Secondary batteries and electronic devices

By adding carbon nanotubes and silicon-based particles to the negative electrode mixture layer of the secondary battery and using specific compounds in the electrolyte, the resistivity growth problem caused by the change in the volume of silicon-based particles is solved, and high energy density and optimization are achieved. Cyclic performance.

CN118156482BActive Publication Date: 2024-11-12NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410574921.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-10
Publication Date
2024-11-12
Estimated Expiration
2044-05-10

AI Technical Summary

Technical Problem

During the high-temperature intermittent cycle and fast charging cycle of secondary batteries, the volume changes of silicon-based particles lead to a significant increase in resistivity, affecting the circulation performance.

Method used

By adding carbon nanotubes and silicon-based particles to the negative electrode mixture layer of the secondary battery, and using dinitrile compounds and trinitrile compounds in the electrolyte, the thickness of the negative electrode mixture layer and the average particle size of the silicon-based particles are controlled to optimize carbon The distribution of nanotubes and the generation of solid electrolyte interface films reduce the possibility of circuit breakage in the conductive network.

Benefits of technology

While achieving high energy density, the growth rate of high-temperature intermittent cycle resistance and the growth rate of fast charging cycle resistance are significantly improved, and the circulation performance of secondary batteries is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
Patent Text Reader

Abstract

The present application provides a secondary battery and an electronic device. The secondary battery comprises a negative electrode, a positive electrode and an electrolyte, wherein the negative electrode comprises a negative electrode current collector and a negative electrode mixture layer disposed on at least one surface of the negative electrode current collector, wherein the thickness of the negative electrode mixture layer is T μm, the negative electrode mixture layer comprises carbon nanotubes and silicon-based particles, the average particle size of the silicon-based particles is D μm, and 3.7≤10T / D 2 ≤24.9; the electrolyte includes a dinitrile compound and a trinitrile compound. The secondary battery provided in the present application achieves a higher energy density while improving the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of energy storage technology, and specifically relates to a secondary battery and an electronic device. Background Art

[0002] In order to meet the requirements of sustainable development, secondary batteries provide a clean energy storage and use solution. With the continuous development of application scenarios, the performance requirements for secondary batteries are also increasing, especially the demand for the energy density of secondary batteries. Because the theoretical capacity of silicon materials is about ten times that of graphite materials, the use of silicon materials to fully or partially replace graphite materials can significantly improve the energy density of secondary batteries. However, during the use of secondary batteries, silicon materials will shrink and expand to a large extent with the insertion and extraction of metal ions, causing the cycle performance of secondary batteries to deteriorate significantly. Therefore, it is necessary to develop a silicon-containing secondary battery that has a high energy density while taking into account the cycle performance of secondary batteries. Summary of the invention

[0003] The purpose of the present application is to provide a secondary battery and an electronic device, which achieve a higher energy density while improving the high-temperature intermittent cycle resistance growth rate and the fast-charge cycle resistance growth rate.

[0004] In a first aspect, the present application provides a secondary battery, comprising a negative electrode, a positive electrode and an electrolyte, wherein the negative electrode comprises a negative electrode current collector and a negative electrode mixture layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode mixture layer comprises carbon nanotubes and silicon-based particles, wherein the thickness of the negative electrode mixture layer is T μm, the average particle size of the silicon-based particles is D μm, and 3.7≤10T / D 2 ≤24.9; the electrolyte includes a dinitrile compound and a trinitrile compound. The secondary battery provided in the present application achieves a higher energy density while improving the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0005] The inventors found that after the secondary battery containing silicon-based particles experienced high-temperature intermittent cycles and fast-charge cycles, the resistivity increased to a large extent. By performing the above-mentioned configuration on the secondary battery, it is possible to achieve a higher energy density while improving the resistance growth rate of the high-temperature intermittent cycle and the resistance growth rate of the fast-charge cycle. The inventors speculate that during the high-temperature intermittent cycle and the fast-charge cycle, the volume of the silicon-based particles expands and contracts significantly, and the carbon nanotubes are displaced as the silicon-based particles expand, and this type of displacement cannot be completely restored as the silicon-based particles shrink, causing the conductive network inside the negative electrode mixture layer to be disconnected, resulting in an increase in resistivity. The thickness T μm of the negative electrode mixture layer and the average particle size D μm of the silicon-based particles jointly affect the distribution state and displaceable space of the carbon nanotubes inside the negative electrode mixture layer; the cyano group in the dinitrile compound and the trinitrile compound has a smaller reaction steric hindrance and a larger nucleophilic property. When the dinitrile and trinitrile compounds containing cyanide groups participate in the formation of the solid electrolyte interface film (SEI film) on the surface of the silicon-based particles, the generated solid electrolyte interface film has a special adsorption force for carbon nanotubes, reducing the possibility of the conductive network inside the negative electrode being broken due to the volume change of the silicon-based particles. By controlling the thickness T μm of the negative electrode mixture layer and the average particle size D μm of the silicon-based particles, the following conditions are met: 3.7≤10T / D 2 ≤24.9, and the electrolyte includes a dinitrile compound and a trinitrile compound, which can enable the secondary battery to achieve a higher energy density while improving the high-temperature intermittent cycle resistance growth rate and the fast-charge cycle resistance growth rate.

[0006] In some embodiments, the dinitrile compound includes at least one of malononitrile, succinonitrile, glutaronitrile, adiponitrile, pimelonitrile, octanonitrile, 3,3'-oxydipropionitrile, hexane-2-enedinitrile, trans-butylenedinitrile, 2-pentene dinitrile, methylglutaronitrile, (Z)-butane-2-enedinitrile, 2,2,3,3-tetrafluorosuccinonitrile or 1,2-bis(2-cyanoethoxy)ethane; and / or, the trinitrile compound includes at least one of 1,3,6-hexanetrinitrile, 1,3,5-pentanetricarbonitrile, 4-(2-cyanoethyl)heptanedinitrile or 1,2,3-tris(2-cyanoethoxy)propane. By adjusting the dinitrile compound to include at least one of the above-mentioned types of substances and / or the trinitrile compound to include at least one of the above-mentioned types of substances, the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery can be improved.

[0007] In some embodiments, the dinitrile compound includes at least two of malononitrile, succinonitrile, glutaronitrile, adiponitrile, heptanenitrile, suberonitrile, 3,3'-oxydipropionitrile, hexane-2-enedinitrile, trans-butylenedinitrile, 2-pentene dinitrile, methylglutaronitrile, (Z)-butane-2-enedinitrile, 2,2,3,3-tetrafluorosuccinonitrile or 1,2-bis(2-cyanoethoxy)ethane; and / or, the trinitrile compound includes at least two of 1,3,6-hexanetrinitrile, 1,3,5-pentanetricarbonitrile, 4-(2-cyanoethyl)heptanedinitrile or 1,2,3-tris(2-cyanoethoxy)propane. By adjusting the dinitrile compound to include at least two of the above-mentioned types of substances and / or the trinitrile compound to include at least two of the above-mentioned types of substances, the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery can be further improved.

[0008] In some embodiments, based on the mass of the electrolyte, the mass percentage of the dinitrile compound is N1%, the mass percentage of the trinitrile compound is N2%, and 1.1≤N1 / N2≤4.9. By adjusting the value of N1 / N2 within the above range, the possibility of the conductive network inside the negative electrode being broken due to the volume change of the silicon-based particles can be reduced, and the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery can be improved. Optionally, 2.2≤N1 / N2≤3.7.

[0009] In some embodiments, based on the quality of the electrolyte, the electrolyte satisfies at least one of the following conditions: (1) 7.0≤10T / D 2 ≤18.1; (2) 60≤T≤122; (3) 7.0≤D≤12.7; (4) 3.2≤N1≤6.8; (5) 1.4≤N2≤2.9. By making the electrolyte satisfy at least one of the above, the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery can be improved. Optionally, the electrolyte satisfies at least one of the following: 78.2≤T≤113.0; 7.6≤D≤10.6; 4.2≤N1≤5.9; 1.6≤N2≤2.5.

[0010] In some embodiments, based on the mass of the electrolyte, the electrolyte satisfies at least one of the following: (1) the electrolyte includes succinonitrile and adiponitrile, based on the mass of the electrolyte, the mass percentage of succinonitrile is A1%, the mass percentage of adiponitrile is A2%, and 1.27≤A1 / A2≤3.36; (2) the electrolyte includes 1,2-bis(2-cyanoethoxy)ethane and 1,3,6-hexanetrinitrile, based on the mass of the electrolyte, the mass percentage of 1,2-bis(2-cyanoethoxy)ethane is B1%, the mass percentage of 1,3,6-hexanetrinitrile is B2%, and 0.83≤B1 / B2≤2.43. By making the electrolyte satisfy at least one of the above, the possibility of the conductive network inside the negative electrode being broken due to the volume change of the silicon-based particles can be reduced, and the high-temperature intermittent cycle resistance growth rate and the fast-charge cycle resistance growth rate of the secondary battery can be improved. Optionally, the electrolyte satisfies at least one of the following: 1.84≤A1 / A2≤2.91; 1.36≤B1 / B2≤2.00.

[0011] In some embodiments, the electrolyte satisfies at least one of the following: (1) 2.8≤A1≤3.7; (2) 1.1≤A2≤2.2; (3) 1.0≤B1≤1.7; (4) 0.7≤B2≤1.2. The mass percentages of succinonitrile, adiponitrile, 1,2-bis(2-cyanoethoxy)ethane and / or 1,3,6-hexanetrinitrile in the electrolyte are regulated to meet the above ranges, which can further improve the high temperature intermittent cycle resistance growth rate and fast charge cycle resistance growth rate of the secondary battery.

[0012] In some embodiments, the electrolyte includes ethylene carbonate and propylene carbonate, and based on the mass of the electrolyte, the mass percentage of ethylene carbonate is X1%, the mass percentage of propylene carbonate is X2%, and the electrolyte satisfies at least one of the following: (1) 29≤X1+X2≤51; (2) 1.1≤X2 / X1≤2.5. By making the electrolyte satisfy at least one of the above, the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery can be improved. Optionally, the electrolyte satisfies at least one of the following: 34≤X1+X2≤46; 1.6≤X2 / X1≤2.2.

[0013] In some embodiments, the electrolyte includes ethyl propionate and propyl propionate, and based on the mass of the electrolyte, the mass percentage of ethyl propionate is Y1%, the mass percentage of propyl propionate is Y2%, and the electrolyte satisfies at least one of the following: (1) 35≤Y1+Y2≤62; (2) 1.2≤Y2 / Y1≤2.9. By making the electrolyte satisfy at least one of the above, the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery can be improved. Optionally, the electrolyte satisfies at least one of the following: 41≤Y1+Y2≤55; 1.5≤Y2 / Y1≤2.5.

[0014] In some embodiments, the electrolyte includes a fluorine-containing compound, and the fluorine-containing compound includes at least one of fluorobenzene or fluoroethylene carbonate. Based on the mass of the electrolyte, the electrolyte satisfies at least one of the following: (1) the mass percentage of fluorobenzene is F1%, 0.9≤F1≤4.1; (2) the mass percentage of fluoroethylene carbonate is F2%, 10.5≤F2≤19.5. By making the electrolyte satisfy at least one of the above, the ability of the generated solid electrolyte interface film to adsorb carbon nanotubes can be enhanced, and the high temperature intermittent cycle resistance growth rate and fast charge cycle resistance growth rate of the secondary battery can be improved. Optionally, the electrolyte satisfies at least one of the following: 2.7≤F1≤3.4; 12.5≤F2≤17.5.

[0015] In some embodiments, the electrolyte includes a compound of formula I, and the mass percentage of the compound of formula I is H%, based on the mass of the electrolyte, and 0.2≤H≤0.9. By making the electrolyte include the compound of formula I and adjusting the value of H within the above range, the elasticity of the solid electrolyte interface film and the ability to adsorb carbon nanotubes can be improved, and the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate can be further improved.

[0016] The chemical formula of the compound of formula I is: .

[0017] In some embodiments, the electrolyte includes a compound of formula II, and the mass percentage of the compound of formula II is G%, 0.2≤G≤0.7 based on the mass of the electrolyte. By adjusting the value of G within the above range, the elasticity of the solid electrolyte interface film and the ability to adsorb carbon nanotubes can be improved, and the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate can be further improved.

[0018] The chemical formula of the compound of formula II is: .

[0019] In some embodiments, the silicon-based particles include a carbon skeleton and a protective layer located on at least a portion of the surface of the carbon skeleton, the material of the protective layer includes amorphous carbon, and the material of the carbon skeleton includes at least one of artificial graphite, natural graphite, mesophase carbon microbeads, soft carbon or hard carbon.

[0020] The second aspect of the present application provides an electronic device, which includes the secondary battery provided by the first aspect of the present application. The electronic device provided by the second aspect of the present application achieves a higher energy density while improving the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0021] Additional aspects and advantages of the embodiments of the present application will be described, shown, or explained in part in the subsequent description through implementation of the embodiments of the present application. DETAILED DESCRIPTION

[0022] The embodiments of the present application will be described in detail below. The embodiments of the present application should not be interpreted as limiting the present application.

[0023] Unless expressly stated otherwise, the following terms used in this application have the meanings indicated below.

[0024] In a first aspect, the present application provides a secondary battery, comprising a negative electrode, a positive electrode and an electrolyte, wherein the negative electrode comprises a negative electrode current collector and a negative electrode mixture layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode mixture layer comprises carbon nanotubes and silicon-based particles, wherein the thickness of the negative electrode mixture layer is T μm, the average particle size of the silicon-based particles is D μm, and 3.7≤10T / D 2 ≤24.9; the electrolyte includes a dinitrile compound and a trinitrile compound. The secondary battery provided in the present application achieves a higher energy density while improving the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0025] negative electrode

[0026] The negative electrode comprises a negative electrode current collector and a negative electrode mixture layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode mixture layer comprises a negative electrode active material. In some embodiments, the chargeable capacity of the negative electrode active material is greater than the discharge capacity of the positive electrode active material to prevent lithium metal from being accidentally deposited on the negative electrode during charging.

[0027] In some embodiments, the thickness of the negative electrode mixture layer is T μm, the negative electrode active material includes silicon-based particles, the average particle size of the silicon-based particles is D μm, and 3.7≤10T / D 2 ≤24.9. In some embodiments, 7.0≤10T / D 2 ≤24.9. In some embodiments, 3.7≤10T / D 2 ≤18.1. In some embodiments, 7.0≤10T / D 2 ≤18.1. In some embodiments, 7.4≤10T / D 2 ≤18.1. In some embodiments, 7.0≤10T / D 2 ≤11.7. In some embodiments, 7.4≤10T / D 2 ≤11.7. In some embodiments, 3.7≤10T / D 2 ≤7.0. In some embodiments, 7.0≤10T / D 2 ≤7.4. In some embodiments, 11.7≤10T / D 2 ≤18.1. In some embodiments, 18.1≤10T / D 2 ≤24.9. In some embodiments, 10T / D 2The value is 3.7, 4.9, 6.6, 6.7, 7.0, 7.38, 7.6, 8.9, 10.5, 11.66, 13.0, 14.5, 15.2, 17.3, 18.1, 18.8, 19.7, 21.0, 22.3, 23.5, 24.9 or a value within the range formed by any two of these values. The present application regulates the thickness T μm of the negative electrode mixture layer and the average particle size D μm of the silicon-based particles to satisfy the above relationship, which can optimize the distribution state and displaceable space of the carbon nanotubes inside the negative electrode mixture layer, and helps to reduce the possibility of short circuits in the conductive network inside the negative electrode due to the volume change of the silicon-based particles, thereby achieving a higher energy density while taking into account the improvement of the high-temperature intermittent cycle resistance growth rate and the fast-charge cycle resistance growth rate.

[0028] In some embodiments, 60≤T≤122. In some embodiments, 78.2≤T≤122. In some embodiments, 60≤T≤113.0. In some embodiments, 78.2≤T≤113.0. In some embodiments, 60≤T≤78.2. In some embodiments, 113.0≤T≤122. In some embodiments, T is 60, 62.2, 69.4, 70.7, 78.2, 80.1, 81.7, 82.9, 83.9, 89.8, 94.2, 98.7, 100.3, 103.2, 108.3, 112.2, 112.9, 114.9, 119.5, 122 or a value within the range of any two of these values. Adjusting the thickness of the negative electrode mixture layer within the above range can improve the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery.

[0029] In some embodiments, 7.0≤D≤12.7. In some embodiments, 7.0≤D≤10.6. In some embodiments, 7.6≤D≤12.7. In some embodiments, 7.6≤D≤10.6. In some embodiments, 7.0≤D≤7.6. In some embodiments, 10.6≤D≤12.7. In some embodiments, D is 7, 7.4, 7.6, 7.7, 7.9, 8.0, 8.5, 9.0, 9.2, 9.6, 10.0, 10.1, 10.6, 10.7, 10.8, 10.9, 11.2, 11.7, 12.0, 12.3, 12.7 or a value within the range of any two of these values. Adjusting the average particle size of the silicon-based particles within the above range can improve the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery.

[0030] In some embodiments, the silicon-based particles include silicon-based materials, silicon-carbon materials (complexes of silicon-based materials and carbon-based materials), or silicon oxide (SiO x , 0<x≤2).

[0031] In some embodiments, the silicon-based material may be silicon particles, silicon alloy particles, etc.

[0032] Exemplarily, the composite of silicon-based substances and carbon-based substances may be an active material obtained by dispersing silicon nanoparticles having an average particle size of 200nm or less on carbon-based substance particles, and then coating with carbon, an active material in which silicon (Si) particles are present on and inside graphite, etc. The average particle size of the secondary particles of the composite of silicon-based substances and carbon-based substances may be 5μm to 20μm. The secondary particles of the composite of silicon-based substances and carbon-based substances in this application refer to silicon-based substance particles and / or carbon-based substance particles in the composite of silicon-based substances and carbon-based substances, such as silicon nanoparticles. The average particle size of silicon nanoparticles may be 5nm or more, for example, 10nm or more, for example, 20nm or more, for example, 50nm or more, for example, 70nm or more. The average particle size of silicon nanoparticles may be 200nm or less, 150nm or less, 100nm or less, 50nm or less, 20nm or less or 10nm or less. For example, the average particle size of silicon nanoparticles may be 100nm to 150nm. The secondary particles of the composite of the silicon-based substance and the carbon-based substance may have an average particle size of 5 μm to 20 μm, for example, 7 μm to 15 μm, for example, 10 μm to 13 μm.

[0033] In some preferred embodiments, the silicon-based particles include a carbon skeleton and a protective layer located on at least a portion of the surface of the carbon skeleton, the material of the protective layer includes amorphous carbon, and the material of the carbon skeleton includes at least one of artificial graphite, natural graphite, mesophase carbon microbeads, soft carbon or hard carbon.

[0034] Optionally, the negative electrode active material may further include an amorphous carbon material, and the amorphous carbon may be soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide or calcined coke, etc.

[0035] The present application has no particular restrictions on the type of negative electrode conductive agent, as long as the purpose of the present application can be achieved. For example, the negative electrode conductive agent can be at least one of acetylene black, Ketjen black, carbon nanotubes, carbon fibers, carbon dots or graphene, and the above carbon nanotubes can include but are not limited to at least one of single-walled carbon nanotubes or multi-walled carbon nanotubes.

[0036] The present application has no particular restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include copper foil, aluminum foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam or a polymer substrate covered with a conductive metal, etc. Among them, the conductive metal includes but is not limited to copper, nickel or titanium, and the material of the polymer substrate includes but is not limited to at least one of polyethylene, polypropylene, ethylene propylene copolymer, polyethylene terephthalate, polyethylene naphthalate or poly(p-phenylene terephthalamide). In the present application, there is no particular restriction on the thickness of the negative electrode current collector and the negative electrode mixture layer, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 12μm, and the thickness of the single-sided negative electrode mixture layer is 30μm to 160μm. In the present application, the negative electrode mixture layer can be arranged on one surface in the thickness direction of the negative electrode current collector, or on two surfaces in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of ​​the negative electrode current collector or a partial area of ​​the negative electrode current collector. This application has no special restrictions as long as the purpose of this application can be achieved.

[0037] The negative electrode active material layer may further include a negative electrode binder. The negative electrode binder can improve the bonding between the negative electrode active material particles and the bonding between the negative electrode active material and the current collector. The type of negative electrode binder is not particularly limited, as long as it is a material that is stable to the solvent used in the electrolyte or electrode manufacturing. In some embodiments, the negative electrode binder includes a resin binder. Examples of resin binders include, but are not limited to, fluororesins, polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, and the like. When an aqueous solvent is used to prepare the negative electrode mixture slurry, the negative electrode binder includes, but is not limited to, hydroxyethylcarboxymethylcellulose (HECMC) or its salt, carboxymethylcellulose (CMC) or its salt, styrene-butadiene rubber (SBR), polyacrylic acid (PAA) or its salt, polyvinyl alcohol, and the like.

[0038] Exemplarily, the negative electrode can be prepared by the following method: a negative electrode mixture slurry containing a negative electrode binder, silicon-carbon composite particles, a conductive agent, etc. is coated on a negative electrode current collector, and after drying, the negative electrode mixture slurry is rolled to form a negative electrode mixture layer on both sides of the negative electrode current collector, thereby obtaining a negative electrode.

[0039] The present application has no particular restrictions on the compaction density of the negative electrode sheet, as long as the purpose of the present application can be achieved. For example, the compaction density of the negative electrode sheet can be 1.0 g / cm 3 Up to 1.85 g / cm 3 The present application has no particular limitation on the cold pressing pressure of the negative electrode sheet, as long as the purpose of the present application can be achieved. For example, the cold pressing pressure of the negative electrode sheet can be 3 tons to 30 tons.

[0040] Electrolyte

[0041] The electrolyte used in the secondary battery of the present application includes an electrolyte and a solvent for dissolving the electrolyte. In some embodiments, the electrolyte of the present application includes dinitrile compounds and trinitrile compounds. The cyano group in the dinitrile compound and the trinitrile compound has a smaller reaction steric hindrance and a larger nucleophilic property. When the dinitrile compound and the trinitrile compound containing the cyano group participate in the generation process of the solid electrolyte interface film on the surface of the silicon-based particles, the generated solid electrolyte interface film has a special adsorption force for adsorbing carbon nanotubes, thereby being able to improve the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery.

[0042] In some embodiments, the dinitrile compound includes at least one of malononitrile, succinonitrile, glutaronitrile, adiponitrile, heptanenitrile, octanonitrile, 3,3'-oxydipropionitrile, hexane-2-enedinitrile, trans-butylenedinitrile, 2-pentene dinitrile, methylglutaronitrile, (Z)-butane-2-enedinitrile, 2,2,3,3-tetrafluorosuccinonitrile or 1,2-bis(2-cyanoethoxy)ethane; and / or, the trinitrile compound includes at least one of 1,3,6-hexanetrinitrile, 1,3,5-pentanetricarbonitrile, 4-(2-cyanoethyl)heptanedinitrile or 1,2,3-tris(2-cyanoethoxy)propane. By adjusting the dinitrile compound and / or the trinitrile compound to include the above-mentioned types of substances respectively, the quality of the SEI film can be improved, and the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery can be improved.

[0043] In some embodiments, the dinitrile compound includes at least two of malononitrile, succinonitrile, glutaronitrile, adiponitrile, heptanenitrile, octanonitrile, 3,3'-oxydipropionitrile, hexane-2-enedinitrile, trans-butylenedinitrile, 2-pentene dinitrile, methylglutaronitrile, (Z)-butane-2-enedinitrile, 2,2,3,3-tetrafluorosuccinonitrile or 1,2-bis(2-cyanoethoxy)ethane; and / or, the trinitrile compound includes at least two of 1,3,6-hexanetrinitrile, 1,3,5-pentanetricarbonitrile, 4-(2-cyanoethyl)heptanedinitrile or 1,2,3-tris(2-cyanoethoxy)propane. By adjusting the dinitrile compound and / or the trinitrile compound to include at least two of the above-mentioned types of substances, it can be better matched with the negative electrode, and the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery are further improved.

[0044] In some embodiments, the mass percentage of the dinitrile compound is N1%, the mass percentage of the trinitrile compound is N2%, and 1.1≤N1 / N2≤4.9. In some embodiments, 2.2≤N1 / N2≤4.9. In some embodiments, 1.1≤N1 / N2≤3.7. In some embodiments, 2.2≤N1 / N2≤3.7. In some embodiments, 2.2≤N1 / N2≤3.3. In some embodiments, 1.1≤N1 / N2≤2.2. In some embodiments, 3.3≤N1 / N2≤3.7. In some embodiments, 3.7≤N1 / N2≤4.9. In some embodiments, the value of N1 / N2 is 1.1, 1.4, 1.6, 1.7, 1.8, 2.0, 2.2, 2.4, 2.9, 3.1, 3.3, 3.5, 3.7, 3.8, 4.3, 4.5, 4.7, 4.9 or a value in the range composed of any two of these values. The present application regulates the value of N1 / N2 within the above range, which can further reduce the possibility of short circuit in the conductive network inside the negative electrode due to the volume change of silicon-based particles, and significantly improve the high-temperature intermittent cycle resistance growth rate and fast-charge cycle resistance growth rate of the secondary battery.

[0045] In some embodiments, 3.2≤N1≤6.8. In some embodiments, 4.9≤N1≤6.8. In some embodiments, 3.2≤N1≤4.9. In some embodiments, 4.9≤N1≤5.9. In some embodiments, 3.2≤N1≤4.9. In some embodiments, 5.9≤N1≤6.8. In some embodiments, the value of N1 is 3.2, 3.4, 3.7, 3.9, 4.1, 4.2, 4.5, 4.7, 4.9, 5.1, 5.2, 5.3, 5.5, 5.6, 5.8, 5.9, 6.2, 6.5, 6.6, 6.8 or a value in the range composed of any two of these values. Regulating the mass percentage of the dinitrile compound in the electrolyte within the above range is conducive to further improving the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery.

[0046] In some embodiments, 1.4≤N2≤2.9. In some embodiments, 1.4≤N2≤2.2. In some embodiments, 1.6≤N2≤2.9. In some embodiments, 1.6≤N2≤2.2. In some embodiments, 1.4≤N2≤1.6. In some embodiments, 2.2≤N2≤2.9. In some embodiments, the value of N2 is 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9 or a value in the range composed of any two of these values. Regulating the mass percentage of the trinitrile compound in the electrolyte within the above range is conducive to further improving the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery.

[0047] In some embodiments, the electrolyte includes succinonitrile and adiponitrile, and the mass percentage of succinonitrile is A1%, the mass percentage of adiponitrile is A2%, and 1.27≤A1 / A2≤3.36 based on the mass of the electrolyte. In some embodiments, 1.84≤A1 / A2≤3.36. In some embodiments, 1.27≤A1 / A2≤2.91. In some embodiments, 1.84≤A1 / A2≤2.91. In some embodiments, 1.27≤A1 / A2≤1.84. In some embodiments, 2.91≤A1 / A2≤3.36. In some embodiments, the value of A1 / A2 is 1.27, 1.33, 1.52, 1.66, 1.78, 2.06, 2.18, 2.35, 2.55, 2.70, 2.77, 3.01, 3.12, 3.26, 3.36, or a value in the range composed of any two of these values. Regulating the mass percentages of succinonitrile and adiponitrile in the electrolyte to satisfy the above relationship can improve the high-temperature intermittent cycle resistance growth rate and the fast-charge cycle resistance growth rate of the secondary battery.

[0048] In some embodiments, 2.8≤A1≤3.7; 1.1≤A2≤2.2. In some embodiments, 2.8≤A1≤3.2. In some embodiments, 2.8≤A1≤3.5. In some embodiments, 3.2≤A1≤3.5. In some embodiments, 3.2≤A1≤3.7. In some embodiments, 3.5≤A1≤3.7. In some embodiments, 1.1≤A2≤1.7. In some embodiments, 1.1≤A2≤1.9. In some embodiments, 1.7≤A2≤2.2. In some embodiments, 1.7≤A2≤1.9. In some embodiments, 1.9≤A2≤2.2. In some embodiments, A1 is 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, or a range consisting of any two of these values. In some embodiments, A2 is 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2 or a value within the range formed by any two of these values. By regulating the succinonitrile and / or adiponitrile in the electrolyte to meet the above ranges, the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery can be further improved.

[0049] In some embodiments, the electrolyte includes 1,2-bis(2-cyanoethoxy)ethane and 1,3,6-hexanetrinitrile, based on the mass of the electrolyte, the mass percentage of 1,2-bis(2-cyanoethoxy)ethane is B1%, the mass percentage of 1,3,6-hexanetrinitrile is B2%, and 0.83≤B1 / B2≤2.43. In some embodiments, 0.83≤B1 / B2≤2.00. In some embodiments, 1.36≤B1 / B2≤2.43. In some embodiments, 1.36≤B1 / B2≤2.00. In some embodiments, 0.83≤B1 / B2≤1.36. In some embodiments, 1.36≤B1 / B2≤2.43. In some embodiments, the value of B1 / B2 is 0.83, 0.91, 1.00, 1.12, 1.32, 1.33, 1.36, 1.55, 1.66, 1.77, 1.82, 2.00, 2.13, 2.19, 2.33, 2.43 or a value in the range of any two of these values. Regulating the mass percentage of 1,2-bis(2-cyanoethoxy)ethane and 1,3,6-hexanetrinitrile in the electrolyte to satisfy the above relationship can improve the high temperature intermittent cycle resistance growth rate and fast charge cycle resistance growth rate of the secondary battery.

[0050] In some embodiments, 1.0≤B1≤1.7; 0.7≤B2≤1.2. In some embodiments, 1.0≤B1≤1.5. In some embodiments, 1.5≤B1≤1.7. In some embodiments, 0.7≤B2≤0.8. In some embodiments, 0.8≤B2≤1.1. In some embodiments, 1.1≤B2≤1.2. In some embodiments, 0.7≤B2≤1.1. In some embodiments, 0.8≤B2≤1.2. In some embodiments, B1 is 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, or a value in a range consisting of any two of these values. In some embodiments, B2 is 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, or a value in a range consisting of any two of these values. By regulating the 1,2-bis(2-cyanoethoxy)ethane and / or 1,3,6-hexanetrinitrile in the electrolyte to meet the above ranges, the high-temperature intermittent cycle resistance growth rate and the fast-charge cycle resistance growth rate of the secondary battery can be further improved.

[0051] In some embodiments, the electrolyte includes ethylene carbonate and propylene carbonate, and based on the mass of the electrolyte, the mass percentage of ethylene carbonate is X1%, the mass percentage of propylene carbonate is X2%, and 29≤X1+X2≤51. In some embodiments, 34≤X1+X2≤51. In some embodiments, 29≤X1+X2≤46. In some embodiments, 34≤X1+X2≤46. In some embodiments, 29≤X1+X2≤34. In some embodiments, 46≤X1+X2≤51. In some embodiments, the value of X1+X2 is 29, 30, 32, 33, 35, 36, 38, 39, 41, 43, 45, 47, 49, 50, 51 or a value within the range composed of any two of these values. The present application regulates the sum of the mass contents of ethylene carbonate and propylene carbonate in the electrolyte within the above range, which can improve the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery.

[0052] In some embodiments, 1.1≤X2 / X1≤2.5. In some embodiments, 1.6≤X2 / X1≤2.5. In some embodiments, 1.1≤X2 / X1≤2.2. In some embodiments, 1.6≤X2 / X1≤2.2. In some embodiments, 1.1≤X2 / X1≤1.6. In some embodiments, 2.2≤X2 / X1≤2.5. In some embodiments, the value of X2 / X1 is 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5 or a value within the range of any two of these values. By regulating the mass content of ethylene carbonate and propylene carbonate in the electrolyte to satisfy the above relationship, the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery can be further improved.

[0053] In some embodiments, the electrolyte includes ethyl propionate and propyl propionate, and based on the mass of the electrolyte, the mass percentage of ethyl propionate is Y1%, the mass percentage of propyl propionate is Y2%, and 35≤Y1+Y2≤62. In some embodiments, 41≤Y1+Y2≤62. In some embodiments, 35≤Y1+Y2≤55. In some embodiments, 41≤Y1+Y2≤55. In some embodiments, 35≤Y1+Y2≤41. In some embodiments, 55≤Y1+Y2≤62. In some embodiments, the value of Y1+Y2 is 35, 36, 39, 40, 41, 43, 44, 47, 48, 50, 52, 55, 56, 59, 61, 62 or a value within the range of any two of these values. The present application regulates the sum of the mass contents of ethyl propionate and propyl propionate in the electrolyte within the above range, which can improve the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery.

[0054] In some embodiments, 1.2≤Y2 / Y1≤2.9. In some embodiments, 1.2≤Y2 / Y1≤2.5. In some embodiments, 1.5≤Y2 / Y1≤2.9. In some embodiments, 1.5≤Y2 / Y1≤2.5. In some embodiments, 1.2≤Y2 / Y1≤1.5. In some embodiments, 2.5≤Y2 / Y1≤2.9. In some embodiments, the value of Y2 / Y1 is 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.9, 2.1, 2.2, 2.3, 2.4, 2.5, 2.7, 2.8, 2.9 or a value within the range of any two of these values. By regulating the mass content of ethyl propionate and propyl propionate in the electrolyte to satisfy the above relationship, the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery can be further improved.

[0055] In some embodiments, the electrolyte includes a fluorine-containing compound, the fluorine-containing compound includes at least one of fluorobenzene or fluoroethylene carbonate, and the mass percentage of fluorobenzene is F1%, 0.9≤F1≤4.1 based on the mass of the electrolyte. In some embodiments, 0.9≤F1≤3.4. In some embodiments, 2.7≤F1≤4.1. In some embodiments, 2.7≤F1≤3.4. In some embodiments, 0.9≤F1≤2.7. In some embodiments, 3.4≤F1≤4.1. In some embodiments, F1 is 0.9, 1.0, 1.2, 1.6, 1.8, 1.9, 2.3, 2.6, 2.7, 2.9, 3.0, 3.2, 3.4, 3.6, 3.9, 4.1 or a value within the range of any two of these values. Regulating the mass percentage of fluorobenzene in the electrolyte within the above range can enhance the ability of the generated solid electrolyte interface film to adsorb carbon nanotubes and improve the high temperature intermittent cycle resistance growth rate and fast charge cycle resistance growth rate of the secondary battery.

[0056] In some embodiments, based on the mass of the electrolyte, the mass percentage of fluoroethylene carbonate is F2%, 10.5≤F2≤19.5. In some embodiments, 12.5≤F2≤19.5. In some embodiments, 10.5≤F2≤17.5. In some embodiments, 12.5≤F2≤17.5. In some embodiments, 10.5≤F2≤12.5. In some embodiments, 12.5≤F2≤17.5. In some embodiments, 17.5≤F2≤19.5. In some embodiments, F2 is 10.5, 10.9, 11.3, 12.5, 13.2, 13.7, 14.1, 14.7, 15.6, 16.6, 16.8, 17.5, 17.8, 18.3, 19.2, 19.5 or a value in the range consisting of any two of these values. By regulating the mass percentage of fluoroethylene carbonate in the electrolyte within the above range, the ability of the generated solid electrolyte interface film to adsorb carbon nanotubes can be enhanced, and the high-temperature intermittent cycle resistance growth rate and fast-charge cycle resistance growth rate of the secondary battery can be improved.

[0057] In some embodiments, the electrolyte includes a compound of formula I, and the mass percentage of the compound of formula I is H%, based on the mass of the electrolyte, 0.2≤H≤0.9. In some embodiments, 0.2≤H≤0.5. In some embodiments, 0.5≤H≤0.9. In some embodiments, H is 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or a value within the range of any two of these values. Adding the compound of formula I to the electrolyte and regulating the mass percentage within the above range can further improve the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0058] In the present application, the chemical formula of the compound of formula I is: .

[0059] In some embodiments, the electrolyte includes a compound of formula II, and the mass percentage of the compound of formula II is G%, based on the mass of the electrolyte, 0.2≤G≤0.7. In some embodiments, 0.2≤G≤0.4. In some embodiments, 0.4≤G≤0.7. In some embodiments, G is 0.2, 0.3, 0.4, 0.5, 0.6, 0.7 or a value within the range of any two of these values. Adding the compound of formula II to the electrolyte and regulating the mass percentage within the above range can further improve the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0060] The chemical formula of the compound of formula II is: .

[0061] The electrolyte may also include a lithium salt and an organic solvent. The present application does not particularly limit the type of lithium salt, as long as the purpose of the present application can be achieved. For example, the lithium salt may include but is not limited to at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium trifluoromethanesulfonyl imide (LiTFSI), lithium bis (fluorosulfonyl) imide (LiFSI), lithium bis oxalate borate (LiBOB) or lithium difluoro oxalate borate (LiDFOB). Based on the mass of the electrolyte, the mass percentage of the lithium salt may be 8% to 15%, for example, the mass percentage of the lithium salt may be 8%, 9%, 10%, 11%, 12.5%, 13%, 15% or a range consisting of any two of the values. The present application does not particularly limit the type of the above-mentioned organic solvent, as long as the purpose of the present application can be achieved, for example, it may include but is not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of chain carbonate compounds or cyclic carbonate compounds. The above-mentioned linear carbonate compound may include but is not limited to at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate or ethyl methyl carbonate. The above-mentioned cyclic carbonate compound may include but is not limited to at least one of ethylene carbonate, propylene carbonate, butylene carbonate or ethylene ethylene carbonate. The above-mentioned carboxylate compound may include but is not limited to at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decalactone, valerolactone or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of ethylene glycol dimethyl ether, dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate.

[0062] positive electrode

[0063] The positive electrode includes a positive electrode current collector and a positive electrode mixture layer disposed on the surface of the positive electrode current collector.

[0064] The positive electrode mixture layer contains positive electrode active material, and the positive electrode mixture layer can be one layer or multiple layers. Each layer of the multiple layers of positive electrode active material can contain the same or different positive electrode active materials. The positive electrode active material is any material that can reversibly embed and de-embed alkali metal ions.

[0065] In some embodiments, the positive electrode active material includes a lithium transition metal oxide containing nickel and other transition metals. In the lithium transition metal oxide including nickel and other transition metals, the amount of nickel relative to the total molar number of the transition metal may be 60 mol% or more, for example, 75 mol% or more, for example, 80 mol% or more, for example, 85 mol% or more, or for example, 90 mol% or more.

[0066] For example, the lithium transition metal oxide may be a compound represented by the following formula α:

[0067] Formula α: Li a Ni x Co y M z O 2-b A b ,

[0068] Wherein, in formula α, 0.9≤a≤1.2, 0≤b≤0.2, 0.6≤x<1, 0<y≤0.3, 0<z≤0.3, and x+y+z=1, M is at least one selected from manganese (Mn), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al) or boron (B), and A is F, S, Cl, Br or a combination thereof. For example, the above subscripts may be 0.7≤x<1, 0<y≤0.3, and 0<z≤0.3; 0.8≤x<1, 0<y≤0.3, and 0<z≤0.3; 0.8≤x<1, 0<y≤0.2, and 0<z≤0.2; 0.83≤x<0.97, 0<y≤0.15, and 0<z≤0.15; or 0.85≤x<0.95, 0<y≤0.1, and 0<z≤0.1.

[0069] For example, the lithium transition metal oxide may be at least one compound represented by the following formula β or formula γ:

[0070] Formula β: LiNi x Co y Mn z O2,

[0071] Wherein, in formula β, 0.6≤x≤0.95, 0<y≤0.2, and 0<z≤0.1, for example, 0.7≤x≤0.95, 0<y≤0.3, and 0<z≤0.3.

[0072] Formula γ: LiNi x Co y Al z O2,

[0073] Wherein, in formula γ, 0.6≤x≤0.95, 0<y≤0.2, and 0<z≤0.1, for example, 0.7≤x≤0.95, 0<y≤0.3, and 0<z≤0.3, for example, 0.8≤x≤0.95, 0<y≤0.3, and 0<z≤0.3, for example, 0.82≤x≤0.95, 0<y≤0.15, and 0<z≤0.15, for example, 0.85≤x≤0.95, 0<y≤0.1, and 0<z≤0.1.

[0074] For example, the lithium transition metal oxide may be LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.88 Co 0.08 Mn 0.04 O2、LiNi 0.8 Co 0.15 Mn 0.05 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.88 Co 0.1 Mn 0.02 O2、LiNi 0.8 Co 0.15 Al 0.05 O2 or LiNi 0.88 Co 0.1 Al 0.02 O2.

[0075] According to another embodiment, the positive electrode active material includes at least one active material selected from the group consisting of Li-Ni-Co-Al (NCA), Li-Ni-Co-Mn (NCM), lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMnO2), lithium nickel oxide (LiNiO2) and lithium iron phosphate (LiFePO4).

[0076] In some embodiments, the positive electrode mixture layer includes a positive electrode conductive material; the type of the positive electrode conductive material is not limited, and any known conductive material can be used. Examples of positive electrode conductive materials may include, but are not limited to, carbon black such as acetylene black and Super-P; amorphous carbon materials such as needle coke; carbon nanotubes; graphene, etc. The above positive electrode conductive materials may be used alone or in any combination.

[0077] There is no particular restriction on the type of positive electrode binder used in the manufacture of the positive electrode mixture layer. In the case of a coating method, any material that can be dissolved or dispersed in the liquid medium used in the manufacture of the electrode can be used. Examples of positive electrode binders may include, but are not limited to, one or more of the following: resin polymers such as polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, and nitrocellulose; rubber polymers such as styrene-butadiene rubber (SBR), nitrile rubber (NBR), fluororubber, isoprene rubber, polybutadiene rubber, and ethylene-propylene rubber; styrene-butadiene-styrene block copolymers or their hydrogenates, ethylene-propylene-diene terpolymers (EPDM), Thermoplastic elastomer polymers such as styrene·ethylene·butadiene·ethylene copolymers, styrene·isoprene·styrene block copolymers or their hydrogenated products; soft resin polymers such as syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene·vinyl acetate copolymers, propylene·α-olefin copolymers; fluorine-based polymers such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene, fluorinated polyvinylidene fluoride, polytetrafluoroethylene·ethylene copolymers; polymer compositions having ion conductivity of alkali metal ions (especially lithium ions), etc. The above positive electrode binders can be used alone or in any combination.

[0078] There is no limitation on the type of solvent used to form the positive electrode slurry, as long as it is a solvent that can dissolve or disperse the positive electrode active material, the conductive material, the positive electrode binder, and the thickener used as needed. Examples of solvents used to form the positive electrode slurry may include any of aqueous solvents and organic solvents. Examples of aqueous media may include, but are not limited to, a mixed medium of alcohol and water or water, etc. Examples of organic media may include, but are not limited to, aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether, propylene oxide, and tetrahydrofuran (THF); amides such as N-methylpyrrolidone (NMP), dimethylformamide, and dimethylacetamide; aprotic polar solvents such as hexamethylphosphoramide and dimethyl sulfoxide, etc.

[0079] Thickeners are generally used to adjust the viscosity of the slurry. In the case of using an aqueous medium, the thickener and styrene-butadiene rubber (SBR) emulsion can be used for slurrying. The type of thickener is not particularly limited, and examples thereof may include, but are not limited to, carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and salts thereof. The above thickeners may be used alone or in any combination.

[0080] The type of positive electrode current collector is not particularly limited, and it can be any material known to be suitable for use as a positive electrode current collector. Examples of positive electrode current collectors may include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, tantalum, and materials such as carbon cloth and carbon paper. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum.

[0081] In order to reduce the electronic contact resistance between the positive electrode current collector and the positive electrode mixture layer, the surface of the positive electrode current collector may include a conductive additive or a conductive coating. Examples of conductive additives may include, but are not limited to, carbon and precious metals such as gold, platinum, and silver. Examples of conductive coatings may include a mixture layer containing an inorganic oxide, a conductive agent, and a binder.

[0082] The positive electrode can be made by forming a positive electrode mixture layer containing a positive electrode active material and a binder on a current collector. The manufacture of a positive electrode using a positive electrode active material can be carried out by a conventional method, that is, the positive electrode active material and the binder, as well as a conductive material and a thickener as required, are dry-mixed to form a sheet, and the obtained sheet is pressed onto the positive electrode current collector; or these materials are dissolved or dispersed in a liquid medium to form a slurry, and the slurry is applied to the positive electrode current collector and dried to form a positive electrode mixture layer on the current collector, thereby obtaining a positive electrode.

[0083] Isolation film

[0084] In order to prevent short circuit, a separator is usually provided between the positive electrode and the negative electrode. In this case, the electrolyte of the present application is usually used by infiltrating the separator.

[0085] There is no particular restriction on the material and shape of the isolation membrane, as long as the effect of the present application is not significantly impaired. The isolation membrane may be a resin, glass fiber, inorganic substance, etc. formed of a material that is stable to the electrolyte of the present application. In some embodiments, the isolation membrane includes a porous sheet or a non-woven fabric-like material with excellent liquid retention. Examples of materials for resin or glass fiber isolation membranes may include, but are not limited to, polyolefins, aromatic polyamides, polytetrafluoroethylene, polyether sulfone, etc. In some embodiments, the polyolefin is polyethylene or polypropylene. In some embodiments, the polyolefin is polypropylene. The materials of the above isolation membranes may be used alone or in any combination.

[0086] The separator may also be a material formed by laminating the above materials, examples of which include, but are not limited to, a three-layer separator formed by laminating polypropylene, polyethylene, and polypropylene in this order.

[0087] Examples of inorganic materials may include, but are not limited to, oxides such as aluminum oxide and silicon dioxide, nitrides such as aluminum nitride and silicon nitride, and sulfates (eg, barium sulfate, calcium sulfate, etc.). The form of the inorganic material may include, but is not limited to, granular or fibrous.

[0088] The separator may be in the form of a thin film, examples of which include, but are not limited to, nonwoven fabrics, woven fabrics, microporous films, etc. In the thin film form, the separator has a pore size of 0.01 μm to 1 μm and a thickness of 5 μm to 50 μm. In addition to the above-mentioned independent thin film separators, the following separators can also be used: a separator formed by forming a composite porous layer containing the above-mentioned inorganic particles on the surface of the positive electrode and / or the negative electrode using a resin-based adhesive, for example, a separator formed by using a fluororesin as an adhesive to form a porous layer on both sides of the positive electrode with alumina particles having a particle size of 90% less than 1 μm.

[0089] The thickness of the separator is arbitrary. In some embodiments, the thickness of the separator is greater than 1 μm, greater than 5 μm, or greater than 8 μm. In some embodiments, the thickness of the separator is less than 50 μm, less than 40 μm, or less than 30 μm. When the thickness of the separator is within the above range, insulation and mechanical strength can be ensured, and the rate characteristics and energy density of the secondary battery can be ensured.

[0090] The present application further provides an electronic device, which includes the secondary battery according to the present application.

[0091] The purpose of the secondary battery of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the secondary battery of the present application can be used for, but not limited to, laptop computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries and lithium-ion capacitors, etc.

[0092] Example

[0093] Below, taking lithium-ion batteries as an example, examples and comparative examples are given to explain the implementation of the secondary battery of the present application in more detail. Those skilled in the art will understand that the preparation method described in this application is only an example, and any other suitable preparation method is within the scope of this application. Various tests and evaluations are carried out according to the following methods. In addition, unless otherwise specified, "parts" and "%" are mass references.

[0094] Test Method

[0095] Resistance growth rate after high temperature (65℃) intermittent cycling

[0096] (1) Test initial resistance: After moving the lithium-ion battery to a charge and discharge device at room temperature (25°C), perform constant current charging at 0.33C to 4.45V, then charge at 4.45V at constant voltage to 0.05C cut-off charging, and discharge at 0.33C to 3.0V. Then, after charging and discharging three times, the battery is set to SOC 50% based on the last discharge capacity. Then, the DC internal resistance is measured by the voltage drop displayed when a discharge pulse is applied at 5A (2.5C) for 10 seconds (PNE-0506 charge and discharge device), and the resistance at this time is defined as the initial resistance.

[0097] (2) High-temperature intermittent cycle: After the lithium-ion battery with the initial resistance measured was moved to a high temperature (65°C), it was charged to 4.25V at a constant current of 0.5C, and then charged to 0.05C at a constant voltage at 4.25V. The battery thickness was recorded and recorded as the initial cycle thickness. After that, it was kept for 24 hours and then discharged to 3.0V at a constant current of 0.5C. The above charging and discharging process was set as one high-temperature intermittent cycle, and a total of 80 high-temperature intermittent cycles of charging and discharging were performed.

[0098] (3) Resistance after high-temperature intermittent cycling: After the lithium-ion battery is placed in a charge-discharge device at room temperature, the SOC is set to 50%. Then, the resistance after 80 cycles is measured by the voltage drop displayed when a discharge pulse is applied at 5A (2.5C) for 10 seconds using a PNE-0506 charge-discharge device.

[0099] (4) Calculate the resistance increase rate R1 after high temperature (65°C) intermittent cycling:

[0100] The resistance increase rate after high temperature (65°C) intermittent cycling R1 (%) = {(resistance after 80 cycles - initial resistance) / initial resistance}×100.

[0101] Fast charge (6C) cycle resistance growth rate

[0102] (1) Test initial resistance: After moving the lithium-ion battery to a charge and discharge device at room temperature (25°C), a constant current of 0.33C was applied to 4.45V, then a constant voltage of 4.45V was charged to 0.05C cut-off charge, and then a discharge of 0.33C was applied to 3.0V. After charging and discharging three times, the battery was set to SOC 50% based on the last discharge capacity. The DC internal resistance was then measured by the voltage drop displayed when a discharge pulse of 5A (2.5C) was applied for 10 seconds (PNE-0506 charge and discharge device), and the resistance at this time was defined as the initial resistance.

[0103] (2) Fast charge cycle: The lithium-ion battery was charged at a constant current of 6C (nominal capacity) to a voltage of 4.25V, then charged at a constant voltage of 4.25V to a current of 0.05C. After standing for 10 min, it was discharged at a constant current of 1C to a cut-off voltage of 2.8V. The above charging and discharging process was set as 1 cycle, and a total of 80 cycles of charging and discharging were performed.

[0104] (3) Resistance after fast charge cycle: The SOC was set to 50%. Then, the resistance after 80 cycles was measured by the voltage drop displayed when a discharge pulse was applied at 5A (2.5C) for 10 seconds using a PNE-0506 charge-discharge device.

[0105] (4) Calculate the fast charge (6C) cycle resistance increase rate R2:

[0106] Fast charge (6C) cycle resistance increase rate R2 (%) = {(resistance after 80 cycles - initial resistance) / initial resistance} × 100.

[0107] Energy density ED

[0108] The lithium ion batteries of each embodiment and comparative example were placed in a constant temperature box at 25°C ± 1°C for 30 minutes, charged to 4.45V at a constant current of 0.5C, then charged to 0.025C at a constant voltage of 4.45V, placed for 5 minutes, and then discharged to 3.0V at 0.5C. The discharge energy E mAh of the lithium ion battery was recorded, and the length, width and height of the battery at a 50% charge state (the lithium ion battery was charged to 3.95V at a constant current of 0.5C) were measured to obtain the volume V cm of the battery. 3 , energy density ED=E / V.

[0109] The average particle size of silica-based particles is D μm

[0110] The negative electrode sheet was cut into a size of 1 cm×1 cm, and then the cut surface of the negative electrode sheet was polished using argon plasma polishing (CP) technology to prepare a CP sample.

[0111] The CP sample was observed by scanning electron microscopy, and the silicon-based particles in the CP sample were selected. The cross-sectional area of ​​the silicon-based particles was counted and recorded as S, and R was calculated according to the formula S=πR². The particle size of the silicon-based particles is 2R.

[0112] A total of 20 silicon-based particles were randomly selected, and the arithmetic mean of the particle sizes of the 20 silicon-based particles was calculated, which was recorded as the average particle size D μm of the silicon-based particles.

[0113] The thickness of the negative electrode mixture layer is T μm

[0114] The negative electrode sheet was cut into a size of 1 cm×1 cm, and then the cut surface of the negative electrode sheet was polished using argon plasma polishing (CP) technology to prepare a CP sample.

[0115] The CP sample is observed by scanning electron microscopy, the thickness of the negative electrode mixture layer disposed on the two surfaces of the current collector is measured respectively, and the arithmetic average of the two thicknesses is calculated to obtain the thickness T μm of the negative electrode mixture layer.

[0116] Example 1-1

[0117] <Preparation of negative electrode>

[0118] Preparation of negative electrode sheet:

[0119] Silicon-based particles and artificial graphite are mixed evenly in a mass ratio of 12:88 as negative electrode active materials. The above-mentioned negative electrode active materials, styrene-butadiene rubber (SBR), polyacrylic acid (PAA), carbon nanotubes, and carboxymethyl cellulose are mixed in a mass ratio of 95.8:2.4:0.5:0.5:0.8, and then deionized water is added and stirred evenly to prepare a negative electrode slurry with a solid content of 45wt%. The negative electrode slurry is evenly coated on one surface of a copper foil with a thickness of 6μm, and a negative electrode sheet coated with a negative electrode mixture layer on one side is obtained after drying. Repeat the above steps on the other surface of the copper foil to obtain a negative electrode sheet coated with a negative electrode mixture layer on both sides. After cold pressing, cutting, slitting, and drying, a negative electrode sheet with a specification of 76.6mm×875mm is obtained.

[0120] <Preparation of positive electrode>

[0121] Lithium cobalt oxide, conductive carbon black, and polyvinylidene fluoride are mixed in a mass ratio of 95:2:3, and N-methylpyrrolidone is added and stirred evenly to obtain a positive electrode slurry with a solid content of 70wt%. The positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 9μm, and a positive electrode sheet coated with a positive electrode mixture layer on one side is obtained after drying. Repeat the above steps on the other surface of the aluminum foil to obtain a positive electrode sheet coated with a positive electrode mixture layer on both sides. After drying, it is cold pressed, cut, and slit, and then dried to obtain a positive electrode sheet with a specification of 74mm×867mm.

[0122] <Preparation of Electrolyte>

[0123] In a dry argon atmosphere glove box, lithium hexafluorophosphate (LiPF6) was dissolved in a mixed solution containing diethyl carbonate (DEC), ethylene carbonate (EC), propylene carbonate (PC), ethyl propionate (EP), propyl propionate (PP), dinitrile compounds, trinitrile compounds and fluoroethylene carbonate (FEC). Based on the mass of the electrolyte, the content of LiPF6 was 12%, the contents of other substances were shown in Table 1, and the balance was DEC.

[0124] The dinitrile compounds are succinonitrile and adiponitrile, and based on the mass of the electrolyte, the content ratio of succinonitrile to adiponitrile is 11:10.

[0125] The trinitrile compound is 1,3,6-hexanetrinitrile.

[0126] <Diaphragm>

[0127] A porous polyethylene film with a thickness of 15 μm (provided by Celgard Company) was used as a separator.

[0128] <Preparation of lithium-ion batteries>

[0129] The positive electrode and negative electrode prepared as above are connected to the pole ears respectively. They are stacked via a separator to obtain a laminate. Then, the laminate is housed in an aluminum laminate housing together with an electrolyte. The opening of the housing is heat-sealed, and a lithium-ion battery is manufactured through steps such as formation and capacity.

[0130] Except for adjusting the parameters shown in Table 1 and the types of the following dinitrile compounds and trinitrile compounds, the other embodiments and comparative examples in Table 1 are the same as Example 1-1.

[0131] Example 1-19 to Example 1-26

[0132] The dinitrile compound is succinonitrile and 1,2-bis(2-cyanoethoxy)ethane, and the content ratio of succinonitrile to 1,2-bis(2-cyanoethoxy)ethane is 11:10 based on the mass of the electrolyte.

[0133] Example 1-27 and Example 1-35

[0134] The dinitrile compound is adiponitrile and 1,2-bis(2-cyanoethoxy)ethane, and the content ratio of adiponitrile to 1,2-bis(2-cyanoethoxy)ethane is 11:10 based on the mass of the electrolyte.

[0135] Example 1-36 and Example 1-52

[0136] The trinitrile compound is 1,3,6-hexanetrinitrile and 4-(2-cyanoethyl)heptane dinitrile, and the content ratio of 1,3,6-hexanetrinitrile to 4-(2-cyanoethyl)heptane dinitrile is 11:10 based on the mass of the electrolyte.

[0137] Example 1-53 and Example 1-70

[0138] The dinitrile compounds are adiponitrile and 1,2-bis(2-cyanoethoxy)ethane, and the content ratio of adiponitrile to 1,2-bis(2-cyanoethoxy)ethane is 11:10 based on the mass of the electrolyte. The trinitrile compounds are 1,3,6-hexanetrinitrile and 4-(2-cyanoethyl)heptanedinitrile, and the content ratio of 1,3,6-hexanetrinitrile to 4-(2-cyanoethyl)heptanedinitrile is 11:10 based on the mass of the electrolyte.

[0139] Table 1

[0140] T(μm) D(μm) <![CDATA[10T / D 2 ]]> <![CDATA[Dinitrile N1(%)]]> <![CDATA[Trinitrile N2(%)]]> <![CDATA[N1 / N2]]> <![CDATA[ECX1(%)]]> <![CDATA[PCX2(%)]]> <![CDATA[X1+X2]]> <![CDATA[X2 / X1]]> <![CDATA[EPY1(%)]]> <![CDATA[PPY2(%)]]> <![CDATA[Y1+Y2]]> <![CDATA[Y2 / Y1]]> <![CDATA[Fluorobenzene F1 (%)]]> <![CDATA[FECF2(%)]]> <![CDATA[R1(%)]]> <![CDATA[R2(%)]]> <![CDATA[ED(mAh / cm 3 )]]> Comparative Example 1 53.3 13.4 3.0 3.0 1.5 2.0 13 13 26 1.0 16 16 32 1.0 \ 5.0 25.6 30.7 721 Comparative Example 2 135.6 7.2 26.2 3.0 1.5 2.0 13 13 26 1.0 16 16 32 1.0 \ 5.0 26.2 30.5 721 Comparative Example 3 87.4 9.6 9.5 3.0 \ \ 13 13 26 1.0 16 16 32 1.0 \ 5.0 25.9 32.4 721 Comparative Example 4 87.4 9.6 9.5 \ 1.5 \ 13 13 26 1.0 16 16 32 1.0 \ 5.0 26.8 31.8 721 Comparative Example 5 87.4 \ / 3.0 1.5 2.0 13 13 26 1.0 16 16 32 1.0 \ 5.0 21.3 26.8 645 Example 1-1 87.4 9.6 9.5 3.0 1.5 2.0 13 13 26 1.0 16 16 32 1.0 \ 5.0 17.9 23.4 721 Example 1-2 60.2 12.7 3.7 3.0 1.5 2.0 13 13 26 1.0 16 16 32 1.0 \ 5.0 20.1 25.1 721 Examples 1-3 78.2 10.9 6.6 3.0 1.5 2.0 13 13 26 1.0 16 16 32 1.0 \ 5.0 18.4 24.6 721 Examples 1-4 80.1 10.7 7.0 3.0 1.5 2.0 13 13 26 1.0 16 16 32 1.0 \ 5.0 17.5 24.1 721 Examples 1-5 82.9 10.6 7.4 3.0 1.5 2.0 13 13 26 1.0 16 16 32 1.0 \ 5.0 17.0 22.5 721 Examples 1-6 98.7 9.2 11.7 3.0 1.5 2.0 13 13 26 1.0 16 16 32 1.0 \ 5.0 16.9 22.8 721 Examples 1-7 112.9 7.9 18.1 3.0 1.5 2.0 13 13 26 1.0 16 16 32 1.0 \ 5.0 16.7 23.0 721 Examples 1-8 108.3 7.6 18.8 3.0 1.5 2.0 13 13 26 1.0 16 16 32 1.0 \ 5.0 17.6 23.8 721 Examples 1-9 121.8 7.0 24.9 3.0 1.5 2.0 13 13 26 1.0 16 16 32 1.0 \ 5.0 19.2 25.3 721 Examples 1-10 89.4 9.4 10.1 2.8 3.5 0.8 15 15 30 1.0 19 19 38 1.0 \ 5.0 16.4 22.1 744 Examples 1-11 89.4 9.4 10.1 3.2 2.9 1.1 15 15 30 1.0 19 19 38 1.0 \ 5.0 15.1 20.4 744 Examples 1-12 89.4 9.4 10.1 4.2 2.5 1.7 15 15 30 1.0 19 19 38 1.0 \ 5.0 14.1 18.2 744 Examples 1-13 89.9 9.4 10.2 4.9 2.2 2.2 15 15 30 1.0 19 19 38 1.0 \ 5.0 12.9 17.3 744 Examples 1-14 89.9 9.4 10.2 5.2 1.8 2.9 15 15 30 1.0 19 19 38 1.0 \ 5.0 13.1 17.1 744 Examples 1-15 89.9 9.4 10.2 5.6 1.7 3.3 15 15 30 1.0 19 19 38 1.0 \ 5.0 13.3 16.9 744 Examples 1-16 89.4 9.4 10.1 5.9 1.6 3.7 15 15 30 1.0 19 19 38 1.0 \ 5.0 13.3 17.0 744 Examples 1-17 89.4 9.4 10.1 6.8 1.4 4.9 15 15 30 1.0 19 19 38 1.0 \ 5.0 15.5 20.7 744 Examples 1-18 89.4 9.4 10.1 7.1 1.1 6.5 15 15 30 1.0 19 19 38 1.0 \ 5.0 16.3 22.3 744 Examples 1-19 92.6 8.6 12.5 4.8 2.1 2.3 13 12 25 0.9 9 12 21 1.3 \ 5.0 13.6 18.4 721 Examples 1-20 92.6 8.6 12.5 4.8 2.1 2.3 15 14 29 0.9 9 12 21 1.3 \ 5.0 12.4 17.9 721 Embodiment 1-21 92.6 8.6 12.5 4.8 2.1 2.3 14 20 34 1.4 9 12 21 1.3 \ 5.0 11.0 13.9 721 Examples 1-22 92.6 8.6 12.5 4.8 2.1 2.3 20 19 39 1.0 9 12 21 1.3 \ 5.0 12.1 15.1 721 Examples 1-23 92.6 8.6 12.5 4.8 2.1 2.3 20 26 46 1.3 9 12 21 1.3 \ 5.0 11.3 14.4 721 Examples 1-24 92.6 8.6 12.5 4.8 2.1 2.3 25 26 51 1.0 9 12 21 1.3 \ 5.0 13.0 17.4 721 Examples 1-25 92.6 8.6 12.5 4.8 2.1 2.3 27 27 54 1.0 9 12 21 1.3 \ 5.0 14.3 18.5 721 Examples 1-26 89.4 9.4 10.1 2.8 3.5 0.8 19 21 40 1.1 9 12 21 1.3 \ 5.0 15.6 21.9 744 Examples 1-27 94.7 8.2 14.1 5.4 2.0 2.7 20 20 40 1.0 9 12 21 1.3 \ 5.0 12.0 15.5 729 Examples 1-28 94.7 8.2 14.1 5.4 2.0 2.7 19 21 40 1.1 9 12 21 1.3 \ 5.0 10.8 14.8 729 Examples 1-29 94.7 8.2 14.1 5.4 2.0 2.7 15 25 40 1.7 9 12 21 1.3 \ 5.0 10.5 13.4 729 Examples 1-30 94.7 8.2 14.1 5.4 2.0 2.7 12 26 38 2.2 9 12 21 1.3 \ 5.0 10.3 13.7 729 Example 1-31 94.7 8.2 14.1 5.4 2.0 2.7 11 27 38 2.5 9 12 21 1.3 \ 5.0 11.0 14.6 729 Example 1-32 94.7 8.2 14.1 5.4 2.0 2.7 10 28 38 2.8 9 12 21 1.3 \ 5.0 11.8 16.4 729 Examples 1-33 94.7 8.2 14.1 5.4 2.0 2.7 17 32 49 1.9 9 12 21 1.3 \ 5.0 10.9 14.4 729 Examples 1-34 94.7 8.2 14.1 5.4 2.0 2.7 24 25 49 1.0 9 12 21 1.3 \ 5.0 11.3 14.5 729 Embodiment 1-35 89.4 9.4 10.1 2.8 3.5 0.8 16 28 44 1.8 9 12 21 1.3 \ 5.0 15.1 20.9 744 Embodiment 1-36 93.4 8.9 11.8 5.8 1.7 3.4 4 6 10 1.5 13 17 30 1.3 \ 5.0 13.1 17.2 721 Embodiment 1-37 93.4 8.9 11.8 5.8 1.7 3.4 4 6 10 1.5 15 20 35 1.3 \ 5.0 11.9 15.7 721 Examples 1-38 93.4 8.9 11.8 5.8 1.7 3.4 4 6 10 1.5 18 23 41 1.3 \ 5.0 11.1 14.7 721 Examples 1-39 93.4 8.9 11.8 5.8 1.7 3.4 4 6 10 1.5 25 30 55 1.2 \ 5.0 10.9 14.9 721 Embodiment 1-40 93.4 8.9 11.8 5.8 1.7 3.4 4 6 10 1.5 28 34 62 1.2 \ 5.0 12.3 15.9 721 Example 1-41 93.4 8.9 11.8 5.8 1.7 3.4 4 6 10 1.5 28 36 64 1.3 \ 5.0 13.4 17.5 721 Example 1-42 89.4 9.4 10.1 2.8 3.5 0.8 4 6 10 1.5 25 30 55 1.2 \ 5.0 15.8 21.4 744 Embodiment 1-43 90.1 8.2 13.4 4.5 1.8 2.5 9 15 24 1.7 25 25 50 1.0 \ 5.0 11.4 14.8 721 Embodiment 1-44 90.1 8.2 13.4 4.5 1.8 2.5 9 15 24 1.7 20 24 44 1.2 \ 5.0 10.7 13.0 721 Embodiment 1-45 90.1 8.2 13.4 4.5 1.8 2.5 9 15 24 1.7 20 30 50 1.5 \ 5.0 10.1 12.1 721 Embodiment 1-46 90.1 8.2 13.4 4.5 1.8 2.5 9 15 24 1.7 13 32 45 2.5 \ 5.0 9.8 12.7 721 Embodiment 1-47 90.1 8.2 13.4 4.5 1.8 2.5 9 15 24 1.7 13 37 50 2.8 \ 5.0 10.5 13.4 721 Examples 1-48 90.1 8.2 13.4 4.5 1.8 2.5 9 15 24 1.7 13 34 47 2.6 \ 5.0 11.3 14.7 721 Examples 1-49 89.4 9.4 10.1 2.8 3.5 0.8 9 15 24 1.7 15 30 45 2.0 \ 5.0 14.6 19.2 744 Embodiment 1-50 89.4 9.4 10.1 2.8 3.5 0.8 17 18 35 1.1 18 22 40 1.2 \ 5.0 15.7 21.4 744 Example 1-51 89.4 9.4 10.1 2.8 3.5 0.8 10 19 29 1.9 15 28 43 1.9 \ 5.0 13.9 18.9 744 Example 1-52 89.4 9.4 10.1 5.2 1.8 2.9 11 21 32 1.9 14 28 42 2.0 \ 5.0 10.0 12.2 744 Embodiment 1-53 89.4 9.4 10.1 4.6 1.8 2.6 11 20 31 1.8 14 27 41 1.9 0.5 5.0 9.4 11.8 744 Embodiment 1-54 89.4 9.4 10.1 4.6 1.8 2.6 11 20 31 1.8 14 27 41 1.9 0.9 5.0 8.8 10.5 744 Embodiment 1-55 89.4 9.4 10.1 4.6 1.8 2.6 11 20 31 1.8 14 27 41 1.9 2.7 5.0 8.2 10.1 744 Example 1-56 89.4 9.4 10.1 4.6 1.8 2.6 11 20 31 1.8 14 27 41 1.9 3.4 5.0 8.4 9.9 744 Example 1-57 89.4 9.4 10.1 4.6 1.8 2.6 11 20 31 1.8 14 27 41 1.9 4.1 5.0 8.7 11.0 744 Embodiment 1-58 89.4 9.4 10.1 4.6 1.8 2.6 11 20 31 1.8 14 27 41 1.9 4.5 5.0 9.1 11.9 744 Embodiment 1-59 89.4 9.4 10.1 2.8 3.5 0.8 10 15 25 1.5 13 32 45 2.5 2.9 5.0 13.5 19.0 744 Example 1-60 89.4 9.4 10.1 2.8 3.5 0.8 11 20 31 1.8 18 20 38 1.1 3.1 5.0 14.9 21.1 744 Example 1-61 89.4 9.4 10.1 5.4 2.0 2.7 15 25 40 1.7 9 12 21 1.3 3.0 5.0 9.7 11.3 729 Example 1-62 93.2 8.9 11.8 4.7 1.8 2.6 8 13 21 1.6 16 19 35 1.2 2.7 8.5 9.8 12.0 744 Example 1-63 93.2 8.9 11.8 4.7 1.8 2.6 8 13 21 1.6 16 19 35 1.2 2.7 10.5 9.5 11.1 744 Embodiment 1-64 93.2 8.9 11.8 4.7 1.8 2.6 8 13 21 1.6 16 19 35 1.2 2.7 12.5 8.9 10.7 744 Example 1-65 93.2 8.9 11.8 4.7 1.8 2.6 8 13 21 1.6 16 19 35 1.2 2.7 17.5 9.0 10.6 744 Example 1-66 93.2 8.9 11.8 4.7 1.8 2.6 8 13 21 1.6 16 19 35 1.2 2.7 19.5 9.6 11.4 744 Example 1-67 93.2 8.9 11.8 4.7 1.8 2.6 8 13 21 1.6 16 19 35 1.2 2.7 22.5 10.1 12.4 744 Example 1-68 89.4 9.4 10.1 2.8 3.5 0.8 10 15 25 1.5 11 25 36 2.3 2.9 14.5 13.1 17.7 744 Embodiment 1-69 89.4 9.4 10.1 2.8 3.5 0.8 5 10 15 2.0 20 23 43 1.2 3.1 15.5 12.1 15.3 744 Example 1-70 89.4 9.4 10.1 2.8 3.5 0.8 11 23 34 2.1 8 16 24 2.0 3.3 14.5 11.1 14.8 744

[0141] In Table 1, T (μm) is the thickness of the negative electrode mixture layer, and D (μm) is the average particle size of the silicon-based particles. Based on the mass of the electrolyte, N1 (%) is the mass percentage of the dinitrile compound, N2 (%) is the mass percentage of the trinitrile compound, X1 (%) is the mass percentage of EC, X2 (%) is the mass percentage of PC, Y1 (%) is the mass percentage of EP, Y2 (%) is the mass percentage of PP, F1 (%) is the mass percentage of fluorobenzene, and F2 (%) is the mass percentage of FEC.

[0142] As shown in Table 1, the present invention regulates the thickness of the negative electrode mixture layer T μm and the average particle size D μm of the silicon-based particles to satisfy 3.7≤10T / D 2 ≤24.9, combined with dinitrile compounds and trinitrile compounds in the electrolyte, it is possible to achieve a higher energy density while improving the high-temperature intermittent cycle resistance growth rate and the fast-charge cycle resistance growth rate. In particular, regulating T and D to meet 7.0≤10T / D 2 When ≤18.1, the high temperature intermittent cycle resistance growth rate and fast charge cycle resistance growth rate of the lithium-ion battery can be further improved.

[0143] In particular, when the mass percentage of dinitrile compounds and trinitrile compounds in the electrolyte is controlled to meet 1.1≤N1 / N2≤4.9, it can better cooperate with the negative electrode system of the present application to further improve the high temperature intermittent cycle resistance growth rate and fast charge cycle resistance growth rate of the lithium ion battery. In particular, under the condition of 2.2≤N1 / N2≤3.7, the high temperature intermittent cycle resistance growth rate and fast charge cycle resistance growth rate of the lithium ion battery can be significantly improved.

[0144] In particular, by adjusting the mass percentage of ethylene carbonate and propylene carbonate in the electrolyte to meet 29≤X1+X2≤51 and / or 1.1≤X2 / X1≤2.5, the high-temperature intermittent cycle resistance growth rate and the fast-charge cycle resistance growth rate of the secondary battery can be improved. Furthermore, when the mass percentage of the two is adjusted to meet 34≤X1+X2≤46 and / or 1.6≤X2 / X1≤2.2, the lithium-ion battery can have a lower high-temperature intermittent cycle resistance growth rate and fast-charge cycle resistance growth rate.

[0145] In particular, controlling the mass percentage of ethyl propionate and propyl propionate in the electrolyte to meet at least one of 35≤Y1+Y2≤62 or 1.2≤Y2 / Y1≤2.9 can improve the high temperature intermittent cycle resistance growth rate and fast charge cycle resistance growth rate of the lithium ion battery. In particular, when at least one of 41≤Y1+Y2≤55 or 1.5≤Y2 / Y1≤2.5 is met, the high temperature intermittent cycle resistance growth rate and fast charge cycle resistance growth rate of the lithium ion battery can be further improved.

[0146] In particular, when fluorinated compounds such as fluorobenzene and / or fluoroethylene carbonate are added to the electrolyte, especially when the mass percentage of fluorobenzene and fluoroethylene carbonate in the electrolyte is controlled to meet 0.9≤F1≤4.1 and / or 10.5≤F2≤19.5, respectively, the ability of the generated solid electrolyte interface film to adsorb carbon nanotubes can be enhanced, and the high-temperature intermittent cycle resistance growth rate and fast-charge cycle resistance growth rate of the lithium-ion battery can be improved. Among them, further regulating the mass percentage of fluorobenzene and fluoroethylene carbonate in the electrolyte to meet 2.7≤F1≤3.4 and / or 12.5≤F2≤17.5, respectively, can significantly improve the high-temperature intermittent cycle resistance growth rate and fast-charge cycle resistance growth rate of the lithium-ion battery.

[0147] Except for <Preparation of electrolyte>, all other examples in Table 2 are the same as Example 1-1.

[0148] The preparation of the electrolyte in each example in Table 2 is:

[0149] In a dry argon atmosphere glove box, lithium hexafluorophosphate (LiPF6) was dissolved in a mixed solution containing ethylene carbonate, propylene carbonate, ethyl propionate, propyl propionate, dinitrile compounds, trinitrile compounds and fluoroethylene carbonate. Based on the mass of the electrolyte, the content of LiPF6 was 12%, and the contents of other substances were shown in Table 2, with the remainder being ethylene carbonate, propylene carbonate, ethyl propionate and propyl propionate. Based on the mass of the electrolyte, the ratio of the contents of ethylene carbonate, propylene carbonate, ethyl propionate and propyl propionate was 1:2:1:2.

[0150] Table 2

[0151] <![CDATA[A1(%)]]> <![CDATA[A2(%)]]> <![CDATA[A1 / A2]]> <![CDATA[B1(%)]]> <![CDATA[B2(%)]]> <![CDATA[B1 / B2]]> <![CDATA[F1(%)]]> <![CDATA[F2(%)]]> H(%) G(%) <![CDATA[R1(%)]]> <![CDATA[R2(%)]]> Example 2-1 3.5 1.0 3.50 1.0 1.4 0.71 3.0 15.0 \ \ 7.8 9.5 Example 2-2 3.5 1.0 3.50 1.5 1.0 1.50 3.0 15.0 \ \ 7.3 8.5 Example 2-3 3.7 1.1 3.36 1.5 1.0 1.50 3.0 15.0 \ \ 5.4 7.7 Embodiment 2-4 3.2 1.1 2.91 1.5 1.0 1.50 3.0 15.0 \ \ 4.8 6.4 Embodiment 2-5 3.5 1.9 1.84 1.5 1.0 1.50 3.0 15.0 \ \ 4.9 6.6 Embodiment 2-6 2.8 2.2 1.27 1.5 1.0 1.50 3.0 15.0 \ \ 5.6 7.2 Embodiment 2-7 2.2 2.0 1.10 1.5 1.0 1.50 3.0 15.0 \ \ 6.8 8.2 Embodiment 2-8 3.4 1.7 2.00 1.8 0.7 2.57 3.0 15.0 \ \ 7.4 8.5 Embodiment 2-9 3.4 1.7 2.00 1.7 0.7 2.43 3.0 15.0 \ \ 6.0 7.3 Embodiment 2-10 3.4 1.7 2.00 1.6 0.8 2.00 3.0 15.0 \ \ 5.0 6.7 Example 2-11 3.4 1.7 2.00 1.5 1.1 1.36 3.0 15.0 \ \ 5.2 6.1 Example 2-12 3.4 1.7 2.00 1.0 1.2 0.83 3.0 15.0 \ \ 6.2 7.5 Example 2-13 3.4 1.7 2.00 0.9 1.4 0.64 3.0 15.0 \ \ 7.3 8.4 Example 2-14 3.2 1.1 2.91 1.5 1.0 1.50 3.0 5.0 \ \ 6.8 8.7 Example 2-15 3.4 1.7 2.00 1.5 1.1 1.36 0.5 15.0 \ \ 6.7 9.3 Example 2-16 3.5 1.9 1.84 1.5 1.0 1.50 3.0 5.0 \ \ 7.4 8.6 Example 2-17 3.5 1.9 1.84 1.5 1.0 1.50 3.0 5.0 0.1 \ 6.9 8.8 Example 2-18 3.5 1.9 1.84 1.5 1.0 1.50 3.0 5.0 0.2 \ 6.3 7.4 Example 2-19 3.5 1.9 1.84 1.5 1.0 1.50 3.0 15.0 0.5 \ 4.5 5.0 Embodiment 2-20 3.5 1.9 1.84 1.5 1.0 1.50 3.0 5.0 0.9 \ 5.8 7.3 Example 2-21 3.5 1.9 1.84 1.5 1.0 1.50 3.0 5.0 1.0 \ 7.3 9.0 Example 2-22 3.5 1.9 1.84 1.5 1.0 1.50 3.0 5.0 \ 0.1 7.4 9.1 Example 2-23 3.5 1.9 1.84 1.5 1.0 1.50 3.0 5.0 \ 0.2 6.2 7.7 Example 2-24 3.5 1.9 1.84 1.5 1.0 1.50 3.0 15.0 \ 0.4 4.4 5.3 Example 2-25 3.5 1.9 1.84 1.5 1.0 1.50 3.0 5.0 \ 0.7 6.3 7.6 Example 2-26 3.5 1.9 1.84 1.5 1.0 1.50 3.0 5.0 \ 0.9 7.6 8.9

[0152] In Table 2, based on the mass of the electrolyte, A1 (%) is the mass percentage of succinonitrile, A2 (%) is the mass percentage of adiponitrile, B1 (%) is the mass percentage of 1,2-bis (2-cyanoethoxy) ethane, B2 (%) is the mass percentage of 1,3,6-hexanetrinitrile, F1 (%) is the mass percentage of fluorobenzene, F2 (%) is the mass percentage of fluoroethylene carbonate, H (%) is the mass percentage of the compound of formula I, and G (%) is the mass percentage of the compound of formula II.

[0153] As can be seen from Table 2, the present application controls the electrolyte to include succinonitrile and adiponitrile, and adjusts the mass percentage of succinonitrile and adiponitrile to meet 1.27≤A1 / A2≤3.36, which can improve the high temperature intermittent cycle resistance growth rate and fast charge cycle resistance growth rate of the lithium ion battery. In particular, when 1.84≤A1 / A2≤2.91 is met, the high temperature intermittent cycle resistance growth rate and fast charge cycle resistance growth rate of the lithium ion battery can be significantly improved.

[0154] In particular, the electrolyte of the present application includes 1,2-bis(2-cyanoethoxy)ethane and 1,3,6-hexane trinitrile, and the mass percentage of 1,2-bis(2-cyanoethoxy)ethane and 1,3,6-hexane trinitrile is adjusted to meet 0.83≤B1 / B2≤2.43, which can improve the high temperature intermittent cycle resistance growth rate and fast charge cycle resistance growth rate of the secondary battery. When the relationship between the two is preferably 1.36≤B1 / B2≤2.00, the high temperature intermittent cycle resistance growth rate and fast charge cycle resistance growth rate of the lithium ion battery can be further reduced.

[0155] In particular, when the compound of formula I is added to the electrolyte and its mass percentage in the electrolyte is adjusted to meet 0.2≤H≤0.9, the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate can be further improved. On the other hand, controlling the addition of the compound of formula II to the electrolyte and adjusting the mass percentage in the electrolyte to meet 0.2≤G≤0.7 can significantly improve the high temperature intermittent cycle resistance growth rate and the fast charge cycle resistance growth rate of the lithium ion battery.

[0156] Although illustrative embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the principles and scope of the present application.

Claims

1. A secondary battery comprising a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode comprises a negative electrode current collector and a negative electrode mixture layer disposed on at least one surface of the negative electrode current collector, characterized in that: The thickness of the negative electrode mixture layer is Tμm; the negative electrode mixture layer contains carbon nanotubes and silicon-based particles, the average particle size of the silicon-based particles is Dμm, 3.7≤10T / D 2 ≤24.9;60≤T≤122; The electrolyte comprises a dinitrile compound and a trinitrile compound; based on the mass of the electrolyte, the mass percentage of the dinitrile compound is N1%, the mass percentage of the trinitrile compound is N2%, 1.1≤N1 / N2≤4.9; 3.2≤N1≤6.8; 1.4≤N2≤2.9; The dinitrile compound includes succinonitrile and adiponitrile. Based on the mass of the electrolyte, the mass percentage of succinonitrile is A1%, the mass percentage of adiponitrile is A2%, 1.27≤A1 / A2≤3.36; 2.8≤A1≤3.7; The electrolyte comprises ethylene carbonate and propylene carbonate. Based on the mass of the electrolyte, the mass percentage of the ethylene carbonate is X1%, the mass percentage of the propylene carbonate is X2%, and 1.1≤X2 / X1≤2.5; The electrolyte includes ethyl propionate and propyl propionate. Based on the mass of the electrolyte, the mass percentage of ethyl propionate is Y1%, the mass percentage of propyl propionate is Y2%, and 1.5≤Y2 / Y1≤2.

5.

2. The secondary battery according to claim 1, wherein the dinitrile compound further comprises at least one of malononitrile, glutaronitrile, pimelonitrile, suberonitrile, 3,3'-oxydipropionitrile, hexane-2-enedinitrile, fumaronitrile, 2-pentene dinitrile, methylglutaronitrile, (Z)-but-2-enedinitrile, 2,2,3,3-tetrafluorosuccinonitrile or 1,2-bis(2-cyanoethoxy)ethane; and / or, The trinitrile compound includes at least one of 1,3,6-hexanetrinitrile, 1,3,5-pentanetricarboxylonitrile, 4-(2-cyanoethyl)heptane dinitrile, or 1,2,3-tris(2-cyanoethoxy)propane.

3. The secondary battery according to claim 1, wherein the dinitrile compound further comprises at least two of malononitrile, glutaronitrile, pimelonitrile, suberonitrile, 3,3'-oxydipropionitrile, hexane-2-enedinitrile, fumaronitrile, 2-pentene dinitrile, methylglutaronitrile, (Z)-but-2-enedinitrile, 2,2,3,3-tetrafluorosuccinonitrile or 1,2-bis(2-cyanoethoxy)ethane; and / or, The trinitrile compound includes at least two of 1,3,6-hexanetrinitrile, 1,3,5-pentanetricarboxylonitrile, 4-(2-cyanoethyl)heptane dinitrile, or 1,2,3-tris(2-cyanoethoxy)propane.

4. The secondary battery according to claim 3, wherein the secondary battery satisfies at least one of the following: (1)7.0≤10T / D 2 ≤18.1; (2)7.0≤D≤12.7; (3) 2.2≤N1 / N2≤3.

7.

5. The secondary battery according to claim 4, wherein the secondary battery satisfies at least one of the following: (1)78.2≤T≤113.0; (2)7.6≤D≤10.6; (3)4.2≤N1≤5.9; (4)1.6≤N2≤2.5。 6. The secondary battery according to any one of claims 1 to 3, wherein the electrolyte comprises 1,2-bis(2-cyanoethoxy)ethane and 1,3,6-hexanetrinitrile, and based on the mass of the electrolyte, the mass percentage of 1,2-bis(2-cyanoethoxy)ethane is B1%, the mass percentage of 1,3,6-hexanetrinitrile is B2%, and 0.83≤B1 / B2≤2.

43.

7. The secondary battery according to claim 6, wherein the electrolyte satisfies at least one of the following: (1)1.1≤A2≤2.2; (2)1.0≤B1≤1.7; (3)0.7≤B2≤1.2; (4) 1.84≤A1 / A2≤2.91; (5) 1.36≤B1 / B2≤2.

00. 8 . The secondary battery according to claim 1 , wherein 29≤X1+X2≤51.

9. The secondary battery according to claim 8, wherein the electrolyte satisfies at least one of the following: (1) 34 ≤ X1 + X2 ≤ 46; (2)1.6≤X2 / X1≤2.

2. 10 . The secondary battery according to claim 1 , wherein 35≤Y1+Y2≤62. 11 . The secondary battery according to claim 10 , wherein 41≤Y1+Y2≤55.

12. The secondary battery according to any one of claims 1 to 3, wherein the electrolyte comprises a fluorine-containing compound, the fluorine-containing compound comprises at least one of fluorobenzene or fluoroethylene carbonate, and based on the mass of the electrolyte, the electrolyte satisfies at least one of the following: (1) The mass percentage of fluorobenzene is F1%, 0.9≤F1≤4.1; (2) The mass percentage of the fluoroethylene carbonate is F2%, 10.5≤F2≤19.

5.

13. The secondary battery according to claim 12, wherein the electrolyte satisfies at least one of the following: (1)2.7≤F1≤3.4; (2)12.5≤F2≤17.5。 14. The secondary battery according to any one of claims 1 to 3, wherein the electrolyte comprises a compound of formula I, and the chemical formula of the compound of formula I is: ; Based on the mass of the electrolyte, the mass percentage of the compound of formula I is H%, 0.2≤H≤0.

9.

15. The secondary battery according to any one of claims 1 to 3, wherein the electrolyte comprises a compound of formula II, and the chemical formula of the compound of formula II is: ; Based on the mass of the electrolyte, the mass percentage of the compound of formula II is G%, 0.2≤G≤0.

7.

16. According to the secondary battery of claim 1, the silicon-based particles include a carbon skeleton and a protective layer located on at least a portion of the surface of the carbon skeleton, the material of the protective layer includes amorphous carbon, and the material of the carbon skeleton includes at least one of artificial graphite, natural graphite, mesophase carbon microbeads, soft carbon or hard carbon. 17 . An electronic device comprising the secondary battery according to claim 1 .