A high-strength titanium alloy MIM forming process
By introducing equal-proportion mixing and particle size screening technology into the titanium alloy MIM forming process, combined with degreasing and sintering processes, and monitoring product volume changes, the problems of uneven particles and inconsistent density shrinkage during mixing are solved, and the quality of the product is improved. rate and accuracy.
Patent Information
- Application Number
- CN202410287026.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-03-13
AI Technical Summary
In the titanium alloy MIM forming process, a small part of the blank material with larger particle size appears during the mixing process, resulting in different densities during subsequent injection molding, resulting in defective products, and the density and shrinkage of different products are inconsistent, affecting the quality of the product. rate and accuracy.
A high-strength titanium alloy MIM forming and preparation process consisting of a proportioning module, a screening module, an injection molding module and a feedback module is used to perform equal-proportion mixing and particle size screening through pressure sensors and centrifugal screening cylinders to ensure the uniformity of the blanks. , and conduct uniform heating and densification processing through a degreasing furnace and a sintering furnace, while using a test closed chamber and a pneumatic pump to monitor the volume change of the product.
It improves the yield and precision of the product, ensures uniform and dense shrinkage of the blank, and enhances the controllability of subsequent processes and the accuracy of production records.
Smart Images

Figure CN117943546B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium alloy MIM forming, and in particular to a high-strength titanium alloy MIM forming preparation process. Background Art
[0002] MIM is the abbreviation of metal powder injection molding technology. It is a new type of powder metallurgy near-net shape molding technology formed by introducing modern plastic injection molding technology into the field of powder metallurgy.
[0003] In the titanium alloy MIM forming process, titanium alloy metal powder and binder are mixed in equal proportions to form processed granular blanks. However, a small portion of blanks with larger particle sizes will appear in the mixing process, which makes the blanks produced during subsequent blank injection molding prone to uneven density. The products produced after subsequent heating, degreasing and sintering are mostly defective. Therefore, a screening process should be added after the blanks are produced to improve the overall product yield. At the same time, after the blanks are sintered, the products will shrink densely to the designed high-precision dimensions. Different products have different structures and their dense shrinkage conditions are also inconsistent. Therefore, it is necessary to constantly detect and monitor the dense shrinkage from blanks to finished products. Therefore, a high-strength titanium alloy MIM forming preparation process is proposed. Summary of the invention
[0004] The purpose of the present invention is to solve the problem in the prior art that a small part of the blanks with larger particles will appear during the mixing process, which makes the blanks produced during the subsequent injection molding of the blanks easy to have different densities, and the products produced after the subsequent heating, degreasing and sintering are mostly defective products. Therefore, a screening process should be added after the blanks are produced to improve the yield rate of the overall product. At the same time, after the blanks are sintered, the products will shrink densely to the designed high-precision dimensions. Different products have different structures and their dense shrinkage conditions are also inconsistent. Therefore, it is necessary to constantly detect and monitor the dense shrinkage conditions from the blanks to the finished products. A high-strength titanium alloy MIM forming preparation process is proposed.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A high-strength titanium alloy MIM forming preparation process, consisting of a proportioning module, a screening module, an injection molding module, a forming module and a feedback module, the proportioning module consisting of a pressure sensor and a proportioning chamber, the screening module consisting of a centrifugal screening cylinder and a multiple screening plate, the injection molding module consisting of an injection molding machine and a syringe, the forming module consisting of a degreasing furnace and a MIM sintering furnace, and the feedback module consisting of a test closed chamber and an air pressure pump.
[0007] Preferably, the pressure sensor in the proportioning module is arranged at the bottom of the proportioning chamber, and the feed port and discharge port of the proportioning chamber are both provided with self-regulating valve ports, the self-regulating valve ports are controlled by electronically controlled elements, the pressure sensor controls the electronically controlled elements through electrical signals, and a feed hopper is provided on the feed port of the proportioning chamber.
[0008] Preferably, the multiple screening plates in the screening module are arranged at the inner bottom of the centrifugal screening cylinder, a feeding cylinder is arranged in the centrifugal screening cylinder, the feeding cylinder is fixedly connected to the top of the centrifugal screening cylinder, and a Jiaolong spiral blade is arranged on the inner side wall of the centrifugal screening cylinder.
[0009] Preferably, an auxiliary heating ring is arranged on the outer side wall of the syringe of the injection molding module, a plurality of groups of electric heating wires are arranged inside the auxiliary heating ring, and the syringe port is connected to an impeller.
[0010] Preferably, two docking turntables are arranged in the degreasing furnace in the forming module, and the opposite end surfaces of the two docking turntables are provided with a plurality of limiting grooves, and the upper and lower end surfaces of the two docking turntables are respectively connected to hydraulic push rods.
[0011] Preferably, a heating drum is provided in the sintering furnace in the forming module, and a placing platform is provided in the heating drum.
[0012] Preferably, a limit clamp is provided in the test closed cavity in the feedback module, the test closed cavity is assembled from two upper and lower cavity plates, a sealing rubber pad is provided between the two cavity plates, and the output end of the air pressure pump is interconnected with the cavity plate above the test closed cavity.
[0013] S1: Pour titanium alloy metal powder and binder into two proportioning chambers from two feed hoppers respectively. The pressure sensors at the bottom of the two proportioning chambers are set with different starting sensing values. After reaching the sensing value, the pressure sensors will control the self-regulating valve port of the upper feed port to close and the self-regulating valve port of the lower discharge port to open through electrical signals, ensuring that the titanium alloy metal powder and binder in the two proportioning chambers are always mixed in equal proportions, thereby improving the overall proportioning rate.
[0014] S2: Pour the mixed raw material particles into the feed cylinder of the centrifugal screening cylinder. The feed cylinder and the centrifugal screening cylinder keep rotating synchronously, and the raw materials with satisfactory particle sizes are screened out from the multiple screening plates. The raw materials with larger particle sizes are thrown to the edge of the centrifugal screening cylinder under the action of centrifugal force, and then transported and screened along the Jiaolong spiral blades.
[0015] S3: The heated blank is loaded into the syringe, and the heating wire in the auxiliary heating ring on the outer wall of the syringe is energized to ensure that the inside of the syringe maintains a high temperature during the continuous injection process. During the continuous injection process, the fine particles will drive the impeller at the syringe port to rotate, thereby evenly injecting the blank into the mold cavity of the injection molding machine.
[0016] S4: Place the molded blank in the limiting groove on the docking turntable in the degreasing furnace, and then dock the two docking turntables through a hydraulic push rod to facilitate continuous adjustment of the heating angle of the injection molded blank and facilitate the gradual discharge of the adhesive from different parts of the blank along the tiny channels between the particles without reducing the strength of the blank.
[0017] S5: The degreased blank is placed on a placement plate in a sintering furnace for sintering. The continuous rotation of the heating drum in the sintering furnace allows the degreased blank to be heated more evenly.
[0018] At different stages of the blank, the blank is placed on the limiting clamp in the test closed cavity, and then gas is introduced into the test closed cavity through an air pressure pump. The change in air pressure after the front and rear air flows enter is used to determine the change in space in the test closed cavity, thereby determining the volume change of the formed product and the injection molded blank and defatted blank, and understanding the shrinkage rate of the produced product, which is convenient for production records.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The blanks are quickly produced into injection molded blanks through proportioning, grade screening and injection molding. In the screening process, large-particle blanks that are not suitable for injection molding are screened out and re-mixed, which can improve the overall yield of subsequent products.
[0021] 2. The space change in the test closed cavity can be known according to the pressure change after the same airflow enters, so as to know the volume change of the formed product and the injection molded blank and the defatted blank, understand the shrinkage rate of the produced product, and facilitate production records. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 A schematic diagram of a high-strength titanium alloy MIM forming preparation process proposed by the present invention;
[0023] Figure 2 This is a preparation process guide diagram for a high-strength titanium alloy MIM forming preparation process proposed in the present invention. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0025] Embodiment 1, refer to Figure 1-2 , a high-strength titanium alloy MIM forming preparation process, consisting of a proportioning module, a screening module, an injection molding module, a forming module and a feedback module, the proportioning module is composed of a pressure sensor and a proportioning chamber, the screening module is composed of a centrifugal screening cylinder and a multiple screening plate, and the injection molding module is composed of an injection molding machine and a syringe;
[0026] Further, the pressure sensor in the proportioning module is arranged at the bottom of the proportioning chamber, the feed port and the discharge port of the proportioning chamber are both provided with self-regulating valve ports, the self-regulating valve ports are controlled by electric control elements, the pressure sensor controls the electric control elements through electric signals, the feed port of the proportioning chamber is provided with a feed hopper, the multiple screen plates in the screening module are arranged at the inner bottom of the centrifugal screening cylinder, the centrifugal screening cylinder is provided with a feed cylinder, the feed cylinder is fixedly connected to the top of the centrifugal screening cylinder, the inner side wall of the centrifugal screening cylinder is provided with Jiaolong spiral blades, the outer side wall of the syringe of the injection molding module is provided with an auxiliary heating sleeve, the auxiliary heating sleeve is provided with multiple groups of electric heating wires, and the syringe port is connected with an impeller member;
[0027] It should be noted that: in the process of producing blanks, titanium alloy metal powder and binder of equal proportions are quickly proportioned in a proportioning chamber for mixing, and then the granular blanks produced by mixing are transported to the screening process area, and the blank particles are poured into a centrifugal screening cylinder, and particles of different particle sizes are screened by the centrifugal force of rotation to prevent particles of larger particle sizes from entering the subsequent production process. The screened blanks are injected into the mold cavity of the injection molding machine through a syringe and solidified to form injection molded blanks;
[0028] A further advantage of adopting the above method is that the blanks can be quickly produced into injection molded blanks through proportioning mixing, grade screening and injection molding, and large particles of blanks that are not suitable for injection molding can be screened out during the screening process for re-mixing, thereby improving the overall yield of subsequent products.
[0029] Example 2, refer to Figure 1-2 , the forming module is composed of a debinding furnace and a MIM sintering furnace, and the feedback module is composed of a test closed chamber and an air pressure pump;
[0030] Furthermore, two docking turntables are arranged in the degreasing furnace in the forming module, and a plurality of limiting grooves are provided on the opposite end surfaces of the two docking turntables, and the upper and lower end surfaces of the two docking turntables are respectively connected with hydraulic push rods, and a heating drum is arranged in the sintering furnace in the forming module, and a placing platform is arranged in the heating drum, and a limiting clamping plate is arranged in the test closed cavity in the feedback module, and the test closed cavity is assembled by upper and lower cavity plates, and a sealing rubber pad is arranged between the two cavity plates, and the output end of the air pressure pump is connected with the cavity plate above the test closed cavity;
[0031] It should be noted that: in the process of degreasing the blank, the main binder in the blank is gradually and efficiently removed through a special degreasing furnace, and the heating angle of the injection molded blank is continuously adjusted during the heating process, so that the binder is gradually discharged from different parts of the blank along the tiny channels between the particles without reducing the strength of the blank. After the blank is degreased, the residual binder is sintered and removed, so that the blank is densified to obtain a high-precision product, and the blank is placed on a limit clamp in the test closed cavity, and then the gas introduced into the test closed cavity is detected by a pneumatic pump;
[0032] A further advantage of adopting the above method is that the space change in the test closed cavity can be known based on the air pressure change after the same airflow enters, thereby knowing the volume change of the formed product and the injection molded blank and the defatted blank, understanding the shrinkage rate of the produced product, and facilitating production records.
[0033] A high-strength titanium alloy MIM forming preparation process, the preparation process includes the following specific processes:
[0034] S1: Pour titanium alloy metal powder and binder into two proportioning chambers from two feed hoppers respectively. The pressure sensors at the bottom of the two proportioning chambers are set with different starting sensing values. After reaching the sensing value, the pressure sensors will control the self-regulating valve port of the upper feed port to close and the self-regulating valve port of the lower discharge port to open through electrical signals, ensuring that the titanium alloy metal powder and binder in the two proportioning chambers are always mixed in equal proportions, thereby improving the overall proportioning rate.
[0035] S2: Pour the mixed raw material particles into the feed cylinder of the centrifugal screening cylinder. The feed cylinder and the centrifugal screening cylinder keep rotating synchronously, and the raw materials with satisfactory particle sizes are screened out from the multiple screening plates. The raw materials with larger particle sizes are thrown to the edge of the centrifugal screening cylinder under the action of centrifugal force, and then transported and screened along the Jiaolong spiral blades.
[0036] S3: The heated blank is loaded into the syringe, and the heating wire in the auxiliary heating ring on the outer wall of the syringe is energized to ensure that the inside of the syringe maintains a high temperature during the continuous injection process. During the continuous injection process, the fine particles will drive the impeller at the syringe port to rotate, thereby evenly injecting the blank into the mold cavity of the injection molding machine.
[0037] S4: Place the molded blank in the limiting groove on the docking turntable in the degreasing furnace, and then dock the two docking turntables through a hydraulic push rod to facilitate continuous adjustment of the heating angle of the injection molded blank and facilitate the gradual discharge of the adhesive from different parts of the blank along the tiny channels between the particles without reducing the strength of the blank.
[0038] S5: The degreased blank is placed on a placement plate in a sintering furnace for sintering. The continuous rotation of the heating drum in the sintering furnace allows the degreased blank to be heated more evenly.
[0039] At different stages of the blank, the blank is placed on the limiting clamp in the test closed cavity, and then gas is introduced into the test closed cavity through an air pressure pump. The change in air pressure after the front and rear air flows enter is used to determine the change in space in the test closed cavity, thereby determining the volume change of the formed product and the injection molded blank and defatted blank, and understanding the shrinkage rate of the produced product, which is convenient for production records.
[0040] When the present invention is used, in the process of producing blanks, titanium alloy metal powder and binder of equal proportions are quickly proportioned by a proportioning chamber for mixing, and then the granular blanks produced by mixing are transported to a screening process area, and the blank particles are poured into a centrifugal screening cylinder, and particles of different particle sizes are screened by the centrifugal force of rotation to prevent particles of larger particle sizes from entering the subsequent production process, and the screened blanks are injected into the mold cavity of an injection molding machine through a syringe for solidification and molding into injection blanks, so that the blanks can be quickly produced into injection blanks through proportioning mixing, grade screening and injection molding, and large particle blanks that are not suitable for injection molding are screened out in the screening process for re-mixing, thereby improving the overall yield rate of subsequent products;
[0041] In the process of degreasing the blank, the main binder in the blank is gradually and efficiently removed through a special degreasing furnace. The heating angle of the injection molded blank is continuously adjusted during the heating process to facilitate the gradual discharge of the binder from different parts of the blank along the tiny channels between the particles without reducing the strength of the blank. After the degreasing of the blank is completed, the residual binder is sintered and removed to densify the blank to obtain a high-precision product. The blank is placed on the limit clamp in the test closed cavity, and then the gas introduced into the test closed cavity is detected by an air pressure pump. In this way, the space change in the test closed cavity can be known based on the pressure change after the same air flow enters, thereby knowing the volume change of the formed product and the injection molded blank and the degreased blank, and understanding the shrinkage rate of the produced product, which is convenient for production records.
[0042] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A high-strength titanium alloy MIM forming preparation process, It is characterized in that It is composed of a proportioning module, a screening module, an injection molding module, a forming module and a feedback module, wherein the proportioning module is composed of a pressure sensor and a proportioning chamber, the screening module is composed of a centrifugal screening cylinder and a multiple screening plate, the injection molding module is composed of an injection molding machine and a syringe, the forming module is composed of a degreasing furnace and a MIM sintering furnace, the feedback module is composed of a test closed chamber and an air pressure pump, two docking turntables are arranged in the degreasing furnace of the forming module, a plurality of limiting grooves are provided on the opposite end surfaces of the two docking turntables, and hydraulic push rods are connected to the upper and lower end surfaces of the two docking turntables respectively, a heating drum is arranged in the sintering furnace of the forming module, a placing platform is arranged in the heating drum, a limiting clamp is arranged in the test closed chamber of the feedback module, the test closed chamber is assembled by upper and lower cavity plates, a sealing rubber pad is arranged between the two cavity plates, and the output end of the air pressure pump is communicated with the cavity plate above the test closed chamber; The injection molded blank is placed in the limiting groove on the docking turntable in the degreasing furnace, and then the two docking turntables are docked by the hydraulic push rod, so as to continuously adjust the heating angle of the injection molded blank and gradually discharge the adhesive from different parts of the blank along the tiny channels between the particles without reducing the strength of the blank. The degreased blank is placed on the placement plate in the sintering furnace for sintering. The continuous rotation of the heating drum in the sintering furnace makes the degreased blank heated more evenly. At different stages of the blank, the blank is placed on the limiting clamp in the test closed cavity, and then gas is introduced into the test closed cavity by the air pressure pump. The space change in the test closed cavity is obtained according to the change in air pressure after the same air flow enters, thereby obtaining the volume change of the formed product and the injection molded blank and the degreased blank, understanding the shrinkage rate of the produced product, and facilitating production records.
2. A high-strength titanium alloy MIM forming preparation process according to claim 1, It is characterized in that The pressure sensor in the proportioning module is arranged at the bottom of the proportioning chamber. The feed inlet and discharge port of the proportioning chamber are both provided with self-regulating valve ports. The self-regulating valve ports control the switch through an electric control element. The pressure sensor controls the electric control element through an electrical signal. A feed hopper is provided on the feed inlet of the proportioning chamber.
3. A high-strength titanium alloy MIM forming preparation process according to claim 2, It is characterized in that The multiple screening plates in the screening module are arranged at the inner bottom of the centrifugal screening cylinder. A feeding cylinder is arranged in the centrifugal screening cylinder. The feeding cylinder is fixedly connected to the top of the centrifugal screening cylinder. A Jiaolong spiral blade is arranged on the inner side wall of the centrifugal screening cylinder.
4. A high-strength titanium alloy MIM forming preparation process according to claim 3, It is characterized in that An auxiliary heating ring is arranged on the outer side wall of the syringe of the injection molding module, and a plurality of groups of electric heating wires are arranged inside the auxiliary heating ring. The syringe port is connected to an impeller.
5. A high-strength titanium alloy MIM forming preparation process according to claim 4, It is characterized in that The preparation process includes the following specific processes: S1: Pour the titanium alloy metal powder and the binder into two proportioning chambers from two feed hoppers respectively. The pressure sensors at the bottom of the two proportioning chambers are set with different starting sensing values. When the sensing values are reached, the pressure sensors will control the self-regulating valve port of the upper feed port to close and the self-regulating valve port of the lower discharge port to open through electrical signals, so as to ensure that the titanium alloy metal powder and the binder in the two proportioning chambers are always mixed in equal proportions, thereby improving the overall proportioning rate. S2: Pour the mixed raw material particles into the feed cylinder of the centrifugal screening cylinder. The feed cylinder and the centrifugal screening cylinder rotate synchronously. The raw materials with the required particle size are screened out from the multiple screening plate. The raw materials with larger particle size are thrown to the edge of the centrifugal screening cylinder under the action of centrifugal force, and then transported and screened along the Jiaolong spiral blade; S3: The heated blank is loaded into the syringe, and the heating wire in the auxiliary heating ring on the outer wall of the syringe is energized to ensure that the inside of the syringe maintains a high temperature during the continuous injection process. During the continuous injection process, the fine particles will drive the impeller at the syringe port to rotate, thereby evenly injecting the blank into the mold cavity of the injection molding machine.