Lithium metal battery electrolyte and method of making same
By using electrolyte additives to generate a LiCl/LiPxOy SEI/CEI film, the problems of negative electrode volume expansion and uneven deposition in lithium metal batteries are solved, achieving long battery life and high-efficiency operation.
Patent Information
- Application Number
- CN202410276389.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-11
AI Technical Summary
Existing lithium metal batteries suffer from problems such as negative electrode volume expansion and reaction with electrolyte to form an unstable SEI film during cycling, leading to uneven lithium metal deposition and reduced battery cycle life.
A lithium metal electrolyte containing electrolyte additives, ester solvents, and lithium salts is used to generate a LiCl/LiPxOy SEI/CEI film, which blocks side reactions between the electrode and the electrolyte, ensuring the uniformity of charge distribution on the lithium metal surface and forming a stable interface.
It effectively suppresses lithium dendrite growth, improves interface stability, significantly extends the cycle life of lithium metal batteries, and maintains high coulombic efficiency. The preparation process is simple and easy to implement.
Smart Images

Figure CN117936908B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of secondary battery technology, and in particular to a lithium metal battery electrolyte and its preparation method. Background Technology
[0002] With the increasing scarcity of fossil resources, the development of new sustainable energy sources is urgently needed. Lithium metal batteries, as one of the most efficient and clean energy sources, possess high energy density and good stability, and are widely used in electric vehicles, 3C electronic products, and other power battery products. Although lithium metal batteries are widely used in these power battery products, their energy density still cannot meet current demands. Therefore, it is necessary to develop lithium metal batteries with high energy density and high cycle stability.
[0003] Lithium metal is hailed as the "holy grail" material for lithium metal batteries due to its high theoretical specific capacity (~3840 mAh / g) and lowest operating potential (-3.04 V). Lithium metal batteries using lithium metal as the negative electrode can achieve high energy density, thus meeting the demand for high-energy-density lithium metal batteries. However, lithium metal undergoes unlimited volume expansion during cycling and reacts with the electrolyte, forming an unstable organic / inorganic hybrid solid electrolyte interphase (SEI) film. Furthermore, as cycling continues, the side reactions at the negative electrode / electrolyte interface become increasingly severe, resulting in uneven lithium metal deposition, leading to the formation of lithium dendrites and dead lithium, significantly reducing the battery's cycle life.
[0004] To address the instability of the electrode / electrolyte interface, researchers have improved the interface by modulating the construction of an artificial SEI film on the negative electrode side, coating the positive electrode side with materials, and controlling the solvation structure of the electrolyte. Among these methods, controlling the electrolyte solvation structure can significantly improve interfacial instability, thereby enhancing the cycle life of lithium metal batteries. Traditional carbonate electrolytes exhibit severe side reactions with lithium metal. Therefore, developing an additive to alter the solvation structure of the electrolyte, thereby controlling the composition of the SEI film and forming a stable SEI film to stabilize the lithium metal / electrolyte interface, is a pressing challenge in this field. Summary of the Invention
[0005] In view of this, the present invention provides a lithium metal battery electrolyte and its preparation method to solve the problems of negative electrode volume expansion and reaction with the electrolyte in existing lithium metal batteries, resulting in the formation of an unstable solid electrolyte interphase (SEI) film. It also solves the problem of uneven lithium metal deposition, which reduces the cycle life of the battery.
[0006] To achieve the above objectives, the present invention adopts the following technical solution:
[0007] A lithium metal battery electrolyte comprises the following components: electrolyte additives, ester solvents, and lithium salts;
[0008] The structural formula of the electrolyte additive is:
[0009] R1 and R2 are independently selected from oxooxazolyl, phenyl, morpholinyl, adamantyl, cyclohexyl, methylamino, ethyl, tolyl, ethylamino, or chlorine.
[0010] Preferably, the mass concentration of electrolyte additives in the lithium metal battery electrolyte is 0.1% to 5%.
[0011] Preferably, the molar concentration of lithium salt in the lithium metal battery electrolyte is 1 mol / L.
[0012] Preferably, the ester solvent includes two or more of ethylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, and propylene carbonate.
[0013] Preferably, the lithium salt is lithium hexafluorophosphate.
[0014] Another object of the present invention is to provide a method for preparing a lithium metal battery electrolyte, comprising the following steps:
[0015] Lithium salts were mixed with ester solvents to obtain blank lithium metal electrolytes; then the blank lithium metal electrolytes were mixed with electrolyte additives to obtain lithium metal battery electrolytes.
[0016] Preferably, the water oxygen value during the preparation process of the lithium metal battery electrolyte is ≤0.1ppm.
[0017] As can be seen from the above technical solution, compared with the prior art, the present invention has the following beneficial effects:
[0018] This invention provides a lithium metal electrolyte containing electrolyte additives. By adding electrolyte additives, LiCl / LiP can be generated on the lithium metal and the positive electrode surface. x O y The SEI / CEI film effectively blocks side reactions between the electrode and the electrolyte, while ensuring the uniformity of charge distribution on the lithium metal surface, thereby effectively reducing the growth of lithium dendrites. At the same time, the inorganic-rich SEI / CEI film improves the stability of the interface, enabling the lithium metal battery system to operate for a long time, maintain a high and stable coulombic efficiency, and significantly improve the cycle life of the metal battery.
[0019] Furthermore, the present invention provides a method for preparing a lithium metal battery electrolyte, which has a simple preparation process, is easy to implement, and can be easily matched with current electrode improvement schemes. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0021] Figure 1 This is a lithium / lithium symmetry performance diagram of Comparative Example 1 of the present invention;
[0022] Figure 2 This is a lithium / lithium symmetry performance diagram of Comparative Example 2 of the present invention;
[0023] Figure 3 This is a lithium / lithium symmetry performance diagram of Example 1 of the present invention;
[0024] Figure 4 This is a lithium / lithium symmetry performance diagram of Example 2 of the present invention;
[0025] Figure 5 This is a graph showing the lithium / lithium titanate cycle performance of Comparative Example 1 of the present invention;
[0026] Figure 6 This is a graph showing the lithium / lithium titanate cycle performance of Comparative Example 2 of the present invention;
[0027] Figure 7 This is a graph showing the lithium / lithium titanate cycle performance of Example 1 of the present invention;
[0028] Figure 8 This is a graph showing the lithium / lithium titanate cycle performance of Example 2 of the present invention. Detailed Implementation
[0029] This invention provides a lithium metal battery electrolyte, comprising the following components: electrolyte additives, ester solvents, and lithium salts;
[0030] The structural formula of the electrolyte additive is:
[0031] R1 and R2 are independently selected from oxooxazolyl, phenyl, morpholinyl, adamantyl, cyclohexyl, methylamino, ethyl, tolyl, ethylamino, or chlorine.
[0032] In this invention, R1 and R2 are preferably the same group.
[0033] In this invention, the mass concentration of electrolyte additives in the lithium metal battery electrolyte is 0.1% to 5%, specifically 0.5%, 1%, 2%, 3%, or 4%.
[0034] In this invention, the molar concentration of lithium salt in the lithium metal battery electrolyte is 1 mol / L.
[0035] In this invention, the ester solvent includes two or more of ethylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, and propylene carbonate.
[0036] In this invention, when multiple ester solvents are included, the different types of ester solvents are preferably mixed in equal volume ratios.
[0037] In this invention, the lithium salt is lithium hexafluorophosphate.
[0038] This invention also provides a method for preparing a lithium metal battery electrolyte, comprising the following steps:
[0039] Lithium salts were mixed with ester solvents to obtain blank lithium metal electrolytes; then the blank lithium metal electrolytes were mixed with electrolyte additives to obtain lithium metal battery electrolytes.
[0040] In this invention, the preferred preparation method is:
[0041] S1: When the oxygen value of water is less than or equal to 0.1 ppm, different types of ester solvents are mixed in equal volume ratio and stirred at room temperature for 30 min to obtain the mixed ester solvent;
[0042] S2: When the oxygen value of water is less than or equal to 0.1 ppm, lithium salt is added to the mixed ester solvent prepared in S1, and the mixture is stirred at room temperature for 60 min to obtain blank lithium metal electrolyte.
[0043] S3: When the water oxygen value is less than or equal to 0.1 ppm, add the electrolyte additive to the blank lithium metal electrolyte and stir for 30 min at room temperature to obtain a lithium metal battery electrolyte containing the electrolyte additive.
[0044] In this invention, the water oxygen value during the preparation of the lithium metal battery electrolyte is ≤0.1ppm, specifically 0.01ppm, 0.02ppm, 0.05ppm, 0.06ppm, or 0.08ppm.
[0045] In this invention, the battery prepared using lithium metal battery electrolyte includes a positive electrode, a negative electrode, a separator, and a lithium metal battery electrolyte.
[0046] In this invention, the cathode material is preferably lithium iron phosphate (LiFePO4), lithium cobalt oxide (LiCoO2), or a ternary material (LiNi). x Co y Mn 1-y O2; the values of x and y are 0.5≤x≤1, 0≤y≤0.2), lithium nickel manganese oxide (LiNi0.5 Mn 1.5 O4), lithium-rich (aLiMnO2·(1-a)LiMO2; the value of a ranges from 0 to a < 1), sulfur, lithium titanate (Li4Ti5O) 12 ).
[0047] In this invention, the negative electrode material is preferably a lithium metal negative electrode; the separator is preferably glass fiber (GF), polyethylene (PE), polypropylene (PP), PP / PE, or PP / PE / PP membrane.
[0048] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0049] Positive electrode: Lithium titanate, acetylene black, and polyvinylidene fluoride are mixed evenly in a mass ratio of 90:5:5. Then, an appropriate amount of N-methylpyrrolidone (NMP) is added to the evenly mixed powder sample and stirred for 8 hours. The resulting slurry is then coated onto aluminum foil by a casting coating method. After drying at 120°C, rolling, and cutting, a positive electrode sheet with a diameter of 13 mm is obtained. The areal density of the positive electrode sheet is 11.5 mg / cm.
[0050] Negative electrode: Φ15mm lithium metal disc.
[0051] Separator: Celgard2325 PP / PE / PP separator.
[0052] When the oxygen content in the water is less than 0.1 ppm, the battery can be assembled in the following order: negative electrode shell - lithium sheet - separator - positive electrode sheet - gasket - spring sheet - positive electrode shell, and electrolyte can be added to obtain a lithium-lithium titanate full cell. By replacing the positive electrode sheet with a lithium sheet, a lithium-lithium symmetric battery can be prepared.
[0053] After the prepared lithium-lithium symmetric battery was left to stand for 12 hours, a current density of 1 mA / cm² was applied. -2 The deposition capacity is 1 mAh / cm³. -2 The test was conducted under the following conditions: the test environment temperature was 25℃. After the prepared lithium-cathode full cell was left to stand for 12 hours, the voltage range was 1.0-2.5V.
[0054] Comparative Example 1
[0055] When the oxygen content in the water is less than 0.1 ppm, ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate are mixed in a volume ratio of 1:1:1 and stirred at room temperature for 30 min to obtain a mixed ester solvent. Lithium hexafluorophosphate (LiPF6) is added to the ester solvent (the concentration of lithium salt in the electrolyte is 1.0 mol / L) and stirred at room temperature for 60 min to obtain an additive-free carbonate electrolyte.
[0056] The electrolyte obtained by this method was used to prepare lithium-lithium symmetric cells and lithium-lithium titanate full cells according to the aforementioned steps, with a current density of 1 mA cm⁻¹. -2 The capacity is 1mA cm -2 Under these conditions, the lithium titanate battery can be stably cycled for 160 hours, with a polarization voltage of 410mV and a voltage range of 1.0-2.5V. After 200 cycles, the capacity retention of the lithium titanate battery is 60.35%. The performance graph of the lithium-lithium symmetric battery is shown below. Figure 1 As shown in the figure, the cycle performance of the lithium-lithium titanate full cell is as follows: Figure 5 As shown.
[0057] Comparative Example 2
[0058] When the oxygen content in the water is less than 0.1 ppm, ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate are mixed in a volume ratio of 1:1:1 and stirred at room temperature for 30 min to obtain a mixed ester solvent. Lithium hexafluorophosphate (LiPF6) is added to the ester solvent (the concentration of lithium salt in the electrolyte is 1.0 mol / L), and stirred at room temperature for 60 min. Then, 5% (by mass) of fluoroethylene carbonate relative to the mass fraction of the carbonate electrolyte is added to the carbonate electrolyte to obtain an electrolyte containing fluoroethylene carbonate.
[0059] The electrolyte obtained by this method was used to prepare lithium-lithium symmetric cells and lithium-lithium titanate full cells according to the aforementioned steps, with a current density of 1 mA cm⁻¹. -2 The capacity is 1mAh cm -2 Under these conditions, the lithium titanate battery can be stably cycled for 170 hours, with a polarization voltage of 105mV and a voltage range of 1.0-2.5V. After 200 cycles, the capacity retention rate is 67.10%. The performance graph of the lithium-lithium symmetric battery is shown below. Figure 2 As shown in the figure, the cycle performance of the lithium-lithium titanate full cell is as follows: Figure 6 As shown.
[0060] Example 1
[0061] When the oxygen content in the water is less than 0.1 ppm, ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate are mixed in a volume ratio of 1:1:1 and stirred at room temperature for 30 min to obtain a mixed ester solvent. Lithium hexafluorophosphate (LiPF6) is added to the ester solvent (the concentration of lithium salt in the electrolyte is 1.0 mol / L), and stirred at room temperature for 60 min. Then, 0.2% (by mass fraction) of bis(2-oxo-3-oxazolyl)phosphine chloride relative to the mass fraction of the carbonate electrolyte is added to the carbonate electrolyte to obtain an electrolyte containing bis(2-oxo-3-oxazolyl)phosphine chloride.
[0062] The electrolyte obtained by this method was used to prepare lithium-lithium symmetric cells and lithium-lithium titanate full cells according to the aforementioned steps, with a current density of 1 mA cm⁻¹. -2 The capacity is 1mAh cm -2 Under these conditions, the lithium titanate battery can be stably cycled for 1200 hours, with a polarization voltage of 87mV and a voltage range of 1.0-2.5V. After 200 cycles, the capacity retention rate is 95.34%. The performance graph of the lithium-lithium symmetric battery is shown below. Figure 3 As shown in the figure, the cycle performance of the lithium-lithium titanate full cell is as follows: Figure 7 As shown. The structural formula of bis(2-oxo-3-oxazolyl)phosphine chloride is as follows:
[0063]
[0064] Example 2
[0065] When the oxygen content in the water is less than 0.1 ppm, ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate are mixed in a volume ratio of 1:1:1 and stirred at room temperature for 30 min to obtain a mixed ester solvent. Lithium hexafluorophosphate (LiPF6) is added to the ester solvent (the concentration of lithium salt in the electrolyte is 1.0 mol / L), and stirred at room temperature for 60 min. Then, 0.5% (by mass fraction) of phenylphosphonic dichloride relative to the mass fraction of the carbonate electrolyte is added to the carbonate electrolyte to obtain an electrolyte containing phenylphosphonic dichloride.
[0066] The electrolyte obtained by this method was used to prepare lithium-lithium symmetric cells and lithium-lithium titanate full cells according to the aforementioned steps, with a current density of 1 mA cm⁻¹. -2 The capacity is 1mAh cm -2 Under these conditions, the lithium titanate battery can be stably cycled for 600 hours, with a polarization voltage of 94mV and a voltage range of 1.0-2.5V. After 200 cycles, the capacity retention rate of the lithium titanate battery is 84.85%. The performance graph of the lithium-lithium symmetric battery is shown below. Figure 4 As shown in the figure, the cycle performance of the lithium-lithium titanate full cell is as follows: Figure 8 As shown. The structural formula of phenylphosphonic dichloride is as follows:
[0067]
[0068] Example 3
[0069] When the oxygen content in the water is less than 0.1 ppm, ethylene carbonate (EC) and diethyl carbonate (DEC) are mixed at a volume ratio of 1:1 and stirred at room temperature for 30 min to obtain a mixed ester solvent. Lithium hexafluorophosphate (LiPF6) is added to the ester solvent (the concentration of lithium salt in the electrolyte is 1.0 mol / L) and stirred at room temperature for 60 min. Then, 0.5% (by mass fraction) of dimorpholine phosphonochloride relative to the mass fraction of the carbonate electrolyte is added to the carbonate electrolyte to obtain an electrolyte containing dimorpholine phosphonochloride.
[0070] The electrolyte obtained by this method was used to prepare lithium-lithium symmetric cells and lithium-lithium titanate full cells according to the aforementioned steps, with a current density of 1 mA cm⁻¹. -2 The capacity is 1mAh cm -2 Under these conditions, lithium titanate can be stably cycled for 800 hours, with a polarization voltage of 85mV and a voltage range of 1.0-2.5V. After 200 cycles, the capacity retention of the tested lithium titanate is 81.05%. The structural formula of dimorpholine phosphonochloride is as follows:
[0071]
[0072] Example 4
[0073] When the oxygen content in the water is less than 0.1 ppm, ethylene carbonate (EC) and diethyl carbonate (DEC) are mixed at a volume ratio of 1:1 and stirred at room temperature for 30 min to obtain a mixed ester solvent. Lithium hexafluorophosphate (LiPF6) is added to the ester solvent (the concentration of lithium salt in the electrolyte is 1.0 mol / L) and stirred at room temperature for 60 min. Then, 0.5% (by mass fraction) of diphenylphosphine chloride relative to the mass fraction of the carbonate electrolyte is added to the carbonate electrolyte to obtain an electrolyte containing diphenylphosphine chloride.
[0074] The electrolyte obtained by this method was used to prepare lithium-lithium symmetric cells and lithium-lithium titanate full cells according to the aforementioned steps, with a current density of 1 mA cm⁻¹. -2 The capacity is 1mAh cm -2 Under these conditions, lithium titanate can be stably cycled for 500 hours, with a polarization voltage of 99mV and a voltage range of 1.0-2.5V. After 200 cycles, the capacity retention of the tested lithium titanate is 79.85%. The structural formula of diphenylphosphine chloride is as follows:
[0075]
[0076] Example 5
[0077] When the oxygen content in the water is less than 0.1 ppm, ethylene carbonate (EC) and propylene carbonate (PC) are mixed at a volume ratio of 1:1 and stirred at room temperature for 30 min to obtain a mixed ester solvent. Lithium hexafluorophosphate (LiPF6) is added to the ester solvent (the concentration of lithium salt in the electrolyte is 1.0 mol / L) and stirred at room temperature for 60 min. Then, 1.0% of bis-1-adamantylphosphine chloride relative to the mass fraction of the carbonate electrolyte is added to the carbonate electrolyte to obtain an electrolyte containing bis-1-adamantylphosphine chloride.
[0078] The electrolyte obtained by this method was used to prepare lithium-lithium symmetric cells and lithium-lithium titanate full cells according to the aforementioned steps, with a current density of 1 mA cm⁻¹. -2 The capacity is 1mAh cm -2 Under these conditions, the lithium titanate can be stably cycled for 505 hours, with a polarization voltage of 97 mV and a voltage range of 1.0-2.5 V. After 200 cycles, the capacity retention of the lithium titanate is 75.65%. The structural formula of bis-1-adamantylphosphinochloride is as follows:
[0079]
[0080] Example 6
[0081] When the oxygen content in the water is less than 0.1 ppm, ethylene carbonate (EC) and propylene carbonate (PC) are mixed at a volume ratio of 1:1 and stirred at room temperature for 30 min to obtain a mixed ester solvent. Lithium hexafluorophosphate (LiPF6) is added to the ester solvent (the concentration of lithium salt in the electrolyte is 1.0 mol / L) and stirred at room temperature for 60 min. Then, 1.0% (by mass fraction) of dicyclohexylphosphoric chloride relative to the mass fraction of the carbonate electrolyte is added to the carbonate electrolyte to obtain an electrolyte containing dicyclohexylphosphoric chloride.
[0082] The electrolyte obtained by this method was used to prepare lithium-lithium symmetric cells and lithium-lithium titanate full cells according to the aforementioned steps, with a current density of 1 mA cm⁻¹. -2 The capacity is 1mAh cm -2 Under these conditions, lithium titanate can be stably cycled for 610 hours, with a polarization voltage of 101 mV and a voltage range of 1.0-2.5 V. After 200 cycles, the capacity retention of the tested lithium titanate is 91.52%. The structural formula of dicyclohexylphosphochloride is as follows:
[0083]
[0084] Example 7
[0085] When the oxygen content in the water is less than 0.1 ppm, ethylene carbonate (EC) and propylene carbonate (PC) are mixed at a volume ratio of 1:1 and stirred at room temperature for 30 min to obtain a mixed ester solvent. Lithium hexafluorophosphate (LiPF6) is added to the ester solvent (the concentration of lithium salt in the electrolyte is 1.0 mol / L) and stirred at room temperature for 60 min. Then, 1.0% (by mass fraction) of bis(dimethylamino)phosphoryl chloride relative to the mass fraction of the carbonate electrolyte is added to the carbonate electrolyte to obtain an electrolyte containing bis(dimethylamino)phosphoryl chloride.
[0086] The electrolyte obtained by this method was used to prepare lithium-lithium symmetric cells and lithium-lithium titanate full cells according to the aforementioned steps, with a current density of 1 mA cm⁻¹. -2 The capacity is 1mAh cm -2 Under these conditions, lithium titanate can be stably cycled for 750 hours, with a polarization voltage of 88mV and a voltage range of 1.0-2.5V. After 200 cycles, the capacity retention of lithium titanate is 82.44%. The structural formula of bis(dimethylamino)phosphoryl chloride is as follows:
[0087]
[0088] Example 8
[0089] When the oxygen content in the water is less than 0.1 ppm, ethylene carbonate (EC) and dimethyl carbonate (DMC) are mixed at a volume ratio of 1:1 and stirred at room temperature for 30 min to obtain a mixed ester solvent. Lithium hexafluorophosphate (LiPF6) is added to the ester solvent (the concentration of lithium salt in the electrolyte is 1.0 mol / L) and stirred at room temperature for 60 min. Then, 2.0% (by mass fraction) of diethylphosphine chloride relative to the mass fraction of the carbonate electrolyte is added to the carbonate electrolyte to obtain an electrolyte containing diethylphosphine chloride.
[0090] The electrolyte obtained by this method was used to prepare lithium-lithium symmetric cells and lithium-lithium titanate full cells according to the aforementioned steps, with a current density of 1 mA cm⁻¹. -2 The capacity is 1mAh cm -2 Under these conditions, lithium titanate can be stably cycled for 850 hours, with a polarization voltage of 83mV and a voltage range of 1.0-2.5V. After 200 cycles, the capacity retention of the tested lithium titanate is 76.49%. The structural formula of diethylphosphine chloride is as follows:
[0091]
[0092] Example 9
[0093] When the oxygen content in the water is less than 0.1 ppm, ethylene carbonate (EC) and dimethyl carbonate (DMC) are mixed at a volume ratio of 1:1 and stirred at room temperature for 30 min to obtain a mixed ester solvent. Lithium hexafluorophosphate (LiPF6) is added to the ester solvent (the concentration of lithium salt in the electrolyte is 1.0 mol / L) and stirred at room temperature for 60 min. Then, 2.0% (by mass fraction) of diisopropoxyphosphoryl chloride relative to the mass fraction of the carbonate electrolyte is added to the carbonate electrolyte to obtain an electrolyte containing diisopropoxyphosphoryl chloride.
[0094] The electrolyte obtained by this method was used to prepare lithium-lithium symmetric cells and lithium-lithium titanate full cells according to the aforementioned steps, with a current density of 1 mA cm⁻¹. -2 The capacity is 1mAh cm -2 Under these conditions, lithium titanate can be stably cycled for 1000 hours, with a polarization voltage of 97mV and a voltage range of 1.0-2.5V. After 200 cycles, the capacity retention of the tested lithium titanate is 89.47%. The structural formula of diisopropoxyphosphoryl chloride is as follows:
[0095]
[0096] Example 10
[0097] When the oxygen content in the water is less than 0.1 ppm, ethylene carbonate (EC) and dimethyl carbonate (EMC) are mixed at a volume ratio of 1:1 and stirred at room temperature for 30 min to obtain a mixed ester solvent. Lithium hexafluorophosphate (LiPF6) is added to the ester solvent (the concentration of lithium salt in the electrolyte is 1.0 mol / L) and stirred at room temperature for 60 min. Then, 2.0% (by mass fraction) of dibis(diethylamino)phosphine chlorate is added to the carbonate electrolyte to obtain an electrolyte containing dibis(diethylamino)phosphine chlorate.
[0098] The electrolyte obtained by this method was used to prepare lithium-lithium symmetric cells and lithium-lithium titanate full cells according to the aforementioned steps, with a current density of 1 mA cm⁻¹. -2 The capacity is 1mAh cm -2 Under these conditions, lithium titanate can be stably cycled for 930 hours, with a polarization voltage of 89mV and a voltage range of 1.0-2.5V. After 200 cycles, the capacity retention of the tested lithium titanate is 90.77%. The structural formula of dibis(diethylamino)phosphine chlorate is as follows:
[0099]
[0100] Comparative Example 3
[0101] The only difference between this comparative example and Example 1 is that the amount of bis(2-oxo-3-oxazolyl)phosphine chloride added is 6.0% of the mass fraction of the carbonate electrolyte.
[0102] Comparative Example 4
[0103] The only difference between this comparative example and Example 3 is that the amount of dimorpholine phosphonochloride added is 8.0% of the mass fraction of the carbonate electrolyte.
[0104] The summary tables of the test results are shown in Tables 1 and 2:
[0105] Table 1 Comparison of cycle life and overpotential of different lithium-lithium symmetric batteries
[0106]
[0107]
[0108] Table 2 Performance Comparison of Lithium-Titanium Oxide Full Batteries
[0109]
[0110] Based on Tables 1 and 2, compared with traditional carbonate electrolytes and carbonate electrolytes containing the traditional additive fluoroethylene carbonate, the lithium / lithium symmetric batteries and lithium / lithium titanate full batteries of Examples 1-10 of this invention, which contain phosphoryl groups and chlorine additives, exhibit superior performance. This superior cycle performance is attributed to the generation of LiCl / LiP-rich electrolytes. x O y The SEI / CEI membrane, in which the electrolyte with added bis(2-oxo-3-oxazolyl)phosphine chloride additive exhibits lower overpotential, longer cycle time, and excellent stability in lithium titanate full cells. At the same time, compared with traditional additives, the additive selected in this invention can achieve better improvement effect with less addition, thus demonstrating that the functional groups selected in this invention and the additives composed of the functional groups have good application effect and development prospects.
[0111] In addition, the amount of additives used in Comparative Examples 3 and 4 exceeded the scope of the present invention, thus losing the corresponding effect and significantly reducing battery performance.
[0112] In summary, compared with traditional carbonate electrolytes, the electrolyte of this invention, containing phosphoryl groups and chlorine, exhibits superior cycle performance, far exceeding that of carbonate electrolytes without additives and those with traditional additives. This superior cycle performance is attributed to the generation of LiCl / LiP-rich electrolytes. x O yThe SEI / CEI film suppresses irreversible side reactions between the electrode and electrolyte, effectively reduces lithium dendrite growth, improves the electrode / electrolyte interface, and enables the lithium metal battery system to operate reversibly over a long cycle time, maintaining a high and stable coulombic efficiency. This significantly improves the cycle life of lithium metal batteries and has good application prospects.
[0113] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.
[0114] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A lithium metal battery electrolyte, characterized in that, The components of the lithium metal battery electrolyte are: electrolyte additives, ester solvents and lithium salts; The structural formula of the electrolyte additive is: R1 and R2 are independently selected from oxooxazolyl, phenyl, morpholinyl, adamantyl, cyclohexyl, methylamino, ethyl, tolyl, ethylamino, or chlorine; The mass concentration of electrolyte additives in lithium metal battery electrolytes is 0.1-5%.
2. The lithium metal battery electrolyte according to claim 1, characterized in that, The molar concentration of lithium salt in the electrolyte of a lithium metal battery is 1 mol / L.
3. A lithium metal battery electrolyte according to any one of claims 1 to 2, characterized in that, The ester solvents include two or more of ethylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, and propylene carbonate.
4. The lithium metal battery electrolyte according to claim 3, characterized in that, The lithium salt is lithium hexafluorophosphate.
5. A method for preparing a lithium metal battery electrolyte according to any one of claims 1 to 4, characterized in that, Includes the following steps: Lithium salts were mixed with ester solvents to obtain blank lithium metal electrolytes; then the blank lithium metal electrolytes were mixed with electrolyte additives to obtain lithium metal battery electrolytes.
6. The method for preparing a lithium metal battery electrolyte according to claim 5, characterized in that, The water oxygen value during the preparation process of the lithium metal battery electrolyte is ≤0.1ppm.
Citation Information
Patent Citations
Electrolyte solution for nonaqueous electrolyte batteries, and nonaqueous electrolyte battery using same
CN108140891A
Nonaqueous electrolyte solution, nonaqueous sodium-ion battery, nonaqueous potassium-ion battery, method for producing nonaqueous sodium-ion battery, and method for producing nonaqueous potassium-ion battery