A flame retardant dye for nylon and its preparation method and application

By combining the flame retardant monomer prepared by using Arbuzov reaction on nylon fabrics with acid dyes, the problem of poor flame retardant effect of nylon fabrics is solved, and efficient dyeing and flame retardant effects are achieved, while shortening the process and maintaining color fastness. The problems of cumbersome processes and energy consumption in the prior art have been solved.

CN118185342BActive Publication Date: 2024-11-29新兴际华(上海)工程科技研究院有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410242113.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-04
Publication Date
2024-11-29
Estimated Expiration
2044-03-04

AI Technical Summary

Technical Problem

The prior art is difficult to achieve efficient flame retardant effects on nylon fabrics. At the same time, the flame retardant process is complicated, energy consumption is high, and has an impact on color. There are no reports on flame retardant dyes for nylon.

Method used

The flame retardant monomer is prepared through the Arbuzov reaction, and the bromide and aniline derivatives are combined with the acid binding agent to form an anthraquinone acid dye, achieving covalent bonding with nylon fibers, and imparting flame retardant to the fabric. performance.

Benefits of technology

It realizes the efficient dyeing and flame retardant effect of nylon fabrics, shortens the process, saves energy, and firmly combines the dye with fibers to maintain good color fastness and flame retardant properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118185342B_ABST
    Figure CN118185342B_ABST
Patent Text Reader

Abstract

The present invention discloses a flame retardant dye for nylon and a preparation method and application thereof, and belongs to the technical field of textile printing and dyeing. The preparation method of the flame retardant dye for nylon of the present invention comprises the following steps: (1) preparing a flame retardant monomer by Arbuzov reaction of cyanuric chloride and trialkyl phosphite; (2) preparing an acid dye by Ullmann condensation reaction of bromoamic acid and aniline derivative; (3) reacting the acid dye with the flame retardant monomer to obtain the flame retardant acid dye. The present invention uses an anthraquinone acid dye suitable for nylon dyeing as a matrix, grafts a phosphorus-nitrogen triazine-based flame retardant with good flame retardant effect, and prepares an anthraquinone flame retardant dye, which can simultaneously give nylon better dyeing and flame retardant effects, and provides a new solution to the flame retardant problem of nylon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile printing and dyeing, and in particular to a flame retardant dye for nylon and a preparation method and application thereof. Background Art

[0002] Nylon is widely used in military and civilian fields due to its advantages such as good wear resistance, high breaking strength, good resilience and low density. However, the flammability of nylon and the droplets generated during combustion seriously threaten people's lives. The current methods for imparting flame retardancy to nylon fabrics are mainly divided into flame retardant modification of raw yarn and flame retardant finishing. Flame retardant modification of raw yarn lacks certain versatility in actual production due to problems such as harsh conditions and high costs; traditional flame retardant finishing is performed after the fabric is dyed, which has problems such as many processes, high energy consumption and easy impact on color.

[0003] Patent CN115466525A discloses a method for preparing a flame-retardant reactive dye and applies it to silk fabrics. Patent CN104830092A discloses a dye with flame-retardant properties and applies it to silk fabrics, but the dye cannot form a covalent bond with the fiber and has poor color fastness. Patent CN105670343A discloses a method for preparing a silicon-nitrogen polymerization flame-retardant dye, but it has not been applied to fabrics. There are currently no reports on flame-retardant dyes for nylon. Summary of the invention

[0004] The invention provides a flame retardant dye for nylon and a preparation method and application thereof. The flame retardant dye prepared by the invention can simultaneously meet the requirements of nylon dyeing and flame retardancy, shorten the operation process and save energy consumption.

[0005] The present invention provides a method for preparing a flame retardant dye for nylon, comprising the following steps:

[0006] (1) preparing a flame retardant monomer by Arbuzov reaction of cyanuric chloride and trialkyl phosphite;

[0007] (2) Preparation of acid dyes by Ullmann condensation reaction of bromoamic acid and aniline derivatives;

[0008] (3) The acid dye reacts with the flame retardant monomer to obtain the flame retardant acid dye.

[0009] The preparation method specifically comprises the following steps:

[0010] (1) dissolving cyanuric chloride in an organic solvent to obtain a cyanuric chloride solution; dissolving trialkyl phosphite in an organic solvent to obtain a trialkyl phosphite solution; dropwise adding the trialkyl phosphite solution to the cyanuric chloride solution to react, removing the organic solvent, and obtaining the flame retardant monomer;

[0011] (2) mixing bromoamic acid, an aniline derivative and water, then adding copper sulfate, reacting, removing water, and obtaining the acid dye;

[0012] (3) dissolving the acid dye and the acid binding agent in an organic solvent, then adding the flame retardant monomer to react, and removing the organic solvent to obtain the flame retardant acid dye.

[0013] In the above-mentioned preparation method, in step (1), the mass ratio of cyanuric chloride to trialkyl phosphite is 20:26-38;

[0014] In the cyanuric chloride solution, the mass ratio of cyanuric chloride to the organic solvent is 20:180-270;

[0015] In the trialkyl phosphite solution, the mass ratio of the trialkyl phosphite to the organic solvent is 36.04:100-150;

[0016] In step (2), the mass ratio of the bromoamic acid, the aniline derivative and the copper sulfate is 19:5 to 14:3 to 4;

[0017] The mass ratio of bromoamic acid to water is 19:80-100;

[0018] In step (3), the mass ratio of the flame retardant monomer to the acid dye is 11.93:10-14;

[0019] The mass ratio of the organic solvent to the acid dye is 50:10-15.

[0020] In the above preparation method, the organic solvent is toluene and / or chloroform;

[0021] The trialkyl phosphite is trimethyl phosphite or triethyl phosphite;

[0022] The aniline derivative is 4-butylaniline, aniline or 2,4,6-trimethylaniline;

[0023] The acid binding agent is triethylamine.

[0024] In the above-mentioned preparation method, in step (1), the reaction temperature is 80 to 100° C. and the reaction time is 10 to 14 hours;

[0025] Step (2) also includes a step of mixing bromoamic acid, aniline derivative and water and adjusting the pH value thereof to 8 to 9; specifically, sodium bicarbonate or sodium hydroxide is used to adjust the pH value;

[0026] In step (2), the reaction temperature is 75 to 85° C. and the reaction time is 6 to 8 hours;

[0027] In step (3), the reaction temperature is 80-85° C. and the reaction time is 8-12 hours.

[0028] In the above-mentioned preparation method, in step (3), the flame retardant monomer is dissolved in an organic solvent to form a solution, which is then added dropwise to the reaction system;

[0029] Specifically, the organic solvent is toluene and / or chloroform.

[0030] In the above-mentioned preparation method, in step (1), the organic solvent is removed by vacuum distillation; specifically, the vacuum distillation temperature is 70 to 80° C. and the pressure is -0.08 to -0.1 MPa;

[0031] In step (2), water is removed by vacuum distillation; specifically, the vacuum distillation temperature is 50 to 60° C. and the pressure is -0.08 to -0.1 MPa;

[0032] In step (3), the organic solvent is removed by vacuum distillation; specifically, the vacuum distillation temperature is 70 to 80° C. and the pressure is -0.08 to -0.1 MPa.

[0033] The present invention also provides a flame retardant dye for nylon prepared by the above preparation method.

[0034] The application of the above flame retardant dyes in nylon dyeing also falls within the protection scope of the present invention.

[0035] In the above application, the nylon is nylon 66.

[0036] The present invention has the following beneficial effects:

[0037] Anthraquinone acid dyes are common dye matrixes suitable for nylon dyeing. They have high light fastness. Under acidic conditions, dye anions can form ionic bonds with amino groups on the molecular chain of nylon fibers, firmly bond with the fibers, and give nylon better color fastness. Triazine and its derivatives are known as flame retardant materials and good carbonizing agents because they can absorb heat and generate non-flammable gases to dilute combustibles through decomposition. Phosphorus-containing functional groups can be converted into phosphoric acid and its derivatives through thermal decomposition in the condensed phase and form a protective carbon layer. The synergistic effect of phosphorus and nitrogen can promote the formation of a more durable and effective carbonization barrier on the combustion surface, and the generated phosphorus and nitrogen intermediates will accelerate the phosphorylation of the fiber, thereby enhancing the flame retardant effect of phosphorus.

[0038] The present invention uses an anthraquinone type acid dye suitable for nylon dyeing as a matrix and grafts a phosphorus-nitrogen triazine-based flame retardant with good flame retardant effect to prepare an anthraquinone type flame retardant dye, which can simultaneously give nylon good dyeing and flame retardant effects, and provides a new solution to the flame retardant problem of nylon. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 Dyeing process curve. DETAILED DESCRIPTION

[0040] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.

[0041] The experimental methods in the following examples are all conventional methods unless otherwise specified.

[0042] The quantitative tests in the following examples were all repeated three times, and the results were averaged.

[0043] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0044] Example 1

[0045] (1) Preparation of flame retardant monomers

[0046] 20 g of cyanuric chloride and 220 g of toluene are added to a reaction container with a stirrer and a condensation reflux device; the condensation reflux device and the stirrer are turned on, the temperature is adjusted to 60°C, and stirred at this temperature for 1 hour, 36.04 g of triethyl phosphite is dissolved in 120 g of toluene, and then added dropwise into the reactor, the temperature is increased to 90°C, and the reaction is kept at this temperature for 12 hours, the reaction liquid is filtered to remove insoluble matter, the filtrate temperature is adjusted to 70°C, the pressure to -0.1Mpa, and toluene is removed by reduced pressure distillation to obtain a flame retardant monomer.

[0047] (2) Preparation of acid dyes

[0048] 19 g of bromoamic acid, 8.16 g of 4-butylaniline and 90 g of water are added to a reaction container with a stirrer and a condensation reflux device; the condensation reflux device and the stirrer are turned on, the temperature is adjusted to 60° C., the mixture is stirred at this temperature for 1 hour, sodium bicarbonate is added to keep the pH value of the reaction solution at 8-9, and then 3 g of copper sulfate is added in three batches, the temperature is increased to 80° C., the mixture is kept warm for 6 hours at this temperature, the reaction solution is filtered to remove insoluble matter, the temperature of the filtrate is adjusted to 50° C., the pressure is adjusted to -0.1 MPa, and water is removed by reduced pressure distillation to obtain an acid dye.

[0049] (3) Preparation of flame retardant acid dyes

[0050] Take 12g of the acid dye prepared in the above step (2), 50g of toluene and 3.23g of triethylamine, add them to a reaction container with a stirrer and a condensation reflux device, turn on the condensation reflux device and the stirrer, stir for 1 hour, dissolve 11.93g of the flame retardant monomer prepared in the above step (1) in 30g of toluene, and then add it dropwise into the reaction container. After the dropwise addition is completed, turn on the heating device and adjust the temperature to 80°C. Keep the reaction at this temperature for 8 hours, filter the reaction solution to remove insoluble matter, adjust the filtrate temperature to 70°C and the pressure to -0.1Mpa, and remove toluene by reduced pressure distillation to obtain a flame retardant acid dye.

[0051] Example 2

[0052] (1) Preparation of flame retardant monomers

[0053] Same as Example 1.

[0054] (2) Preparation of acid dyes

[0055] 19g of bromoamic acid, 5.09g of aniline and 90g of water are added to a reaction container with a stirrer and a condensation reflux device; the condensation reflux device and the stirrer are turned on, the temperature is adjusted to 60°C, and the mixture is stirred at this temperature for 1 hour, and sodium bicarbonate is added to keep the pH value of the reaction solution at 8-9, and then 3g of copper sulfate is added in three batches, the temperature is increased to 80°C, and the mixture is kept warm for reaction at this temperature for 6 hours, the reaction solution is filtered to remove insoluble matter, the temperature of the filtrate is adjusted to 50°C, the pressure is adjusted to -0.1Mpa, and water is removed by reduced pressure distillation to obtain an acid dye.

[0056] (3) Preparation of flame retardant acid dyes

[0057] Take 10.5g of the acid dye prepared in the above step (2), 50g of toluene and 3.23g of triethylamine, add them to a reaction container with a stirrer and a condensation reflux device, turn on the condensation reflux device and the stirrer, stir for 1 hour, dissolve 11.93g of the flame retardant monomer prepared in the above step (1) in 30g of toluene, and then add it dropwise into the reaction container. After the dropwise addition is completed, turn on the heating device and adjust the temperature to 80°C. Keep the reaction at this temperature for 8 hours, filter the reaction solution to remove insoluble matter, adjust the filtrate temperature to 70°C and the pressure to -0.1Mpa, and remove toluene by reduced pressure distillation to obtain a flame retardant acid dye.

[0058] Example 3

[0059] (1) Preparation of flame retardant monomers

[0060] Same as Example 1.

[0061] (2) Preparation of acid dyes

[0062] 19 g of bromoamic acid, 7.39 g of 2,4,6-trimethylaniline and 90 g of water are added to a reaction container with a stirrer and a condensation reflux device; the condensation reflux device and the stirrer are turned on, the temperature is adjusted to 60° C., and the mixture is stirred at this temperature for 1 hour. At the same time, sodium bicarbonate is added to keep the pH value of the reaction solution at 8-9, and then 3 g of copper sulfate is added in three batches, the temperature is increased to 80° C., and the mixture is kept warm for 6 hours at this temperature. The reaction solution is filtered to remove insoluble matter, the temperature of the filtrate is adjusted to 50° C., the pressure is adjusted to -0.1 MPa, and water is removed by reduced pressure distillation to obtain an acid dye.

[0063] (3) 11.63 g of the acid dye prepared in step (2), 50 g of toluene and 3.23 g of triethylamine are added to a reaction vessel equipped with a stirrer and a condensation reflux device, the condensation reflux device and the stirrer are turned on, and the mixture is stirred for 1 hour. 11.93 g of the flame retardant monomer prepared in step (1) is dissolved in 30 g of toluene, and then the mixture is added dropwise to the reaction vessel. After the addition is completed, the heating device is turned on, the temperature is adjusted to 80° C., and the mixture is kept warm for reaction at this temperature for 8 hours. The reaction solution is filtered to remove insoluble matter, the filtrate temperature is adjusted to 70° C., the pressure is adjusted to -0.1 MPa, and the toluene is removed by reduced pressure distillation to obtain a flame retardant acid dye.

[0064] Comparative Example 1

[0065] 19g of bromoamic acid, 5.09g of aniline and 90g of water are added to a reaction container with a stirrer and a condensation reflux device; the condensation reflux device and the stirrer are turned on, the temperature is adjusted to 60°C, and the mixture is stirred at this temperature for 1 hour, and sodium bicarbonate is added to keep the pH value of the reaction solution at 8-9, and then 3g of copper sulfate is added in three batches, the temperature is increased to 80°C, and the mixture is kept warm for reaction at this temperature for 6 hours, the reaction solution is filtered to remove insoluble matter, the temperature of the filtrate is adjusted to 50°C, the pressure is adjusted to -0.1Mpa, and water is removed by reduced pressure distillation to obtain an acid dye.

[0066] The dyes synthesized in the above Examples 1-3 and Comparative Example 1 were used for dyeing nylon 66. The dye liquor formula was: dye 7% (owf), glacial acetic acid 5 mL / L, acid leveling agent HTW 1% (owf) purchased from Guangdong Honghao Chemical Co., Ltd. The dyeing process curve is shown in Figure 1 shown.

[0067] The dyed fabrics were subjected to flame retardant performance tests, and the limiting oxygen index of the fabrics was tested according to GB / T 5454-1997 "Textile Combustion Performance Test Oxygen Index Method", the smoldering time, afterflame time and damage length of the fabrics were tested according to GB / T 5455-1997 "Textile Combustion Performance Test Vertical Method", and the washing resistance test was carried out according to AATCC 124-1996 "Appearance of Fabrics after Multiple Home Washing". The flame retardant performance test results of the dyed fabrics are shown in Table 1.

[0068] Table 1 Dyed fabric performance test results

[0069]

[0070] As shown in Table 1, compared with the dyed fabric of Comparative Example 1, the flame retardant properties of the dyed fabric of the embodiment are significantly enhanced, which is specifically manifested in the improvement of the limiting oxygen index (LOI), the shortening of the afterflaming time, and the shortening of the damaged length. This is because the dye of the embodiment contains phosphate groups and triazine groups, which will promote the formation of the carbon layer during the combustion process, isolate the air, and terminate the combustion reaction. In addition, it will release non-combustible gas to reduce the combustible gas components in the environment, thereby achieving the effect of curbing combustion. After 10 times of washing, the dyed fabric still has a certain flame retardant property. This is mainly because in addition to the dye anion and the cation of the nylon terminal amino group being combined to form a salt bond by Coulomb force, there are also strong van der Waals forces and hydrogen bonds between the dye and the nylon molecules. Under the chemical and physical double cross-linking network, the flame retardant dye can be more firmly combined with the fiber. In summary, the flame retardant acid dye prepared by the present invention can give nylon fabrics a better flame retardant effect.

[0071] The dyed fabrics were subjected to color fastness grade tests. The color fastness grade of the fabrics to rubbing was tested in accordance with GB / T 3920-2008 “Textiles - Tests for Color Fastness - Color Fastness to Rubbing”, and the color fastness grade of the fabrics to washing was tested in accordance with GB / T 3921-2008 “Textiles - Tests for Color Fastness - Color Fastness to Washing with Soap”. The color fastness grade test results of the dyed fabrics are shown in Table 2.

[0072] Table 2 Test results of color fastness grades of dyed fabrics

[0073]

[0074] It can be seen from Table 2 that, compared with the dyed fabric of the comparative example, the color fastness grade of the dyed fabric of the embodiment has a certain degree of decrease in some color fastness grades. This may be because the flame retardant group grafted in the acid dye affects the stability of the dye, and then affects the fixation of the dye on the fiber. However, it can be found that the decrease in the color fastness grades of each embodiment is not large, basically about half a grade, which shows that the flame retardant acid dye prepared by the present invention has good dyeing affinity for nylon.

[0075] In summary, the flame retardant acid dye prepared by the present invention can not only impart good flame retardant effect to nylon fabric, but also has strong dyeing affinity to nylon fabric.

Claims

1. A method for preparing a flame retardant dye for nylon, comprising the following steps: (1) Preparation of flame retardant monomers from cyanuric chloride and trialkyl phosphite by Arbuzov reaction; (2) Preparation of acid dyes from bromoamic acid and aniline derivatives via Ullmann condensation reaction; (3) The acid dye reacts with the flame retardant monomer to obtain the flame retardant dye for nylon.

2. The preparation method according to claim 1, Features: The preparation method comprises the following steps: (1) dissolving cyanuric chloride in an organic solvent to obtain a cyanuric chloride solution; dissolving trialkyl phosphite in an organic solvent to obtain a trialkyl phosphite solution; dropping the trialkyl phosphite solution into the cyanuric chloride solution to react, removing the organic solvent, and obtaining the flame retardant monomer; (2) mixing bromoamic acid, an aniline derivative and water, then adding copper sulfate, reacting, removing water, and obtaining the acid dye; (3) The acid dye and the acid binding agent are dissolved in an organic solvent, and then the flame retardant monomer is added to react, and the organic solvent is removed to obtain the flame retardant dye for nylon.

3. The preparation method according to claim 2, Features: In step (1), the mass ratio of cyanuric chloride to trialkyl phosphite is 20:26-38; In the cyanuric chloride solution, the mass ratio of cyanuric chloride to the organic solvent is 20:180-270; In the trialkyl phosphite solution, the mass ratio of the trialkyl phosphite to the organic solvent is 36.04:100-150; In step (2), the mass ratio of bromoamic acid, aniline derivative and copper sulfate is 19:5-14:3-4; The mass ratio of bromoamic acid to water is 19:80-100; In step (3), the mass ratio of the flame retardant monomer to the acid dye is 11.93:10-14; The mass ratio of the organic solvent to the acid dye is 50:10-15.

4. The preparation method according to claim 2 or 3, Features: The organic solvent is toluene and / or chloroform; The trialkyl phosphite is trimethyl phosphite or triethyl phosphite; The aniline derivative is 4-butylaniline, aniline or 2,4,6-trimethylaniline; The acid binding agent is triethylamine.

5. The preparation method according to claim 2 or 3, Features: In step (1), the reaction temperature is 80-100°C and the reaction time is 10-14 hours; Step (2) further comprises the step of mixing bromoamic acid, aniline derivative and water and adjusting the pH value thereof to 8 to 9; In step (2), the reaction temperature is 75-85°C and the reaction time is 6-8 hours; In step (3), the reaction temperature is 80-85° C. and the reaction time is 8-12 hours.

6. The preparation method according to claim 5, Features: In step (2), sodium bicarbonate or sodium hydroxide is used to adjust the pH value.

7. The preparation method according to claim 2 or 3, Features: In step (3), the flame retardant monomer is dissolved in an organic solvent to form a solution, which is then added dropwise to the reaction system.

8. The preparation method according to claim 7, Features: The organic solvent in which the flame retardant monomer is dissolved is toluene and / or chloroform.

9. The preparation method according to claim 2 or 3, Features: In step (1), the organic solvent is removed by distillation under reduced pressure; In step (2), water is removed by distillation under reduced pressure; In step (3), the organic solvent is removed by distillation under reduced pressure.

10. The preparation method according to claim 9, Features: In step (1), the temperature of the reduced pressure distillation is 70-80°C and the pressure is -0.08--0.1Mpa; In step (2), the temperature of the reduced pressure distillation is 50-60°C and the pressure is -0.08--0.1Mpa; In step (3), the temperature of the reduced pressure distillation is 70-80°C and the pressure is -0.08--0.1 MPa.

11. The flame retardant dye for nylon prepared by the preparation method according to any one of claims 1 to 10.

12. Use of the flame retardant dye according to claim 11 in nylon dyeing.

13. The use according to claim 12, Features: The nylon is nylon 66.

Citation Information

Patent Citations

  • Preparation method and applications of fire retardation dye

    CN104830092A

  • Silicon nitrogen containing flame retardant type polymer dye and preparation method thereof

    CN105670343A

  • Synthesis process of light-resistant and ultraviolet-resistant polyamide fiber

    CN116356447A