A metal organic framework derived carbon magnetic solid phase extraction material and its preparation method and application
Through the combination of metal organic framework-derived carbon magnetic solid-phase extraction material adsorbent and liquid chromatography-tandem mass spectrometry, the accuracy and efficiency of trace PPDs and PPD-Qs detection in ambient water is solved, and an efficient analysis method is achieved.
Patent Information
- Application Number
- CN202410290321.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-03-14
AI Technical Summary
In the prior art, when detecting trace amounts of p-phenylenediamine anti-aging agents (PPDs) and their derivatives (PPD-Qs) in ambient water, the pre-treatment method is cumbersome, time-consuming and low accuracy, which affects the accuracy of the results.
The MOF precursor with Fe3+ and Ni2+ as the center metal ions and ferrocene dicarboxylic acid as the organic ligand was constructed by solvothermal method. The porous structure was constructed by high-temperature carbonization, which was used for magnetic solid phase extraction technology and was detected in combination with liquid chromatography-tandem mass spectrometry.
It realizes simple, fast and efficient enrichment and analysis of trace amounts of PPDs and PPD-Qs in environmental water, improving the accuracy and efficiency of detection, and simplifying the pre-processing operation process.
Smart Images

Figure CN118179439B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of analysis and detection, and particularly relates to a metal organic framework derived carbon magnetic solid phase extraction material and a preparation method and application thereof. Background Art
[0002] Tire wear particles (TWP) are a mixture of tire fragments produced by friction and shear force between the tire tread and the road. They are widely migrated to the atmosphere, rivers, oceans, sediments, soil and other environmental media through wind, ocean currents and atmospheric deposition and continue to accumulate. It is estimated that the global TWP release in 2021 will be as high as 7.22×109t, and about 0.22×106~2.2×106t will eventually be discharged into the marine environment. It is considered by environmental scientists to be one of the important sources of pollutants in the ocean. TWP continuously leaches a large amount of heavy metals and organic pollutants during migration and transformation. Among them, p-phenylenediamine antioxidants (PPDs) are additives in the tire processing process to inhibit ozone aging, fatigue aging, thermal oxidation aging and catalytic oxidation of metal ions of rubber products. They are currently the largest rubber antioxidants used in the global tire manufacturing industry. With the above applications, PPDs will be continuously released into environmental water with industrial wastewater and urban runoff. N-isopropyl-N′-phenyl-p-phenylenediamine (IPPD) is an allergen for allergic dermatitis and can cause human contact dermatitis and occupational eczema. Exposure to N-(1,3-dimethylbutyl)-N′-phenyl-p-phenylenediamine (6PPD) reduces the hatching rate of zebrafish embryos, leads to changes in hormone levels and expression of genes related to the hypothalamus-pituitary-adrenal axis, and causes developmental disorders. It is worth noting that in 2020, it was first discovered that N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediaminequinone (6PPD-Q) is a derivative of 6PPD produced under heat and ozone conditions, with a median lethal concentration (LC50) of 6PPD for juvenile coho salmon. 50 ) was 90.82±0.27ng / L, compared with 6PPD (LC 50 , 250±60μg / L), and the toxicity is increased by more than 300 times. PPDs and PPD-Qs are easily migrated in water bodies due to their low volatility. After being ingested by marine organisms, they enter the human body through the food chain and cause potential harm. Literature reports that PPDs and PPD-Qs have been detected in lake water, sea water, river water and urban runoff. Therefore, the detection of PPDs and PPD-Qs in environmental water has become a primary issue for understanding the level of pollutant exposure, evaluating human health risks and conducting safety prevention and control.
[0003] At present, the detection methods of PPDs and PPD-Qs in environmental water mainly include liquid chromatography-tandem mass spectrometry (LC-MS / MS) and ultra-high-performance liquid chromatography-tandem mass spectrometry (UHPLC-MS / MS). Since PPDs and PPD-Qs in environmental water are usually at trace levels and water samples are diverse, pretreatment is required before instrumental analysis to achieve the purpose of enrichment and purification. At present, the only pretreatment methods for PPDs and PPD-Qs in environmental water are liquid-liquid extraction and solid phase extraction based on commercial HLB columns. The above two methods are cumbersome and time-consuming, and are prone to cause the loss of the target substance, which is already at an extremely low concentration, and directly affect the accuracy of the final result.
[0004] Magnetic solid-phase extraction (MSPE), as a revolutionary technology in the field of separation and enrichment, is a pre-treatment technology that uses magnetic or magnetizable functional materials as adsorbents and is widely used in environmental sanitation, food safety, biomedicine and other fields. This technology does not require centrifugation, filtration and other operations, and can achieve separation of the target and the sample solution only by relying on an external magnet; at the same time, the adsorbent dispersed in the solution can fully contact with the target, with a short diffusion distance and high extraction efficiency. Among them, the adsorbent, as the core of MSPE, determines the efficiency and cost of the method.
[0005] Therefore, how to provide a metal organic framework derived carbon magnetic solid phase extraction material, which can be directly used as an MSPE adsorbent for simple, rapid and efficient analysis of PPDs and PPD-Qs in environmental water, is a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention
[0006] The object of the present invention is to provide a metal organic framework derived carbon magnetic solid phase extraction material and a preparation method and application thereof, so as to solve at least one of the above technical problems.
[0007] To achieve the above object, the first aspect of the present invention provides a method for preparing a metal organic framework-derived carbon magnetic solid phase extraction material, the preparation method comprising:
[0008] S1. Dissolve FeCl3·6H2O and NiCl2·6H2O in DMF and mix them evenly with ultrasound to obtain solution A;
[0009] S2, dissolving ferrocene dicarboxylic acid and PVP in DMF, and mixing evenly by ultrasonication to obtain solution B;
[0010] S3, mixing the solution A and the solution B evenly to obtain a solution C;
[0011] S4, transferring the solution C to a high temperature and high pressure reactor to react and obtain a reactant;
[0012] S5, centrifuging, washing, and drying the reactant to obtain Fc-MOF;
[0013] S6. Carbonizing the Fc-MOF at high temperature to obtain Fc-MOF@NC, i.e., a metal organic framework-derived carbon magnetic solid phase extraction material.
[0014] In the first aspect, in step S4, the reaction conditions include: reaction temperature of 120-130° C.; reaction time of 10-14 h.
[0015] In the first aspect, the step S5 centrifuges, washes, and dries the reactant to obtain Fc-MOF, comprising the following steps: centrifuging the reactant to obtain a centrifuged product; washing the centrifuged product three times with DMF to obtain a first washed product; washing the first washed product three times with ethanol to obtain a second washed product; and drying the second washed product in a vacuum drying oven to obtain Fc-MOF.
[0016] In the first aspect, the drying temperature is 60-80°C.
[0017] In the first aspect, the high-temperature carbonization of the Fc-MOF comprises: heating the Fc-MOF to 600-800° C. under argon protection, and keeping the temperature for 1-2 hours.
[0018] In the first aspect, the heating rate is 1-2°C / min.
[0019] The second aspect of the present invention provides a metal organic framework derived carbon magnetic solid phase extraction material, which is prepared by the preparation method of the metal organic framework derived carbon magnetic solid phase extraction material described in the first aspect.
[0020] The third aspect of the present invention provides an application of a metal organic framework derived carbon magnetic solid phase extraction material, which includes applying the metal organic framework derived carbon magnetic solid phase extraction material described in the second aspect to the detection of PPDs and PPD-Qs in environmental water.
[0021] A fourth aspect of the present invention provides a method for detecting PPDs and PPD-Qs in environmental water, the detection method comprising:
[0022] Environmental water samples were collected and filtered through a 0.45 μm filter membrane to obtain a filtrate;
[0023] Add 6 mg of the metal organic framework derived carbon magnetic solid phase extraction material described in the second aspect to 100 mL of the filtrate, shake thoroughly for 3 minutes, apply an external magnetic field to separate the metal organic framework derived carbon magnetic solid phase extraction material from the sample solution, discard the supernatant, use 1 mL of dichloromethane / ACN (8 / 2, v / v) to elute 3 times, combine the eluates, concentrate to dryness with nitrogen blowing, use 0.1 mL of MeOH to re-dissolve, and filter through a 0.22 μm organic filter membrane to obtain a test solution;
[0024] The liquid to be tested is detected by liquid chromatography-tandem mass spectrometry.
[0025] In the fourth aspect, the detection conditions of the liquid chromatography-tandem mass spectrometry include: liquid chromatography conditions and mass spectrometry conditions; the liquid chromatography conditions include: the chromatographic column is C 18 Column; mobile phase A is 0.1% formic acid-water solution; mobile phase B is methanol; gradient elution program: at 0-2min, the volume of mobile phase A accounts for 30%, and the volume of mobile phase B accounts for 70%; at 2-10min, the volume of mobile phase A accounts for 0%-30%, and the volume of mobile phase B accounts for 30%-100%; injection volume is 5μL, flow rate is 0.4mL / min, and column oven temperature is 30°C;
[0026] The mass spectrometry conditions include: electrospray ion source positive ion mode; ion spray voltage 5.0 kV, declustering voltage 70 V, ion source temperature 500° C., curtain gas pressure 25 psi, collision gas pressure medium, spray gas pressure 40 psi, auxiliary heating gas pressure 45 psi.
[0027] Beneficial effects:
[0028] The present invention provides a method for preparing a metal organic framework-derived carbon magnetic solid phase extraction material, which adopts a two-step method to construct Fc-MOF@NC. First, a solvothermal method is used to construct a Fe 3+ and Ni 2+ The Fc-MOF precursor with a central metal ion and ferrocene dicarboxylic acid as an organic ligand provides a stable three-dimensional spatial structure and a high specific surface area for the magnetic solid phase extraction material; then, a Fc-MOF@NC (magnetic solid phase extraction material) with a porous structure is constructed by high-temperature carbonization to improve the adsorption performance. The present invention uses Fc-MOF@NC as an adsorbent in the magnetic solid phase extraction technology to enrich trace PPDs and PPD-Qs in environmental water, and combines liquid chromatography-tandem mass spectrometry to establish a detection method for PPDs and PPD-Qs in environmental water, thereby simply, quickly and efficiently analyzing PPDs and PPD-Qs in environmental water.
[0029] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of this specification or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 This is a flow chart of a method for preparing a metal organic framework-derived carbon magnetic solid phase extraction material in this application;
[0032] Figure 2 This is the Fourier infrared spectrum of Fc-MOF@NC in Examples 1-3 of the present application;
[0033] Figure 3 The X-ray diffraction spectrum of Fc-MOF@NC in Examples 1-3 of the present application;
[0034] Figure 4 This is the Raman spectrum of Fc-MOF@NC in Examples 1-3 of the present application;
[0035] Figure 5 : This is the hysteresis curve of Fc-MOF@NC in Examples 1-3 of the present application;
[0036] Figure 6 The nitrogen adsorption-desorption isotherm diagram of Fc-MOF@NC in Examples 1-3 of the present application;
[0037] Figure 7 This is the pore size distribution diagram of Fc-MOF@NC in Examples 1-3 of the present application;
[0038] Figure 8 A scanning electron microscope image of Fc-MOF provided in the examples of the present application;
[0039] Fig. 9 A scanning electron microscope image of Fc-MOF@NC provided in the examples of the present application;
[0040] Fig.10 A transmission electron microscopy image of Fc-MOF provided in the examples of the present application;
[0041] Fig.11A transmission electron microscopy image of Fc-MOF@NC provided in the examples of the present application;
[0042] Fig.12 This is a graph showing the experimental results of the effect of solution pH on target recovery provided in the examples of the present application;
[0043] Fig.13 This is a graph showing the experimental results of the effect of ion strength on target recovery provided in the examples of the present application;
[0044] Fig.14 This is a graph showing the experimental results of the effect of adsorbent dosage on target recovery rate provided in the examples of the present application;
[0045] Fig.15 This is a graph showing the experimental results of the effect of adsorption time on the recovery rate of the target substance provided in the examples of the present application;
[0046] Fig.16 This is a graph showing the experimental results of the effect of the type of elution solvent on the recovery rate of the target substance provided in the examples of the present application;
[0047] Fig.17 A graph showing the effect of elution volume on target recovery provided in the examples of the present application;
[0048] Fig.18 This is the MRM mass spectrum of the target enrichment after the seawater sample was treated with magnetic solid phase extraction technology in this application. DETAILED DESCRIPTION
[0049] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.
[0050] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.
[0051] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or obtained by existing methods.
[0052] The general idea of the present invention is as follows:
[0053] Magnetic solid phase extraction is a pretreatment technology that uses magnetic or magnetizable functional materials as adsorbents. The adsorbent, as the core of MSPE, determines the efficiency and cost of the method.
[0054] Metal-organic framework-derived porous carbon (MPCs) is a porous carbon material constructed by using metal-organic frameworks (MOFs) as precursors, retaining carbon or heteroatoms in organic ligands under inert gas and pyrolysis conditions, converting metal ions into metal elements or oxides and embedding them into carbon frameworks. MPCs are composite materials composed of metals (oxides) and carbon in a regular and ordered structure. They are both the inheritance of the excellence of MOFs and the development of the performance of novel carbon materials.
[0055] From the perspective of MOFs materials, MOFs are porous crystalline materials formed by metal ions or ion clusters connected to organic ligands in a highly ordered manner. They have the characteristics of diverse structures, adjustable pores, large specific surface area and diverse compositions. There is no doubt that these characteristics make MOFs excellent adsorbents, but some MOFs have poor stability in aqueous or organic phases, which can easily lead to structural collapse, limiting their application in sample pretreatment. MPCs materials solve the problem of solvent stability while maintaining the original MOFs properties. Compared with traditional carbon materials, in terms of synthesis, MOFs are composed of organic skeletons and do not require the addition of additional carbon sources. They can be directly calcined to obtain porous carbon; for metal sources such as Fe 3+ 、Co 2+ and Ni 2+ The MOFs precursor, calcination directly gives MPCs sufficient magnetic strength, and the synthesis is simple and convenient. In terms of structure, MPCs inherit the stable and orderly structure of MOFs, and the metal elements or oxides are evenly distributed in the carbon skeleton. It has a larger specific surface area and higher porosity than traditional carbon materials. When used as an adsorbent, it has a large adsorption capacity and high extraction efficiency. These excellent properties make MPCs as MSPE adsorbents have great development prospects in the field of sample pretreatment.
[0056] Based on this, the present invention aims to solve the problems of the existing pretreatment methods such as cumbersome operation, time-consuming and low accuracy. 3+ and Ni 2+ A ferrocenyl MOF (Fc-MOF) precursor was constructed by solvothermal method with ferrocenyl dicarboxylic acid as the central metal ion and ferrocenyl dicarboxylic acid as the organic ligand. For the first time, magnetic Fc-MOF-derived porous carbon (Fc-MOF@NC) with uniform particle size and high adsorption performance was constructed by high-temperature carbonization. It was directly used as an MSPE adsorbent for simple, rapid and efficient analysis of PPDs and PPD-Qs in environmental water.
[0057] See also Figure 1 The present invention provides a method for preparing a metal organic framework-derived carbon magnetic solid phase extraction material, the preparation method comprising:
[0058] S1. Dissolve FeCl3·6H2O and NiCl2·6H2O in DMF and mix them evenly with ultrasound to obtain solution A;
[0059] S2, dissolving ferrocene dicarboxylic acid and PVP in DMF, and mixing evenly by ultrasonication to obtain solution B;
[0060] S3, mixing the solution A and the solution B evenly to obtain a solution C;
[0061] S4, transferring the solution C to a high temperature and high pressure reactor to react and obtain a reactant;
[0062] In some possible embodiments, the reaction conditions include: reaction temperature of 120-130° C.; reaction time of 10-14 h.
[0063] By controlling the temperature and time of the reaction, a stable three-dimensional spatial structure can be constructed and the generation of impurities can be controlled.
[0064] S5, centrifuging, washing, and drying the reactant to obtain Fc-MOF;
[0065] In some possible embodiments, the step S5 centrifuges, washes, and dries the reactant to obtain Fc-MOF, comprising the following steps: centrifuging the reactant to obtain a centrifuged product; washing the centrifuged product three times with DMF to obtain a first washed product; washing the first washed product three times with ethanol to obtain a second washed product; and drying the second washed product in a vacuum drying oven to obtain Fc-MOF.
[0066] In some possible embodiments, the drying temperature is 60-80°C.
[0067] The reactants are preliminarily purified by centrifugation to remove the solvent; since DMF is used as the reaction solvent, some small molecule impurities can be removed by washing with DMF first; since DMF has a high boiling point and is difficult to remove, residual DMF and impurities can be removed by further washing with ethanol to reduce the temperature of subsequent drying; the temperature of the vacuum drying oven is set at 60-80°C to remove the residual solvent.
[0068] S6. Carbonizing the Fc-MOF at high temperature to obtain Fc-MOF@NC, i.e., a metal organic framework-derived carbon magnetic solid phase extraction material.
[0069] In some possible embodiments, the high-temperature carbonization of the Fc-MOF includes: heating the Fc-MOF to 600-800° C. under argon protection, and keeping the temperature for 1-2 hours.
[0070] In some possible embodiments, the heating rate is 1-2° C. / min.
[0071] Specifically, the present invention provides a method for preparing a metal organic framework-derived carbon magnetic solid phase extraction material, which adopts a two-step method to construct Fc-MOF@NC. First, a solvothermal method is used to construct a Fe 3+ and Ni 2+ The Fc-MOF precursor with a central metal ion and ferrocene dicarboxylic acid as an organic ligand provides a stable three-dimensional spatial structure and a high specific surface area for the magnetic solid phase extraction material; then, a Fc-MOF@NC (magnetic solid phase extraction material) with a porous structure is constructed by high-temperature carbonization to improve the adsorption performance. The present invention uses Fc-MOF@NC as an adsorbent in the magnetic solid phase extraction technology to enrich trace PPDs and PPD-Qs in environmental water, and combines liquid chromatography-tandem mass spectrometry to establish a detection method for PPDs and PPD-Qs in environmental water, thereby simply, quickly and efficiently analyzing PPDs and PPD-Qs in environmental water.
[0072] Based on a general inventive concept, the present invention provides a metal organic framework derived carbon magnetic solid phase extraction material, and the metal organic framework derived carbon magnetic solid phase extraction material is prepared by the preparation method of the metal organic framework derived carbon magnetic solid phase extraction material described in the first aspect.
[0073] The metal organic framework derived carbon magnetic solid phase extraction material of the present application, as an adsorbent in MSPE, has a high specific surface area, a typical mesoporous structure and sufficient magnetic strength, simplifies the operation process of the MSPE pretreatment method, and improves work efficiency and the accuracy of detection and analysis.
[0074] Based on a general inventive concept, the present invention provides an application of a metal organic framework derived carbon magnetic solid phase extraction material, which includes applying the metal organic framework derived carbon magnetic solid phase extraction material described in the second aspect to the detection of PPDs and PPD-Qs in environmental water.
[0075] Based on a general inventive concept, the present invention provides a method for detecting PPDs and PPD-Qs in environmental water, the detection method comprising:
[0076] Environmental water samples were collected and filtered through a 0.45 μm filter membrane to obtain a filtrate;
[0077] Add 6 mg of the metal organic framework derived carbon magnetic solid phase extraction material described in the second aspect to 100 mL of the filtrate, shake thoroughly for 3 minutes, apply an external magnetic field to separate the metal organic framework derived carbon magnetic solid phase extraction material from the sample solution, discard the supernatant, use 1 mL of dichloromethane / ACN (8 / 2, v / v) to elute 3 times, combine the eluates, concentrate to dryness with nitrogen blowing, use 0.1 mL of MeOH to re-dissolve, and filter through a 0.22 μm organic filter membrane to obtain a test solution;
[0078] The liquid to be tested is detected by liquid chromatography-tandem mass spectrometry.
[0079] In conjunction with the fourth aspect of the present application, the detection conditions of the liquid chromatography-tandem mass spectrometry include: liquid chromatography conditions and mass spectrometry conditions; the liquid chromatography conditions include: the chromatographic column is C 18 Column; mobile phase A is 0.1% formic acid-water solution; mobile phase B is methanol; gradient elution program: at 0-2min, the volume of mobile phase A accounts for 30%, and the volume of mobile phase B accounts for 70%; at 2-10min, the volume of mobile phase A accounts for 0%-30%, and the volume of mobile phase B accounts for 30%-100%; injection volume is 5μL, flow rate is 0.4mL / min, and column oven temperature is 30°C;
[0080] The environmental water samples in this application were selected from Bohai Bay seawater, Qinglong Lake water and urban runoff in Caofeidian District, Tangshan City, Hebei Province. Before sample analysis, the samples were filtered through a 0.45 μm filter membrane to remove suspended particles, and then stored at 4°C for use in magnetic solid phase extraction.
[0081] The above detection conditions were used to locate the four target PPDs (IPPD and 6PPD) and PPD-Qs (6PPD-Q and IPPD-Q). The retention times, quantitative ion pairs, qualitative ion pairs and collision energy reference values are shown in Table 1:
[0082] Table 1 Retention time, quantitative ion pair, qualitative ion pair and collision energy of PPDs and PPD-Qs
[0083]
[0084] The metal organic framework derived carbon magnetic solid phase extraction material of the present application and its preparation method and application will be described in detail below in combination with examples and experimental data.
[0085] Example 1
[0086] A method for preparing a metal organic framework derived carbon magnetic solid phase extraction material, the preparation method comprising:
[0087] (1) Weigh 135.25 mg of FeCl3·6H2O and 119 mg of NiCl2·6H2O, dissolve them in 10 mL of DMF, sonicate for 30 min, and mix well to obtain solution A;
[0088] (2) Weigh 274.05 mg of ferrocene dicarboxylic acid and 3330 mg of PVP and dissolve them in 10 mL of DMF. Ultrasonicate for 30 min and mix well to obtain solution B.
[0089] (3) Mixing solution A and solution B evenly to obtain solution C;
[0090] (4) transferring solution C to a high temperature and high pressure reactor and reacting at 125° C. for 12 h to obtain a reactant;
[0091] (5) centrifuging the reactant to obtain a centrifugal product; washing the centrifugal product three times with DMF to obtain a first washed product; washing the first washed product three times with ethanol to obtain a second washed product (brown yellow precipitate); drying the second washed product in a vacuum drying oven at 60° C. to obtain Fc-MOF;
[0092] (6) Fc-MOF was placed in a tubular furnace and heated to 800°C at a heating rate of 1.5°C / min under an argon protection environment and kept warm for 1.5 h. After the reaction was completed, it was naturally cooled to room temperature to obtain Fc-MOF@NC-800 (black powder), i.e., a metal organic framework-derived carbon magnetic solid phase extraction material.
[0093] Example 2
[0094] Compared with Example 1, the difference lies in step (6), placing Fc-MOF in a tubular furnace, heating to 700°C at a heating rate of 1.5°C / min under an argon protection environment, and keeping warm for 1.5 hours; after the reaction is completed, naturally cooling to room temperature to obtain Fc-MOF@NC-700 (black powder), i.e., a metal organic framework-derived carbon magnetic solid phase extraction material.
[0095] Example 3
[0096] Compared with Example 1, the difference lies in step (7), placing Fc-MOF in a tubular furnace, heating to 600°C at a heating rate of 1.5°C / min under an argon protection environment, and keeping warm for 1.5 hours; after the reaction is completed, naturally cooling to room temperature to obtain Fc-MOF@NC-600 (black powder), i.e., a metal organic framework-derived carbon magnetic solid phase extraction material.
[0097] The Fc-MOF@NC prepared in Examples 1-3 were characterized using a scanning electron microscope, a transmission electron microscope, a Fourier transform infrared spectrometer, an X-ray diffractometer, a Raman spectrometer, a vibrating sample magnetometer, and a fully automatic specific surface area and porosity analyzer.
[0098] Fourier transform infrared spectrum ( Figure 2 ) showed that Fc-MOF@NC-600, Fc-MOF@NC-700 and Fc-MOF@NC-800 were at 1591cm -1 、1420cm -1 and 572cm -1 There are bending vibration peaks of C=C, CO and Fe-O at all locations; from the X-ray diffraction spectrum ( Figure 3 ) observed the typical diffraction peaks of Fe and Ni nanoparticles: 42.2°(400), 45.6°(200) and 48.1°(220); in the Raman spectrum ( Figure 4 ), 1350cm -1 and 1595cm -1 The vibration peaks of carbon D band (amorphous carbon) and G band (graphite carbon) appeared at the D / I G ) represents the degree of graphitization. The smaller the ratio, the higher the degree of graphitization of the carbon material. D / I G The values are 1.24, 1.13 and 0.85 respectively. With the increase of carbonization temperature, I D / I G The value gradually decreases, and the higher the graphitization degree of Fc-MOF@NC is.
[0099] Hysteresis curve diagram ( Figure 5 ) showed that the saturation magnetic intensities of Fc-MOF@NC-600, Fc-MOF@NC-700 and Fc-MOF@NC-800 were 65.93, 72.94 and 105.18emu / g, respectively.
[0100] The specific surface area of Fc-MOF@NC prepared in Examples 1-3 was analyzed by nitrogen adsorption-desorption experiment. The results are as follows: Figure 6 and Figure 7 As shown in the (pore size distribution diagram), the nitrogen adsorption-desorption curves of the three Fc-MOF@NCs are all type III curves. According to calculations, the specific surface areas of Fc-MOF@NC-600, Fc-MOF@NC-700, and Fc-MOF@NC-800 are 180.93, 184.23, and 219.48 m 2 / g, and the average pore sizes were 8.81, 7.18 and 6.64 nm, respectively, which are within the pore size range of typical mesoporous materials (2-50 nm), proving that Fc-MOF@NC constructed under different conditions all have typical mesoporous structures.
[0101] In summary, with the increase of carbonization temperature, the specific surface area and magnetic strength of the calcined Fc-MOF@NC gradually increase. When Fc-MOF@NC is used as an adsorbent, the higher its specific surface area, the higher the adsorption efficiency; the greater the saturation magnetic strength, the faster the separation of the adsorbent and the sample matrix. Therefore, the experiment finally chose a carbonization temperature of 800℃ to construct Fc-MOF@NC.
[0102] Scanning electron microscopy and transmission electron microscopy were used to characterize Fc-MOF and Fc-MOF@NC: Figure 8 and Fig. 9 The results show that Fc-MOF is a typical spherical flower-like structure, which is composed of interconnected nanosheets with distinct contours. After high-temperature carbonization, Fc-MOF@NC still maintains the original morphology of the Fc-MOF precursor, and the Fe and Ni nanoparticles are evenly embedded in the porous carbon skeleton ( Fig.10 and Fig.11 ), proving that Fc-MOF@NC has been successfully prepared.
[0103] In order to establish MSPE conditions and obtain the best extraction conditions, the present invention used 100 mL of 20 ng / mL PPDs and PPD-Qs standard aqueous solution to investigate the effects of adsorbent dosage, adsorption time, solution pH, ionic strength, elution solvent type and volume on the recovery rates of four PPDs and PPD-Qs. All experiments were repeated 3 times. The results are as follows: Figure 12-17 As shown:
[0104] (1) Solution pH and ionic strength
[0105] The pH of environmental water is usually 6.0-8.5. The pH of the solution affects the ionization of the target and the active sites of the adsorbent; the ionic strength is an important factor affecting the solubility of the target. The experiment used 6 mg of Fc-MOF@NC for adsorption for 3 minutes and 1 mL of dichloromethane / ACN (8 / 2, v / v) for elution three times to investigate the effects of solution pH 5-9 and ionic strength (0, 50, 100, 150 and 200 mmol / L NaCl) on the recovery rates of four PPDs and PPD-Qs. The results are shown in Fig.12 and Fig.13 As shown in the figure, with the changes of solution pH and ionic strength, the recoveries of the four PPDs and PPD-Qs did not change significantly, indicating that solution pH and ionic strength had no significant effect on the recovery of the target substances, and there was no need to adjust the solution pH and ionic strength in the experiment.
[0106] (2) Adsorbent dosage and adsorption time
[0107] The appropriate amount of adsorbent and adsorption time can make the target fully contact with the adsorbent, which is beneficial to reduce the cost of pretreatment methods, save time, and obtain the highest extraction efficiency. The experiment fixed the adsorption time to 3min and investigated the effect of 3-7mg Fc-MOF@NC on the recovery rate of 4 PPDs and PPD-Qs. Fig.14 It can be seen that as the amount of adsorbent increased from 3 mg to 6 mg, the recovery rates of the four PPDs and PPD-Qs increased significantly to 98.1% to 105%. The recovery rate of the target product did not change significantly when the amount of adsorbent was further increased to 7 mg. At the same time, the study investigated the effects of 0.5, 1, 2, 3 and 4 min on the recovery rates of PPDs and PPD-Qs. Fig.15 It shows that within 0.5 to 3 minutes, the recovery rates of the four PPDs and PPD-Qs gradually increase with the extension of adsorption time, reaching the best (98.1% to 105%) at 3 minutes. Further extension to 4 minutes has no effect on the recovery rates of the three targets. Therefore, the experiment finally used 6 mg Fc-MOF@NC to complete the adsorption within 3 minutes.
[0108] (3) Elution solvent and elution volume
[0109] Elution is the process of completely releasing the target from the adsorbent, which determines the accuracy of the method. Under the optimal loading conditions, the effects of elution solvent types MeOH, ACN, dichloromethane / ACN (5 / 5, v / v), dichloromethane / ACN (8 / 2, v / v) and dichloromethane, and elution volume (single elution volume × elution times) on the recovery rates of four PPDs and PPD-Qs were investigated. The results are shown in Figure 2. Fig.16 and Fig.17 As shown, from left to right are IPPD, IPPD-Q, 6PPD and 6PPD-Q. When eluted three times with 1 mL of dichloromethane / ACN (8 / 2, v / v), the recoveries of the four PPDs and PPD-Q reached the best of 98.1% to 105%. Therefore, the experiment selected 1 mL of dichloromethane / ACN (8 / 2, v / v) for elution three times.
[0110] This application provides a method for detecting PPDs and PPD-Qs in environmental water. In order to verify the feasibility of the method, the matrix effect, linear range, detection limit (LODs), quantification limit (LOQs), accuracy and precision of the method are evaluated, and actual sample analysis is performed:
[0111] (1) Matrix effect
[0112] In positive ion mode, matrix co-extracts compete with target analytes for H+ , matrix inhibition will occur; on the contrary, if the matrix co-extract can provide H + In LC-MS / MS, matrix effect (ME) is an important factor affecting the accuracy and precision of the results.
[0113] This application investigates the matrix effects of three matrices: seawater, lake water, and urban runoff. The three blank sample matrices were used to prepare seven concentrations of matrix mixed standard solutions, and the standard curves were drawn with the peak area corresponding to the quantitative ion as the ordinate y and the concentration of the standard solution as the abscissa x (ng / mL). The study used the slope ratio of four PPDs and PPD-Qs standard working solutions and matrix mixed standard solutions within the linear range to explore the matrix effect of the target. When the slope ratio is >1.2, it indicates that the target has an enhanced matrix effect in the matrix; the slope ratio is <0.8, indicating that PPDs and PPD-Qs have a significantly weakened matrix effect in the matrix.
[0114] Table 2 shows that the slope ratios of PPDs and PPD-Qs in seawater, lake water and urban runoff are 0.98-1.08, 0.87-1.03 and 0.92-1.11, respectively, all less than 1.2, indicating that this method has no obvious matrix effect. The constructed Fc-MOF@NC as MSPE adsorbent can effectively remove impurities in environmental water and realize accurate analysis of PPDs and PPD-Qs in various environmental waters.
[0115] Table 2 Slope ratios of PPDs and PPD-Qs in three matrices
[0116] Analytes seawater Lake Urban runoff IPPD 0.94 1.00 0.99 IPPD-Q 0.95 0.96 1.00 6PPD 0.93 0.92 0.98 6PPD-Q 0.97 0.96 1.00
[0117] (2) Linear range, detection limit and quantification limit
[0118] Under the above optimal experimental conditions, based on Fc-MOF@NC magnetic solid phase extraction and combined with LC-MS / MS analysis, the analytical method for IPPD, IPPD-Q, 6PPD and 6PPD-Q in water environment was established. Table 3 shows that the linear range of the method in seawater and urban runoff is 0.015-1000 ng / L, and the linear correlation coefficient r≥0.9992; the linear range of the method in lake water is 0.020-1000 ng / L, and r≥0.9994. The LODs and LOQs of the above method in seawater are 0.006-0.045 ng / L and 0.020-0.150 ng / L, respectively; the LODs and LOQs of the above method in lake water are 0.006-0.030 ng / L and 0.020-0.120 ng / L, respectively; the LODs and LOQs of the above method in urban runoff are 0.006-0.030 ng / L and 0.020-0.120 ng / L, respectively, indicating that the method has a low detection limit and good sensitivity.
[0119] The blank control seawater sample was spiked (the concentration of the four PPDs and PPD-Qs was 200 ng / L) and the enrichment factor (EF) was calculated by comparing the concentration of the target before and after the magnetic solid phase extraction technology pretreatment in this application. Fig.18 As shown, when the sample volume is 100 mL, the adsorption can be completed within 3 minutes using 6 mg Fc-MOF@NC, and the EFs are as high as 981 to 1050 times, indicating that this method can efficiently enrich PPDs and PPD-Qs in environmental water samples.
[0120] Table 3 Linear range, detection limit and quantification limit of the method
[0121]
[0122]
[0123] Note: ① Peak area; ② Target concentration, ng / L
[0124] (3) Accuracy and precision
[0125] Spike recovery experiments were carried out on blank seawater, lake water and urban runoff at three concentration levels (1, 20 and 500 ng / L), and the precision of the method was evaluated by the RSD of the chromatographic peak area determined three times within the day (n=3) and between days (n=3). Table 4 shows that the recoveries of the four PPDs and PPD-Qs in seawater samples were 84.1% to 104%, the intra-day precision was 1.4% to 5.1%, and the inter-day precision was 2.1% to 9.4%; the recoveries of the four PPDs and PPD-Qs in lake water samples were 87.4% to 108%, the intra-day precision was 1.3% to 6.5%, and the inter-day precision was 3.2% to 8.4%; the recoveries of the four PPDs and PPD-Qs in urban runoff were 84.9% to 101%, the intra-day precision was 1.2% to 7.1%, and the inter-day precision was 1.9% to 11%; the above results show that this method has good accuracy and precision.
[0126] Table 4 Recovery and precision of the method
[0127]
[0128]
[0129] (4) Actual sample analysis
[0130] The detection method established in this application was used to analyze 8 samples of 4 PPDs and PPD-Qs in seawater, lake water and urban runoff. The results are shown in Tables 5 to 7. In seawater samples, IPPD was detected in 5 samples with a detection concentration of 2.8±0.20 to 3.3±0.15; IPPD-Q was detected in 2 samples with a detection concentration of 0.9±0.04 and 4.0±0.24; 6PPD was detected in all 8 samples with a detection concentration of 0.1±0.01 to 6.7±0.45; 6PPD-Q was detected in 3 samples with a detection concentration of 1.9±0.10 to 20.6±0.52. In lake water samples, IPPD was detected in 5 samples with a detection concentration of 2.3±0.02~64.1±2.16; IPPD-Q was detected in 1 sample with a detection concentration of 3.5±0.11; 6PPD was detected in all 8 samples with a detection concentration of 5.7±0.18~93.8±6.96; in urban runoff, IPPD was detected in 7 samples with a detection concentration of 2.6±0.14~5.9±0.55, IPPD-Q, 6PPD and 6PPD-Q were detected in all 8 samples, with detection concentrations of 82.2±1.62~479.5±6.09, 4.9±0.05~10.5±0.06 and 4.6±0.09~167.8±1.94, respectively. All samples were spiked with 20 ng / L of PPDs and PPD-Qs, and the recoveries of seawater, lake water, and urban runoff samples were 85.3%-108%, 82.7%-107%, and 83.3%-106%, respectively. This indicates that the method has good accuracy and can be used for the analysis of PPDs and PPD-Qs in actual water environments.
[0131] Table 5 Analysis results of four PPDs and PPD-Qs in seawater
[0132]
[0133]
[0134] Table 6 Analysis results of four PPDs and PPD-Qs in lake water
[0135]
[0136]
[0137] Table 7 Analysis results of four PPDs and PPD-Qs in urban runoff
[0138]
[0139]
[0140] One or more technical solutions in the embodiments of the present application also have at least the following technical effects or advantages:
[0141] (1) The present invention uses Fc-MOF@NC as an adsorbent in magnetic solid phase extraction technology to enrich trace amounts of PPDs and PPD-Qs in environmental water, and combines liquid chromatography-tandem mass spectrometry to establish a detection method for PPDs and PPD-Qs in environmental water, thereby simply, quickly and efficiently analyzing PPDs and PPD-Qs in environmental water.
[0142] (2) The magnetic solid phase extraction material Fc-MOF@NC provided in this application has a high specific surface area (180-220 m 2 / g) and saturation magnetic strength (65-105emu / g). When the sample volume is 100mL, the adsorption can be completed within 3min using 6mg Fc-MOF@NC. The enrichment multiples of PPDs and PPD-Qs are as high as 981-1050 times, which can accurately detect trace amounts of PPDs and PPD-Qs in environmental water samples.
[0143] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.
[0144] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0145] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing a metal organic framework derived carbon magnetic solid phase extraction material, It is characterized in that The preparation method comprises: S1, FeCl 3 6H 2 O and NiCl 2 6H 2 O was dissolved in DMF and mixed evenly by ultrasonication to obtain solution A; S2, dissolving ferrocene dicarboxylic acid and PVP in DMF, and mixing evenly by ultrasonication to obtain solution B; S3, mixing the solution A and the solution B evenly to obtain a solution C; S4, transferring the solution C to a high temperature and high pressure reactor to react and obtain a reactant; S5, centrifuging, washing, and drying the reactant to obtain Fc-MOF; S6, carbonizing the Fc-MOF at high temperature to obtain Fc-MOF@NC, i.e., a metal organic framework-derived carbon magnetic solid phase extraction material; In step S4, the reaction conditions include: reaction temperature of 120-130°C; reaction time of 10-14 h; The high-temperature carbonization of the Fc-MOF comprises: heating the Fc-MOF to 600-800° C. under argon protection, and keeping the temperature for reaction for 1-2 hours.
2. The method for preparing the metal organic framework derived carbon magnetic solid phase extraction material according to claim 1, It is characterized in that The step S5 centrifuges, washes, and dries the reactant to obtain Fc-MOF, comprising the following steps: Centrifuging the reactant to obtain a centrifugal product; The centrifuged product is washed three times with DMF to obtain a first washed product; Washing the first washed product three times with ethanol to obtain a second washed product; The second washed product is placed in a vacuum drying oven and dried to obtain Fc-MOF.
3. The method for preparing the metal organic framework derived carbon magnetic solid phase extraction material according to claim 2, It is characterized in that The drying temperature is 60-80°C.
4. The method for preparing the metal organic framework derived carbon magnetic solid phase extraction material according to claim 3, It is characterized in that The heating rate is 1-2°C / min.
5. A metal organic framework derived carbon magnetic solid phase extraction material, It is characterized in that The metal organic framework derived carbon magnetic solid phase extraction material is prepared by the preparation method of the metal organic framework derived carbon magnetic solid phase extraction material according to any one of claims 1 to 4.
6. Application of a metal organic framework derived carbon magnetic solid phase extraction material, It is characterized in that The application includes applying the metal organic framework-derived carbon magnetic solid phase extraction material of claim 5 to detect PPDs and PPD-Qs in environmental water.
7. A method for detecting PPDs and PPD-Qs in environmental water, It is characterized in that The detection method comprises: Environmental water samples were collected and filtered through a 0.45 μm filter membrane to obtain a filtrate; Add 6 mg of the metal organic framework derived carbon magnetic solid phase extraction material according to claim 5 to 100 mL of the filtrate, shake thoroughly for 3 min, apply an external magnetic field to separate the metal organic framework derived carbon magnetic solid phase extraction material from the sample solution, discard the supernatant, elute three times with 1 mL of dichloromethane / ACN in a volume ratio of 8:2, combine the eluates, concentrate to dryness with nitrogen blowing, re-dissolve with 0.1 mL of MeOH, filter through a 0.22 µm organic filter membrane, and obtain a test solution; The liquid to be tested is detected by liquid chromatography-tandem mass spectrometry.
8. The method for detecting PPDs and PPD-Qs in environmental water according to claim 7, It is characterized in that The detection conditions of the liquid chromatography-tandem mass spectrometry include: liquid chromatography conditions and mass spectrometry conditions; The liquid chromatography conditions include: The chromatographic column is C 18 column; Mobile phase A was 0.1% formic acid-water solution; mobile phase B was methanol; The gradient elution program is: from 0 to 2 min, excluding 0, the volume of the mobile phase A accounts for 30%, and the volume of the mobile phase B accounts for 70%; from 2 to 10 min, the volume of the mobile phase A accounts for 0% to 30%, and the volume of the mobile phase B accounts for 30% to 100%; The injection volume was 5 μL, the flow rate was 0.4 mL / min, and the column oven temperature was 30 °C; The mass spectrometry conditions include: Electrospray ion source positive ion mode; The ion spray voltage was 5.0 kV, the declustering voltage was 70 V, the ion source temperature was 500 °C, the curtain gas pressure was 25 psi, the collision gas pressure was medium, the spray gas pressure was 40 psi, and the auxiliary heating gas pressure was 45 psi.