%; in some embodiments, the mass percentage 'a' of Al element in the positive electrode active material is 0.3% to 0.5%. As an example, 'a' can be any value within the range of 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, or any combination thereof.
[0066] According to an embodiment of the present invention, the positive electrode active material may be doped with Al element, that is, the mass percentage of Al element in the above positive electrode active material is the doping amount of Al element.
[0067] When the Al doping amount in the positive electrode active material is too low, it will affect the overall structural stability or surface stability of the positive electrode active material, and will not effectively suppress the reaction and heat generation between the positive electrode material and the electrolyte at high temperatures, thus reducing the stability of the positive electrode at high temperatures and failing to effectively reduce heat generation, thereby leading to a decrease in the cell's thermal box failure temperature. When the Al doping amount in the positive electrode active material is too high, it will affect the specific capacity of the positive electrode active material, leading to a decrease in the energy density of the cell. Therefore, in this embodiment of the invention, the mass percentage 'a' of Al in the positive electrode active material is preferably 0.2% to 0.6%. When the Al doping amount meets the above-mentioned value range, it can effectively ensure the battery's energy density and high thermal box failure temperature.
[0068] In this embodiment, the method for testing the mass percentage of Al element in the positive electrode active material, i.e., the Al element doping amount, can be as follows:
[0069] (1) Weigh 0.1-0.3g of positive electrode active material and add 10ml of hydrochloric acid solution (hydrochloric acid to water volume ratio is 1:1).
[0070] (2) Digest at 230°C for 30 minutes on a heating plate.
[0071] (3) The solution after decomposition (Al element dissolved in the solution) was tested using ICP (inductively coupled plasma atomic emission spectrometer).
[0072] In some embodiments, the areal density c of the positive electrode film is 115 g / m². 2 ~190g / m 2 In some embodiments, the areal density c of the positive electrode film is 150 g / m². 2 ~190g / m 2 As an example, c can be 115g / m³. 2 120g / m2 125g / m 2 130g / m 2 135g / m 2 140g / m 2 150g / m 2 155g / m 2 160g / m 2 165g / m 2 170g / m 2 175g / m 2 180g / m 2 190g / m 2 , or any point value within the range of pairwise combinations.
[0073] When the areal density of the positive electrode film layer is too low, it increases the proportion of the positive current collector, such as foil, in the battery cell, reducing the proportion of the positive active material and thus lowering the energy density. When the areal density of the positive electrode film layer is too high, it results in a low proportion of the positive current collector, such as foil, which cannot effectively perform its heat dissipation function during high-temperature processes and cannot effectively suppress heat propagation and thermal runaway caused by local overheating. Consequently, the thermal stability of the battery cell decreases, the failure temperature of the thermal chamber is lower, and thermal safety is reduced. Therefore, in this embodiment of the invention, the areal density c of the positive electrode film layer is preferably 115 g / m³. 2 ~190g / m 2 When the surface density of the positive electrode film is within the range specified above, it can effectively guarantee the battery energy density and high thermal box failure temperature.
[0074] In some embodiments, the thickness t of the ceramic coating is 4 μm to 8 μm; in other embodiments, the thickness t of the ceramic coating is 5 μm to 7 μm. As an example, t can be any value within the range of 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, or any combination thereof.
[0075] When the ceramic coating thickness is too low, it reduces the coating's mechanical strength at high temperatures, causing shrinkage and breakage that leads to short-circuit heat generation between the positive and negative electrodes, resulting in a lower thermal box failure temperature and reduced thermal safety. When the ceramic coating thickness is too high, it encroaches on the cell's thickness space, reducing the proportion of active material and thus lowering the energy density. Therefore, in this embodiment of the invention, the ceramic coating thickness t is preferably 4μm to 8μm. When the ceramic coating thickness meets the above-mentioned range, it can effectively ensure the battery's energy density and high thermal box failure temperature.
[0076] In this embodiment, the positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one side or at least one surface of the positive current collector. The phrase "positive electrode film layer disposed on at least one side or at least one surface of the positive current collector" means that the positive electrode film layer can be disposed on one surface of the positive current collector along its thickness direction, or on two surfaces of the positive current collector along its thickness direction. Here, "surface" can refer to the entire area of the positive current collector or only a portion of it; this application does not impose any particular limitation, as long as the purpose of this application is achieved.
[0077] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on the two opposite surfaces of the positive current collector. It can be understood that the positive electrode film layer can also be stacked on either of the two surfaces of the positive current collector.
[0078] In some embodiments, the positive current collector may be a metal foil or a composite current collector.
[0079] This application does not impose any particular limitation on the positive electrode current collector; any positive electrode current collector well-known to those skilled in the art can be used, as long as it achieves the purpose of this application. As an example, the metal foil can be aluminum foil, aluminum alloy foil, carbon-coated aluminum foil, or nickel mesh, etc. The composite current collector may include a polymer material base layer (such as polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.) and a metal material layer formed on at least one surface of the polymer material base layer; the metal material layer may include at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. In this embodiment, the positive electrode current collector is preferably aluminum foil, carbon-coated aluminum foil, or nickel mesh.
[0080] In some embodiments, the thickness of the positive electrode current collector is 3 μm to 50 μm, preferably 5 μm to 30 μm, more preferably 5 μm to 20 μm, and most preferably 8 μm to 11 μm.
[0081] The positive electrode active material in the positive electrode film layer of this application may include any material known in the art. For example, the positive electrode active material may be selected from lithium-ion nickel-cobalt-manganese oxides, such as ternary cathode materials doped with Al, but is not limited to these. Other lithium-containing transition metal oxides doped with aluminum may also be used.
[0082] Optionally, the positive electrode active material can be a high-nickel positive electrode active material doped with aluminum. For example, the positive electrode active material can be a high-nickel ternary material doped with aluminum.
[0083] In some embodiments, the positive electrode active material comprises a lithium-containing transition metal oxide, the general chemical formula of which is:
[0084] Lid Ni x Co y Mn z Al f M n O2;
[0085] Wherein, 1.0≤d≤1.2, 0.8≤x<1, 0.01≤y≤0.15, 0.01≤z≤0.15, 0.001≤f≤0.10, 0≤n≤0.05, x+y+z+f+n=1;
[0086] M includes at least one of Ti, Cr, B, K, Mg, Zn, Sn, Si, P, Mo, Zr, Fe, V, Ba, Sr, Nb, W, or Cu;
[0087] Preferably, M includes at least one of Ti, Mg, Zn, Nb, Zr or Sr.
[0088] Preferably, in some embodiments, f satisfies: 0.007 ≤ f ≤ 0.022. By optimizing the range of values for f, the content of Al element can be optimized, that is, the mass percentage content 'a' of Al element in the positive electrode active material can be kept within the required range.
[0089] In the above general chemical formula, the subscript f of Al element is related to the mass percentage a of Al element in the positive electrode active material:
[0090] a = 26.98f / (6.94d + 58.69x + 58.93y + 54.98z + 26.98f + M*n + 32) * 100; where M is the relative atomic mass of element M.
[0091] However, this application is not limited to these materials. Other traditional materials that can be used as positive electrode active materials for batteries can also be used, as long as they contain aluminum, without limiting the purpose of this application. These positive electrode active materials can be used alone or in combination of two or more.
[0092] In some embodiments, the mass of the positive electrode active material is 94% to 98% of the mass of the positive electrode film layer, that is, the mass percentage of the positive electrode active material in the positive electrode film layer is 94% to 98%, and may further be 95% to 98%.
[0093] In some embodiments, the positive electrode film layer further includes a binder and optionally a conductive agent, the binder improving the bonding between the positive electrode active material particles and also improving the bonding between the positive electrode active material and the positive electrode current collector.
[0094] The conductive agent in the aforementioned positive electrode film layer can be any conductive agent well known to those skilled in the art, and there are no special limitations. As an example, the conductive agent includes one or more of conductive graphite, conductive carbon black, conductive carbon fiber, carbon nanotubes, or graphene.
[0095] In some embodiments, the mass of the conductive agent is 0.5% to 2% of the mass of the positive electrode film, that is, the mass percentage of the conductive agent in the positive electrode film is 0.5% to 2%, and may further be 1% to 1.8%.
[0096] The binder in the aforementioned positive electrode film layer can be any binder well known to those skilled in the art, and there are no special limitations. As an example, the binder may be one or more of the following: chitosan, xanthan gum, gellan gum, gum arabic, polyacrylonitrile, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, polymethacrylamide, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, polyacrylamide, styrene-butadiene rubber, sodium alginate, polyethylene glycol, guar gum, guar gum polymers, or guar gum copolymers.
[0097] In some embodiments, the mass of the binder is 0.8% to 2% of the mass of the positive electrode film layer, that is, the mass percentage of the binder in the positive electrode film layer is 0.8% to 2%, and may further be 1.2% to 1.8%.
[0098] The positive electrode sheet can be prepared by methods known in the art. For example, the positive electrode sheet can be obtained by mixing a positive electrode active material, a conductive agent, and a binder in a solvent to prepare an active material composition, and then coating the active material composition onto a positive electrode current collector. In some embodiments, the solvent may include, but is not limited to, N-methylpyrrolidone, etc.
[0099] In some embodiments, the negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector. The phrase "a negative electrode film layer disposed on at least one surface of the negative current collector" means that the negative electrode film layer can be disposed on one surface of the negative current collector along its thickness direction, or on two surfaces of the negative current collector along its thickness direction. Here, "surface" can refer to the entire area of the negative current collector or only a portion of it; this application does not impose any particular limitation, as long as the purpose of this application is achieved.
[0100] As an example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode film layer is disposed on the two opposite surfaces of the negative electrode current collector. It can be understood that the negative electrode film layer can also be stacked on either of the two surfaces of the negative electrode current collector.
[0101] This application does not impose any particular limitation on the negative electrode current collector; any negative electrode current collector well-known to those skilled in the art can be used, as long as it achieves the purpose of this application. In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. The metal foil includes copper foil, copper alloy foil, nickel foil, titanium foil, etc. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. In this embodiment, the negative electrode current collector is preferably copper foil.
[0102] In some embodiments, the thickness of the negative electrode current collector is 3μm to 50μm, preferably 5μm to 30μm, more preferably 5μm to 20μm, and most preferably 4.5μm to 8μm.
[0103] In some embodiments, the negative electrode film layer includes a negative electrode active material, which may be a negative electrode active material known in the art for use in batteries. This application does not have any particular limitation on the type of negative electrode active material, as long as it can achieve the purpose of this application.
[0104] As an example, the negative electrode active material includes one or more of silicon-based materials, graphite, soft carbon, hard carbon, carbon fiber, and mesophase carbon microspheres.
[0105] However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials in batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0106] Optionally, the areal density of the negative electrode film is 60 g / m². 2 ~120g / m 2 Optionally, the areal density of the negative electrode film is 70 g / m². 2 ~110g / m 2 .
[0107] In some embodiments, the mass of the negative electrode active material is 94% to 98% of the mass of the negative electrode film layer, that is, the mass percentage of the negative electrode active material in the negative electrode film layer is 94% to 98%, and may further be 95% to 97%.
[0108] In some embodiments, the negative electrode film layer further includes at least one of a conductive agent, a thickener, and a binder. This application does not impose any particular limitation on the types of conductive agents, thickeners, and binders in the negative electrode film layer, as long as they achieve the purpose of this application.
[0109] As an example, the conductive agent in the negative electrode film layer may be selected from one or more of conductive graphite, conductive carbon black, conductive carbon fiber, carbon nanotubes, and graphene. The binder in the negative electrode film layer may be selected from one or more of chitosan, xanthan gum, gellan gum, gum arabic, polyacrylonitrile, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, polymethacrylamide, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, polyacrylamide, styrene-butadiene rubber, sodium alginate, polyethylene glycol, guar gum, guar gum polymers, and guar gum copolymers. The thickener may be sodium carboxymethyl cellulose (CMC-Na).
[0110] In some embodiments, the mass of the conductive agent is 0.2% to 10% of the mass of the negative electrode film, that is, the mass percentage of the conductive agent in the negative electrode film is 0.2% to 10%, preferably 0.5% to 8%, more preferably 0.8% to 5%, and most preferably 1% to 3%.
[0111] In some embodiments, the mass of the binder is 0.3% to 10% of the mass of the negative electrode film layer, that is, the mass percentage of the binder in the negative electrode film layer is 0.3% to 10%, preferably 0.5% to 8%, more preferably 1% to 5%, and most preferably 2% to 4%.
[0112] In this invention, there are no special limitations on the material of the separator substrate in the separator membrane; any separator material well known to those skilled in the art can be used. As an example, in some embodiments, the separator substrate includes at least one of polyethylene, polypropylene, poly(p-phenylene terephthalamide), polyethylene terephthalate, polyacrylonitrile, polytetrafluoroethylene, polyamide, or polyimide. In this embodiment, the separator substrate is preferably polyethylene, polypropylene, or a mixture of polyethylene and polypropylene.
[0113] The aforementioned "separator membrane includes a separator substrate and a coating disposed on at least one surface of the separator substrate" means that the coating may be disposed on one surface of the separator substrate along its own thickness direction, or on two surfaces of the separator substrate along its own thickness direction. Here, "surface" may be the entire area of the separator substrate or a part of the separator substrate. This application does not have any particular limitation, as long as the purpose of this application can be achieved.
[0114] As an example, the diaphragm substrate has two surfaces opposite each other in its own thickness direction, and the coating is disposed on the two opposite surfaces of the diaphragm substrate. It is understood that the coating may also be laminated on either of the two surfaces of the diaphragm substrate.
[0115] The coating described above includes a ceramic coating; for example, the coating may consist only of a ceramic coating. Of course, in other embodiments, the coating may also include other types of coatings, such as an adhesive layer, etc., and the present invention does not impose any particular limitations on this.
[0116] In some embodiments, the ceramic particles in the ceramic coating include at least one of alumina, titanium dioxide, zirconium oxide, barium titanate, yttrium-doped zirconium oxide, gadolinium-doped cerium oxide, lithium aluminate, lithium lanthanum titanate, lithium titanium aluminum phosphate, lithium lanthanum zirconate, or lithium zirconium lanthanum tantalate.
[0117] However, this application is not limited to these ceramic materials. Other conventional materials that can be used as the separator coating can also be used, such as silicon oxide, calcium oxide, titanium oxide, magnesium oxide, boron nitride, zinc oxide, chromium oxide, barium oxide, magnesium hydroxide, boehmite, etc., as long as they do not limit the purpose of this application. These ceramic materials can be used alone or in combination of two or more.
[0118] In some embodiments, the particle size of the ceramic particles is 0.8 μm to 1.2 μm. In some embodiments, the particle size of the ceramic particles is 0.9 μm to 1.1 μm.
[0119] In some embodiments, the thickness of the diaphragm substrate is 5 μm to 15 μm. In some embodiments, the thickness of the diaphragm substrate is 6 μm to 13 μm.
[0120] According to the present invention, the electrolyte can be any electrolyte well known to those skilled in the art, and there are no special limitations. As an example, the electrolyte in the present invention includes lithium salt and organic solvent, wherein the types of lithium salt and organic solvent are not specifically limited and can be selected according to actual needs.
[0121] Optionally, the lithium salt preferably includes one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium tetrafluoroborate, lithium dioxalate borate, lithium trifluoromethanesulfonate, lithium difluoroborate oxalate, lithium difluorophosphate, lithium 4,5-dicyano-2-trifluoromethylimidazolium, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.
[0122] Optionally, the organic solvent preferably includes one or more of 1,2-dimethoxypropane, dimethoxymethane, ethylene glycol dimethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl acetate, methyl propionate, ethyl propionate, propyl acetate, and propyl propionate.
[0123] Optionally, the concentration of lithium salt in the electrolyte is preferably 0.1-6 mol / L, more preferably 0.5-4 mol / L, even more preferably 1-3 mol / L, and most preferably 1-2 mol / L; in the embodiments provided by the present invention, the concentration of lithium salt in the electrolyte is specifically 1.2 mol / L.
[0124] In this embodiment of the invention, the battery can be selected as either wound or stacked, and the manufacturing method is not limited.
[0125] This invention achieves excellent energy density and maintains a high thermal box failure temperature by rationally combining the content of Al element in the positive electrode active material, the single-sided areal density of the positive electrode film layer, and the thickness of the ceramic coating, thus enabling the battery cell to meet the EVTOL requirements in terms of performance and safety.
[0126] In some embodiments, this application provides an electrical device that includes a battery selected from those described above.
[0127] Optional, the electrical device is EVTOL.
[0128] It should be understood that the battery provided by this invention can be used in EVTOL, but is not limited thereto. Other electrical devices with the same or similar needs can also use the battery provided by this invention. For example, electrical devices can also be mobile phones, tablets, laptops, e-book players, electric toys, power tools, lighting fixtures, vehicles such as electric vehicles, electric cars, electric bicycles, electric trucks, etc., ships, other aircraft, energy storage systems, and other electrical devices.
[0129] To further illustrate the present invention, the battery of the present invention will be described in detail below with reference to the embodiments. All reagents used in the following embodiments are commercially available.
[0130] Example 1
[0131] 1. Preparation of positive electrode sheet
[0132] Lithium nickel cobalt manganese oxide cathode active materials containing Al element doping, such as LiNi 0.8 Co 0.1 Mn 0.05 Al 0.03 Mg 0.02 O2, a composition of conductive carbon black (SP) and carbon nanotubes, and a binder of polyvinylidene fluoride (PVDF5130) are mixed in a mass ratio of 97:2:1. Then, N-methylpyrrolidone (NMP) is added, and the mixture is stirred and mixed uniformly to form a stable positive electrode slurry with a solid content of 75%. The positive electrode slurry is uniformly coated on a 10μm aluminum foil as a positive electrode current collector, and then dried, cold-pressed, and slit to obtain the positive electrode sheet.
[0133] The mass percentage (a) of Al element in the positive electrode active material is 0.2%.
[0134] The surface density c of the positive electrode film is 150 g / m². 2 .
[0135] 2. Preparation of negative electrode sheet
[0136] The negative electrode active material graphite, conductive agent conductive carbon black (SP), thickener sodium carboxymethyl cellulose (CMC Na), and binder styrene-butadiene rubber (SBR) were mixed in a mass ratio of 96.5:1:1:1.5. Deionized water was added and the mixture was stirred to form a uniform and stable negative electrode slurry with a solid content of 50%. The negative electrode slurry was uniformly coated onto a 6μm copper foil negative electrode current collector. After drying, cold pressing, and slitting, the negative electrode sheet was obtained.
[0137] 3. Preparation of electrolyte
[0138] In a glove box filled with inert gas, ethylene carbonate, methyl ethyl carbonate, and diethyl carbonate were mixed in a mass ratio of 1:1:1. Then, lithium salt LiPF6 was dissolved in an organic solvent with a concentration of 1.2 mol / L to obtain the electrolyte.
[0139] 4. Separating membrane
[0140] A 9μm thick polypropylene membrane was selected as the substrate for the separator, and Al2O3 ceramic was coated on one side to form a ceramic coating.
[0141] The thickness t of the ceramic coating is 6 μm.
[0142] 5. Preparation of lithium-ion batteries
[0143] Arrange and assemble the positive electrode, separator, and negative electrode in sequence, using a winding method.
[0144] Electrolyte was injected into the dry cell and soaked for 24 hours. Then, it was formed at 45°C with a formation rate of 0.05-0.2C and a cutoff voltage of 3.75V. After aging at room temperature for 24 hours, the cell was completed. The cell model is 2614897.
[0145] Examples 2-7
[0146] The lithium-ion batteries in Examples 2-7 were all prepared according to the preparation method of Example 1 above. The only difference was the setting of the mass percentage of Al element a in the positive electrode active material, the single-sided surface density c of the positive electrode film, and the thickness t of the ceramic coating. The specific differences are shown in Table 1.
[0147] Comparative Examples 1-6
[0148] The lithium-ion batteries in Comparative Examples 1-6 were all prepared according to the preparation method of Example 1 above. The only difference was the setting of the mass percentage of Al element a in the positive electrode active material, the single-sided surface density c of the positive electrode film, and the thickness t of the ceramic coating. The specific differences are shown in Table 1.
[0149] Performance testing
[0150] The lithium-ion batteries prepared in Examples 1-7 and Comparative Examples 1-6 were subjected to energy density and thermal chamber safety tests. The energy density was tested at 25°C and 1°C. The thermal chamber test conditions were as follows: the temperature was increased to 130°C at room temperature at a rate of 5°C / min, held for 30 minutes, then the temperature was stopped and observed for 1 hour. The ambient temperature was then increased to 130°C again at a rate of 5°C / min and held for 30 minutes. Then the temperature was increased in a gradient of 5°C and held for 30 minutes, and so on until failure. The failure temperature of each battery was recorded. The higher the temperature, the higher the thermal stability of the cell and the better the safety performance. Generally, a thermal chamber failure temperature higher than 130°C meets the national standard requirements.
[0151] The test results are shown in Table 1 below.
[0152] Table 1. Lithium-ion batteries prepared in Examples 1-7 and Comparative Examples 1-6 and test results.
[0153]
[0154]
[0155] As can be seen from the data in Table 1, the mass percentage of Al element a, the single-sided surface density c of the positive electrode film, and the thickness t of the ceramic coating in the lithium-ion battery positive electrode active material provided in Examples 1-7 of the present invention meet the requirements of 0.3≤1000*(9a+t) / c^2≤0.58, and the energy density and thermal test performance of the battery are excellent.
[0156] However, in Comparative Example 1, the Al doping content in the positive electrode active material was too low, failing to meet the requirement of 0.3≤1000*(9a+t) / c^2≤0.58, resulting in poor material stability and an excessively low thermal box failure temperature. In Comparative Example 2, the Al doping content in the positive electrode active material was too high, failing to meet the requirement of 0.3≤1000*(9a+t) / c^2≤0.58, affecting the specific capacity of the material and resulting in a low energy density. In Comparative Example 3, the single-sided areal density of the positive electrode film was too low, failing to meet the requirement of 0.3≤1000*(9a+t) / c^2≤0.58, and the high proportion of current collector foil led to an excessively low energy density. In Comparative Example 4, the single-sided areal density of the positive electrode film was too high, failing to meet the requirement of 0.3≤1000*(9a+t) / c^2≤0.58, and the low proportion of current collector foil reduced the thermal stability and heat dissipation capacity of the electrode, resulting in an excessively low thermal box failure temperature. In Comparative Example 5, the ceramic coating thickness of the separator is too thin, failing to meet the requirement of 0.3≤1000*(9a+t) / c^2≤0.58. This results in low mechanical strength of the coating at high temperatures, leading to shrinkage and breakage, causing a short circuit between the positive and negative electrodes and generating heat, thus resulting in a lower failure temperature of the thermal chamber. In Comparative Example 6, the ceramic coating thickness of the separator is too thick, also failing to meet the requirement of 0.3≤1000*(9a+t) / c^2≤0.58. This excessive thickness occupies too much space, resulting in a lower energy density of the battery cell.
[0157] The parts of this invention not described in detail are techniques known to those skilled in the art.
[0158] The basic principles of the present invention have been described above with reference to specific embodiments. However, it should be noted that the advantages, benefits, and effects mentioned in the present invention are merely examples and not limitations, and should not be considered as essential features of each embodiment of the present invention. Furthermore, the specific details disclosed above are for illustrative and facilitative purposes only, and are not limitations. These details do not limit the present invention to the necessity of employing the aforementioned specific details.
[0159] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, then the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, then the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single element or multiple elements. Item B may contain a single element or multiple elements. Item C may contain a single element or multiple elements.
[0160] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A battery, characterized in that, It includes a positive electrode, a negative electrode, an electrolyte, and a separator disposed between the positive electrode and the negative electrode; The positive electrode sheet includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector, the positive electrode film layer including a positive electrode active material, the positive electrode active material containing Al element; The separator includes a separator substrate and a coating disposed on at least one surface of the separator substrate, the coating including a ceramic coating; The battery satisfies: 0.3 ≤ 1000·(9a+t) / c^2 ≤ 0.58; The mass percentage (a) of Al element in the positive electrode active material is 0.2%–0.6%; the thickness (t) of the ceramic coating is 4 μm–8 μm; and the surface density (c) of the positive electrode film is 115 g / m³. 2 ~190g / m 2 ; Wherein, 'a' represents the mass percentage of Al element in the positive electrode active material, expressed in % (%). t represents the thickness of the ceramic coating, in μm; c is the areal density of the positive electrode film, in g / m³. 2 .
2. The battery according to claim 1, characterized in that, The battery satisfies: 0.32≤1000·(9a+t) / c^2≤0.
55.
3. The battery according to claim 1, characterized in that, The mass percentage (a) of Al element in the positive electrode active material is 0.3% to 0.5%.
4. The battery according to claim 1, characterized in that, The thickness t of the ceramic coating is 5μm to 7μm.
5. The battery according to claim 1, characterized in that, The surface density c of the positive electrode film is 150 g / m². 2 ~190g / m 2 .
6. The battery according to claim 2, characterized in that, The battery satisfies: 0.34≤1000·(9a+t) / c^2≤0.
52.
7. The battery according to any one of claims 1 to 6, characterized in that, The positive electrode active material includes a lithium-containing transition metal oxide, and the general chemical formula of the lithium-containing transition metal oxide is: Li d Ni x Co y Mr z Al f M n O2; Wherein, 1.0≤d≤1.2, 0.8≤x<1, 0.01≤y≤0.15, 0.01≤z≤0.15, 0.001≤f≤0.10, 0≤n≤0.05, x+y+z+f+n=1; The M includes at least one of Ti, Cr, B, Mg, Zn, Sn, Mo, Zr, Fe, V, Sr, Nb, W, or Cu; And / or, the ceramic particles in the ceramic coating include at least one of alumina, silicon oxide, titanium oxide, zirconium oxide, barium titanate, yttrium-doped zirconium oxide, gadolinium-doped cerium oxide, and lithium aluminate; And / or, the membrane substrate comprises at least one of polyethylene, polypropylene, poly(p-phenylene terephthalamide), polyethylene terephthalate, polyacrylonitrile, polytetrafluoroethylene, polyamide, or polyimide; And / or, the thickness of the positive current collector is 3μm to 50μm; And / or, the mass percentage of the positive electrode active material in the positive electrode film layer is 94% to 98%.
8. The battery according to claim 7, characterized in that, The M includes at least one of Ti, Mg, Zn, Nb, Zr, or Sr; And / or, the f satisfies: 0.007 ≤ f ≤ 0.022; And / or, the thickness of the positive current collector is 5 μm to 30 μm.
9. The battery according to claim 7, characterized in that, The ceramic particles have a particle size of 0.8 μm to 1.2 μm; And / or, the thickness of the diaphragm substrate is 5 μm to 15 μm.
10. An electrical appliance, characterized in that, Includes the battery selected from any one of claims 1 to 9.
Citation Information
Patent Citations
High-power lithium battery and preparation method thereof
CN113013497A
Lithium ion battery, battery and electric device
CN117154188A