Polycyclic compound and preparation method, use, electrolyte and battery thereof
By using polycyclic compounds containing low metal ion content in lithium battery electrolyte, the synthesis process is optimized, the problem of impurity metal ions is solved, the electrochemical performance and cycle stability of the battery are improved, and more efficient electricity is achieved Chemical properties and longer battery life.
Patent Information
- Application Number
- CN202410758086.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-06-13
AI Technical Summary
The commonly used polycyclic sulfate additives in existing lithium battery electrolytes are prone to introduce impurity metal ions during use, resulting in a decline in the electrochemical performance of the battery. It is difficult to effectively control the impurity content in its synthesis process, which affects the cycle stability and electricity of the battery. Chemical properties.
Using a polycyclic compound, which includes a specific sulfate structure and metal ion content ≤10ppm, by optimizing the transesterification and condensation reaction process, combined with azeotropic treatment of nonaqueous solvents, remove impurity metal ions and chloride ions, improve product purity and Selective.
It effectively reduces the content of impurity metal ions in the electrolyte, improves the electrochemical performance of the battery, extends the cycle stability and service life of the battery, and enhances the battery's high and low temperature resistance.
Smart Images

Figure CN118307531B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of batteries, and specifically, relates to polycyclic compounds and preparation methods, uses, electrolytes and batteries thereof. Background Art
[0002] With the rapid development of electronic equipment, electric vehicles, smart homes, power tools, smart transportation and other markets, the demand for batteries is also increasing. Taking lithium-ion batteries as an example, they are widely used in consumer electronics, energy storage and power batteries, smart homes and other fields because of their advantages such as high specific energy, long cycle life and low self-discharge. Usually, the battery includes a positive electrode, a negative electrode, a separator and an electrolyte. The electrolyte usually includes a solvent, an electrolyte lithium salt and an electrolyte additive. The performance of the battery can be improved by adding electrolyte additives to the electrolyte. The selection of appropriate additives has an important influence on the electrochemical performance of the battery. Summary of the invention
[0003] The present application aims to solve one of the related technical problems to a certain extent.
[0004] Additives are an important component of the electrolyte, and suitable additives can significantly improve the electrochemical performance of the battery. The inventors found that applying the compound shown in Formula I as an additive to the electrolyte of a lithium battery has a good improvement effect on the electrochemical performance of the battery. The inventors analyzed that the reason may be because: the compound shown in Formula I is easy to obtain electrons and be reduced, resulting in the breakage of the SO single bond, and the three O atoms in O, S=O and S=O on another cyclic sulfate group in the transition state formed after the break can form a claw-type spatial structure, which is easy to capture metal ions and form a cage complex, thereby stabilizing the already dissolved transition metal, reducing the catalytic decomposition side reaction of the transition metal on the SEI film, and inhibiting the negative impact caused by the deposition of the transition metal in the form of a single substance after the negative electrode is reduced. But at the same time, the inventors realized that the transition metal dissolved in the positive electrode material is not in the electrolyte at the beginning, but slowly begins to dissolve with the use of the battery. If metal ions are introduced into the electrolyte due to the use of additives, these free metal ions will preferentially form complexes with the compound shown in Formula I relative to the transition metal gradually dissolved from the positive electrode during the charge and discharge process, reducing the complexing sites and stabilizing effects of the compound shown in Formula I on the transition metal ions dissolved from the positive electrode, weakening the ability of Formula 1 to inhibit the deposition of transition metal elements at the negative electrode, and is not conducive to the full play of the electrochemical performance of the battery. In order to solve this problem, the initial inventors considered increasing the amount of Formula 1 added to the electrolyte, but found that excessive addition of Formula 1 would lead to an increase in Li consumption, resulting in problems of reduced first effect and reduced capacity. After repeated experiments and thinking, it was finally found that controlling the residual metal ion content in the compound shown in Formula 1 is the key to improving its application performance.
[0005] The existing synthesis process of the compound shown in Formula I generally has the problem of containing a large number of impurity ions in the product. For example, there is currently a method of obtaining a target product by transesterifying a hexavalent alcohol and a carbonate under a catalyst, and then adding sulfonyl chloride for recrystallization. Most of the methods use hypochlorous acid (salt) as an oxidant. Due to the limitation of the use of alkaline catalysts and oxidants, it is easy to introduce more metal ions into the synthesized target product. For example, sodium hydroxide, potassium hydroxide, potassium carbonate, sodium carbonate, etc. are used as alkaline catalysts, which will introduce sodium ions or potassium ions. For example, if sodium hypochlorite is used as an oxidant, it is very easy to introduce more sodium ions into the synthesized target product, and the removal effect of sodium ions by using ordinary water washing process is not ideal.
[0006] In view of this, the first object of the present application is to provide a polycyclic sulfate product, in which the metal ion content is low, below 10 ppm, so as to reduce the adverse effects of impure metal ions on battery performance while improving battery performance.
[0007] In the first aspect of the present application, a polycyclic compound is provided, comprising: a compound represented by formula I and a metal ion, wherein the content of the metal ion is ≤10 ppm based on the mass of the polycyclic compound,
[0008] ,
[0009] In Formula I, R 1 , R 2 Each is independently any one of H, F, alkyl and fluoroalkyl.
[0010] The above-mentioned polycyclic compound of the present application has the following beneficial effects: the compound shown in Formula I can be used as an electrolyte additive in the electrolyte, which can improve the electrochemical performance of the battery. Specifically, it is not only conducive to forming a dense CEI film at the positive electrode and a dense SEI film at the negative electrode, but also forms a small amount of inorganic salts in the CEI film formed by decomposition at the positive electrode (taking lithium battery as an example, the inorganic salts include Li 2 SO 4 and / or Li 2 O), improve the rigidity and flexibility of the positive electrode interface layer, inhibit the decomposition of the electrolyte, improve the stability of the positive electrode interface film, and the CEI film formed by the compound shown in formula I can also reduce the electrochemical impedance of the positive electrode and accelerate the active ions (such as Li +) transmission rate, and at the same time help to form a more stable electrode-electrolyte interface, reduce the internal resistance and interface reaction of the battery, and play a role in protecting the positive electrode. In addition, it can also inhibit the dissolution of transition metal ions in the active material of the positive electrode plate, reduce the cycle capacity attenuation of the battery, and improve the cycle stability; furthermore, the compound shown in Formula I will generate lithium carbonate in the SEI film formed at the negative electrode, and lithium carbonate helps to improve the film formation uniformity and stability of the SEI film. In addition, the compound shown in Formula I is easy to obtain electrons and be reduced to cause the SO single bond to break, and the three O atoms in O, S=O and S=O on another cyclic sulfate group in the transition state formed after the break can form a claw-type space structure, which is easy to capture metal ions to form a cage complex, thereby stabilizing the impurity metal ions in the electrolyte and the dissolved transition metal ions, reducing the catalytic decomposition side reaction of the transition metal on the SEI film, and inhibiting the negative impact caused by the deposition of the transition metal in the form of a single substance after the negative electrode is reduced; furthermore, the compound shown in Formula I has a low impedance, which is also beneficial to reducing the battery impedance. However, based on the conventional synthesis process of the compound shown in Formula I, impurities are inevitably present, among which impurity metal ions are directly introduced into the electrolyte along with the compound shown in Formula I. Compared with the transition metal elements that slowly begin to dissolve with the use of the battery, the impurity metal ions introduced into the electrolyte along with the compound shown in Formula I are not only easier to combine with the compound shown in Formula I, but also, as the initial component in the electrolyte, they also have a greater time advantage in combining with the compound shown in Formula I, thereby not only reducing the electrochemical stability of the battery, but also affecting the ability of the compound shown in Formula I to inhibit the deposition of the dissolved transition metal ions on the negative electrode surface, reducing the improvement effect of the compound shown in Formula I on the electrochemical performance of the battery.
[0011] In the present application, by using a polycyclic compound containing a compound represented by formula I and having a metal ion content of ≤10ppm as an additive in an electrolyte, the problem that the improvement effect of the compound represented by formula I on the electrochemical performance of the battery is easily reduced due to the presence of impurity metal ions, and the problem that the complexing sites and stabilizing effect of the compound represented by formula I on the dissolved transition metal ions are reduced due to the high content of impurity metal ions, can be effectively reduced, thereby effectively improving the improvement effect of the polycyclic compound on the electrochemical performance of the battery.
[0012] In some embodiments, R 1 , R 2 Each independently represents any one of H, F and fluoromethyl.
[0013] In some embodiments, based on the mass of the polycyclic compound, the content of the compound represented by Formula I is ≥ 99 wt %, thereby further improving the effect of the polycyclic compound on the electrochemical performance of the battery.
[0014] In some embodiments, based on the mass of the polycyclic compound, the content of the metal ions is ≤5 ppm, thereby further reducing the problem of the reduced effect of the compound represented by Formula I on the electrochemical performance of the battery due to the presence of impurity ions.
[0015] In some embodiments, the polycyclic compound further comprises chloride ions, and the content of the chloride ions is ≤10 ppm based on the mass of the polycyclic compound. This can improve the effect of the compound shown in Formula I on inhibiting the dissolution of transition metal ions in the active material of the positive electrode.
[0016] In some embodiments, the polycyclic compound further comprises: chlorine-containing organic matter, and the total content of the chlorine-containing organic matter is ≤300 ppm based on the mass of the polycyclic compound, thereby further reducing the chloride ion content that may be generated after the polycyclic compound is used in the electrolyte.
[0017] In some embodiments, the polycyclic compound further comprises: other organic matter, wherein the other organic matter is selected from one or more of the following six compounds:
[0018] , , , , , , based on the mass of the polycyclic compound, the total content of the other organic substances is ≤500ppm. Thus, the purity of the compound represented by Formula I can be further improved.
[0019] In some embodiments, based on the mass of the polycyclic compound, the content of the chloride ions is ≤5 ppm. This can further improve the problem of the compound shown in Formula I in inhibiting the dissolution of transition metal ions in the positive electrode active material.
[0020] In some embodiments, the chlorine-containing organic compound includes chlorine-containing organic compound without cyclic sulfate groups and cyclic carbonate groups, chlorine-containing organic compound containing only cyclic carbonate groups, chlorine-containing organic compound containing only cyclic sulfate groups, and chlorine-containing organic compound containing 1 to 2 cyclic carbonate groups and 1 cyclic sulfate group.
[0021] In some embodiments, based on the mass of the polycyclic compound, the total content of the chlorine-containing organic matter, the metal ions and the chloride ions is ≤150 ppm. This can further improve the problem that the improvement effect of the compound represented by Formula I on the electrochemical performance of the battery is reduced due to the presence of impurities.
[0022] In some embodiments, based on the mass of the polycyclic compound, the total content of the other organic matter is ≤200 ppm. This can further solve the problem of decreased purity of the compound represented by Formula I and the effect of improving the electrochemical performance of the battery.
[0023] In some embodiments, based on the mass of the polycyclic compound, the content of the compound represented by Formula I is ≥ 99.9 wt %, thereby further improving the effect of the polycyclic compound on the electrochemical performance of the battery.
[0024] In some embodiments, based on the mass of the polycyclic compound, the total content of the chlorine-containing organic matter, the metal ions and the chloride ions is ≤100 ppm. This can further reduce the problem of the reduced effect of the compound represented by Formula I on the electrochemical performance of the battery due to the presence of impurity ions.
[0025] In some embodiments, based on the mass of the polycyclic compound, the content of the metal ions is ≤1 ppm, and the content of the chloride ions is ≤1 ppm. This can further reduce the problem of the reduced effect of the compound represented by Formula I on the electrochemical performance of the battery due to the presence of impurity ions.
[0026] In some embodiments, the chlorine-containing organic impurities include , , One or more of, based on the mass of the polycyclic compound, , , The total content of is ≤50ppm. This can further improve the problem that the improvement effect of the compound represented by formula I on the electrochemical performance of the battery due to the presence of impurities is reduced.
[0027] In some embodiments, the compound represented by Formula I comprises: The polycyclic compound has good stability, which is conducive to further improving the effect of the polycyclic compound on the electrochemical performance of the battery.
[0028] Based on the same inventive concept as the first aspect of the present application, it is desired to obtain a polycyclic compound product containing a compound shown in formula I and a metal ion content of ≤10ppm. Based on this purpose, a method for preparing polycyclic compounds in the second aspect of the present application was developed.
[0029] In a second aspect of the present application, a method for preparing a polycyclic compound is provided, comprising:
[0030] (1) mixing a hexahydric alcohol, a monohydric alcohol, a carbonate and an alkaline catalyst to carry out an ester exchange reaction to obtain a compound 1;
[0031] (2) dissolving the compound 1 in a solvent and subjecting the compound to a condensation reaction with thionyl chloride;
[0032] (3) mixing the condensation reaction product with an aqueous sodium hypochlorite solution and subjecting it to oxidation treatment to obtain a reaction product containing compound 2;
[0033] (4) subjecting the reaction product obtained in step (3) to azeotropic treatment with a non-aqueous solvent;
[0034] (5) filtering the product after the azeotropic treatment, and performing a desolvation treatment on the liquid phase product to obtain a compound represented by formula I,
[0035] Wherein, the compound represented by Formula I is soluble in the non-aqueous solvent and NaCl is insoluble in the non-aqueous solvent, and the structural formulas of the hexavalent alcohol, the compound 1, and the compound 2 are respectively:
[0036] , , , R 1 , R 2 Each is independently any one of H, F, alkyl and fluoroalkyl.
[0037] The above-mentioned method for preparing polycyclic compounds in the present application has the following beneficial effects: during the preparation process, the use of alkaline catalysts and sodium hypochlorite will inevitably introduce metal ions. In addition, the use of thionyl chloride and sodium hypochlorite will also introduce chloride ions. Impurity metal ions and chloride ions will be directly introduced into the electrolyte along with the compound shown in Formula I. Free chloride ions are likely to cause the dissolution of transition metal ions in the active material of the positive electrode plate. Moreover, relative to the transition metal elements that slowly begin to dissolve with the use of the battery, the impurity metal ions introduced into the electrolyte along with the compound shown in Formula I are not only easier to combine with the compound shown in Formula I, but also, as the initial component in the electrolyte, they also have a greater time advantage in combining with the compound shown in Formula I, thereby not only reducing the electrochemical stability of the battery, but also affecting the ability of the polycyclic compound described in Formula I to inhibit the deposition of the dissolved transition metal ions on the surface of the negative electrode. Ability to reduce the improvement effect of the compound shown in Formula I on the electrochemical performance of the battery. In the present application, the reaction product obtained by oxidation treatment is first subjected to azeotropic treatment with a non-aqueous solvent to remove water from the product after oxidation treatment. Since there is a certain matching relationship between the impurity metal cations and the chloride ions existing as anions, as the water content gradually decreases, the impurity metal cations and chloride ions that match each other combine to form inorganic salts (such as NaCl). Since the inorganic salt cannot be dissolved in the selected non-aqueous solvent, it appears in the non-aqueous solvent in the form of a precipitate, while the polycyclic compound shown in the target product Formula 1 is still dissolved in the non-aqueous solvent. Therefore, the inorganic salt (such as NaCl) can be removed by filtration. As a result, not only the residual metal ion content in the target product shown in Formula I can be greatly reduced, such as the metal ion content can be reduced to less than a few ppm, but also the chloride ion content can be reduced.
[0038] In summary, the method not only has high selectivity and high conversion rate for the compound shown in formula I, but also has low impurity content of metal ions and chloride ions, which is conducive to obtaining the target product shown in formula I with a metal ion content of ≤10ppm. The target product shown in formula I is used in the electrolyte to effectively reduce the content of impurity metal ions and chloride ions in the electrolyte, reduce the risk of dissolution of transition metal ions in the positive electrode active material caused by the presence of chloride ions, and improve the problem of reducing the complexing site and stabilizing effect of the compound shown in formula I on the already dissolved transition metal ions due to the high content of impurity metal ions, thereby effectively improving the problem of reduced improvement effect of the compound shown in formula I on the electrochemical performance of the battery due to the presence of impurities, and improving the improvement effect of the obtained polycyclic compound on the electrochemical performance of the battery.
[0039] In some embodiments, the transesterification reaction is carried out under heating and pressurization conditions. Further preferably, the temperature of the transesterification reaction is 65-100° C., and the pressure is controlled to be less than 2.5 MPa, thereby further improving the selectivity of compound 1 and the conversion efficiency of compound 1 in the transesterification reaction. In the transesterification reaction, the reaction activity of the hydroxyl groups at the terminal positions (1 and 6) of the hexamethylene alcohol is suppressed by using a monohydric alcohol and controlling the pressure to be less than 2.5 MPa, and then the reaction temperature is raised to 65-100°C, which is higher than the boiling point of the monohydric alcohol (methanol has the lowest boiling point of 65°C among the monohydric alcohols used in this application), to increase the reaction activity of the hydroxyl groups at the middle positions (2, 3, 4, and 5) of the hexamethylene alcohol, so that the activity of the hydroxyl groups at the middle positions of the hexamethylene alcohol is much higher than that of the hydroxyl groups at the terminal positions. At the same time, under the conditions of heating and pressurization, compared with the products generated by the reaction of the hydroxyl groups at the 2 and 3 positions and the products generated by the reaction of the hydroxyl groups at the 4 and 5 positions, the products generated by the reaction of the hydroxyl groups at the 3 and 4 positions (i.e., compound 1) have good symmetry and better stability. Therefore, under these conditions, the selectivity for compound 1 and the conversion efficiency of compound 1 in the transesterification reaction can be improved, and an intermediate product having compound 1 can be obtained with a high conversion rate and high selectivity. This can effectively reduce the residual hexamethylene alcohol content in the transesterification reaction product on the one hand, and reduce impurities on the other hand. , The content of the product is beneficial to further reduce the impurities that may be generated by the residual hexavalent alcohol or impurities participating in the subsequent condensation reaction and oxidation reaction. , , , , , The content.
[0040] In the present application, since monohydric alcohol is used as the reaction raw material, it is limited by the boiling point of the monohydric alcohol (methanol has the lowest boiling point of 65°C among the monohydric alcohols used in the present application). Therefore, under normal pressure or negative pressure conditions, in the reaction system of the present application, the monohydric alcohol will evaporate and reflux when the temperature reaches its boiling point. During the reflux process, the solution temperature and the steam temperature will continuously adjust to each other and eventually reach a dynamic equilibrium. The inventors found that under this dynamic equilibrium, the temperature of the reaction system will stabilize at around the boiling point of the monohydric alcohol, making it difficult to increase the temperature of the reaction system, thereby limiting the reaction rate. The pressurization method of the present application can not only cooperate with the monohydric alcohol to improve the selectivity of the reaction, but also increase the boiling point of the monohydric alcohol, so that the reaction temperature can also be appropriately increased, thereby ultimately increasing the reaction rate.
[0041] In some embodiments, the temperature of the transesterification reaction is 70-90°C, the pressure is 0.5-2.2 MPa, and the time is 0.5-6 h; more preferably, the temperature of the transesterification reaction is 75-85°C, and the pressure is 1-2 MPa. In this way, a high raw material conversion rate and a suitable transesterification reaction rate can be taken into account, thereby obtaining compound 1 with high selectivity and yield and low impurity content.
[0042] In some embodiments, the molar ratio of the carbonate to the hexahydric alcohol is 3: 1 to 5: 1. This is beneficial for obtaining a suitable transesterification reaction rate and a high conversion rate, and is also beneficial for reducing the impurity content in the final product.
[0043] In the present application, the monohydric alcohol is used as a solvent on the one hand, and its addition amount is generally required to completely dissolve the reaction raw materials mannitol and carbonate. Under normal circumstances, the molar ratio of the monohydric alcohol to the hexahydric alcohol is greater than or equal to 10 to meet the dissolution requirements. The prior art mentions that in order to dissolve the reaction raw materials, it does not matter if the solvent methanol is added excessively, but in fact, the inventors have found that the content of the monohydric alcohol also affects the selectivity of the transesterification reaction. If the content of the monohydric alcohol is too high (the molar ratio of the monohydric alcohol to the hexahydric alcohol is greater than 20:1), the selectivity of the transesterification reaction will be reduced to a certain extent. Based on this, in some embodiments, the molar ratio of the monohydric alcohol to the hexahydric alcohol is 10:1~20:1, preferably 12:1~18:1, and more preferably 14:1~16:1. This is conducive to obtaining a suitable transesterification reaction rate and a high conversion rate, and is also conducive to reducing the impurity content in the final product.
[0044] In some embodiments, based on the mass of the hexavalent alcohol, the amount of the alkaline catalyst is 0.01-5wt%, optionally 0.01-1wt%, and more preferably 0.02-0.1wt%. This is conducive to the smooth progress of the transesterification reaction and can also reduce the risk of increasing the amount of thionyl chloride used in the subsequent condensation reaction due to excessive use of the alkaline catalyst and generating more sulfur dioxide.
[0045] In some embodiments, the hexavalent alcohol includes one or more of mannitol, sorbitol, and galactitol.
[0046] In some embodiments, the carbonate includes one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and diphenyl carbonate.
[0047] In some embodiments, the monohydric alcohol includes one or more of methanol, ethanol, propanol, isopropanol, butanol, and tert-butanol.
[0048] In some embodiments, the alkaline catalyst includes one or more of sodium hydroxide, potassium hydroxide, potassium carbonate, sodium carbonate, lithium carbonate, sodium methoxide, sodium ethoxide, sodium tert-butoxide, potassium tert-butoxide, triethylamine, and pyridine.
[0049] In some embodiments, after the transesterification reaction is completed, the process further comprises: decompression treatment to remove low-boiling point components, thereby further improving the purity of the compound represented by Formula I and reducing the impurity content.
[0050] In some embodiments, in step (2), after the condensation reaction is completed, the step further includes: reflux deacidification treatment, thereby reducing the residual HCl generated by the condensation reaction.
[0051] In some embodiments, in step (2), the temperature of the reflux deacidification treatment is 40-80° C., and / or the time of the reflux deacidification treatment is 10-50 min. Meeting the reflux deacidification treatment conditions is conducive to further reducing the residual HCl generated by the condensation reaction.
[0052] In some embodiments, in step (2), the chloride ion content in the condensation reaction product after the reflux deacidification treatment is 100-200 ppm. Since the molar ratio of chloride ions to sodium ions in sodium hypochlorite is 1:1, and after the post-treatment of step (4) and step (5), when the chloride ions and metal ions are precipitated and removed in the form of chloride (such as sodium chloride), the chloride ions and metal ions are also removed in a 1:1 relationship. However, the alkaline catalyst in step (1) and the sodium hypochlorite in step (3) will introduce metal ions, that is, the actual content of metal ions will be higher than the content of chloride ions introduced in step (3). Therefore, the chloride ion content in the condensation reaction product is controlled between 100 and 200 ppm by reflux deacidification treatment, which is not only conducive to saving the time used for deacidification, but also the chloride ions remaining in this step can be matched with the metal ions in steps (4) and step (5), and finally removed simultaneously in the form of chloride (such as sodium chloride or potassium chloride), which is more conducive to reducing the content of metal ions and chloride ions at the same time.
[0053] In some embodiments, in step (2), after dissolving compound 1 in a solvent, thionyl chloride is added dropwise to carry out the condensation reaction. This can better inhibit impurities. Generation of.
[0054] In some embodiments, in step (2), the condensation reaction temperature is 20-100° C. and the reaction time is 1-4 hours, thereby achieving a good balance between reaction efficiency and purity of the final product.
[0055] In some embodiments, in step (2), the molar ratio of the compound 1 to the thionyl chloride is 1:(2-3), and the thionyl chloride is added for 0.5-2 hours. This can take into account the reaction rate, improve the purity of the compound 2 and the final product, and reduce the impurity content.
[0056] In some embodiments, in step (2), the solvent is a solvent that can be azeotroped with water. In this way, after the condensation reaction is completed, there is no need to perform a solvent removal step, and the solvent can directly participate in the reaction of step (3), so that the reaction product obtained in step (3) contains water and solvent, and no other solvent needs to be added in step (4).
[0057] In some embodiments, in step (2), the solvent is a solvent that cannot be azeotropic with water. In this case, after the condensation reaction is completed, a solvent removal step is further included to remove the solvent in step (2). At the same time, before the oxidation treatment in step (3), a non-aqueous solvent is added to dissolve the condensation reaction product to facilitate the oxidation treatment with the sodium hypochlorite aqueous solution. The oxidation product after the oxidation treatment contains water and non-aqueous solvent, and an azeotropic reaction can be carried out by heating. The non-aqueous solvent includes one or more of chloroform, toluene, alcohol solvents, ether solvents, and ester solvents. The temperature for the azeotropic reaction and the amount of addition are selected according to the characteristics of each solvent, and the amount of addition is based on the ability to dissolve the product of the condensation reaction. For example, ether, the azeotropic temperature is 34~35℃, and the addition amount is 20~25 times the mass of the hexamethylene alcohol; acetonitrile, the azeotropic temperature is 76~82℃, and the addition amount is 8~10 times the mass of the hexamethylene alcohol; ethyl acetate, the azeotropic temperature is 70~77℃, and the addition amount is 12~15 times the mass of the hexamethylene alcohol; toluene, the azeotropic temperature is 85~110℃, and the addition amount is 19~22 times the mass of the hexamethylene alcohol; tetrahydrofuran, the azeotropic temperature is 63~65℃, and the addition amount is 10~15 times the mass of the hexamethylene alcohol; dichloroethane, the azeotropic temperature is 72~84℃, and the addition amount is 19~23 times the mass of the hexamethylene alcohol; chloroform, the azeotropic temperature is 56~62℃, and the addition amount is 18~20 times the mass of the hexamethylene alcohol; dimethyl carbonate, the azeotropic temperature is 85~90℃, and the addition amount is 15~20 times the mass of the hexamethylene alcohol. This helps to further reduce the content of chloride ions and metal ion impurities in the target product shown in Formula I.
[0058] In some embodiments, in step (2), the solvent includes one or more of an ether solvent, N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, and an ester solvent.
[0059] In some embodiments, in step (3), the molar ratio of the compound 2 to the sodium hypochlorite is 1:(2-2.5), which is beneficial to improve the yield and purity of the target product shown in Formula I.
[0060] In some embodiments, in step (5), the desolvation treatment comprises one or more of distillation, extraction, and chromatography.
[0061] In the third aspect of the present application, a polycyclic compound prepared by the method for preparing a polycyclic compound is proposed, wherein the prepared polycyclic compound comprises: a compound shown in Formula I and a metal ion, wherein the content of the metal ion is ≤10ppm based on the mass of the polycyclic compound. The characteristics and effects described for the preparation of the polycyclic compound are also applicable to the polycyclic compound, and will not be repeated here.
[0062] In the fourth aspect of the present application, a use of the above-mentioned polycyclic compound and the above-mentioned method for preparing the polycyclic compound in the field of electrolyte and battery is proposed.
[0063] In a fifth aspect of the present application, an electrolyte is provided, comprising: an electrolyte additive, wherein the electrolyte additive comprises the above-mentioned polycyclic compound, or a polycyclic compound prepared by the above-mentioned method for preparing a polycyclic compound. The electrolyte is used in a battery to improve the electrochemical performance of the battery.
[0064] In some embodiments, based on the total mass of the electrolyte, the content of the electrolyte additive is 0.1-5 wt %.
[0065] In a sixth aspect of the present application, a battery is proposed, comprising: the above-mentioned electrolyte.
[0066] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0068] Figure 1 The present invention is a flow chart of preparing polycyclic compounds according to one embodiment of the present application.
[0069] Figure 2 This is the H NMR spectrum of the final product obtained according to Example 1 of the present application.
[0070] Figure 3 This is the NMR carbon spectrum of the final product obtained according to Example 1 of the present application. DETAILED DESCRIPTION
[0071] The embodiments of the present application are described in detail below, which are intended to be used to explain the present application but should not be construed as limiting the present application.
[0072] In the first aspect of the present application, a polycyclic compound is provided, comprising: a compound represented by formula I and a metal ion, wherein the content of the metal ion is ≤10 ppm based on the mass of the polycyclic compound,
[0073] ,
[0074] In Formula I, R 1 , R 2 Each is independently any one of H, F, alkyl and fluoroalkyl.
[0075] It should be noted that R 1 , R 2 can be the same or different; the alkyl group and the fluoroalkyl group can be independently an alkyl group and a fluoroalkyl group with 1 to 10 carbon atoms, and can be an alkyl group and a fluoroalkyl group with 1 to 10 carbon atoms, and the fluoroalkyl group can be an alkyl group partially or completely substituted with fluorine. Exemplarily, based on the mass of the polycyclic compound, the content of metal ions can be ≤10ppm, 9ppm, 8ppm, 7ppm, 6ppm, 5ppm, 4ppm, 3ppm, 2ppm, 1ppm, and the like.
[0076] The compound shown in Formula I can be used as an electrolyte additive in the electrolyte, which can improve the electrochemical performance of the battery. Specifically, it is not only conducive to forming a dense CEI film at the positive electrode and a dense SEI film at the negative electrode, but also forms a small amount of inorganic salts in the CEI film formed by decomposition at the positive electrode (taking lithium batteries as an example, the inorganic salts include Li 2 SO 4 and / or Li 2 O), improve the rigidity and flexibility of the positive electrode interface layer, inhibit the decomposition of the electrolyte, improve the stability of the positive electrode interface film, and the CEI film formed by the compound shown in formula I can also reduce the electrochemical impedance of the positive electrode and accelerate the active ions (such as Li +) transmission rate, and at the same time help to form a more stable electrode-electrolyte interface, reduce the internal resistance and interface reaction of the battery, and play a role in protecting the positive electrode. In addition, it can also inhibit the dissolution of transition metal ions in the active material of the positive electrode plate, reduce the cycle capacity attenuation of the battery, and improve the cycle stability; furthermore, the compound shown in Formula I will generate lithium carbonate in the SEI film formed at the negative electrode, and lithium carbonate helps to improve the film formation uniformity and stability of the SEI film. In addition, the compound shown in Formula I is easy to obtain electrons and be reduced to cause the SO single bond to break, and the three O atoms in O, S=O and S=O on another cyclic sulfate group in the transition state formed after the break can form a claw-type space structure, which is easy to capture metal ions to form a cage complex, thereby stabilizing the impurity metal ions in the electrolyte and the dissolved transition metal ions, reducing the catalytic decomposition side reaction of the transition metal on the SEI film, and inhibiting the negative impact caused by the deposition of the transition metal in the form of a single substance after the negative electrode is reduced; furthermore, the compound shown in Formula I has a low impedance, which is also beneficial to reducing the battery impedance.
[0077] The conventional synthesis process of the compound shown in Formula I inevitably contains impurities, especially the existing synthesis method using an alkaline catalyst to catalyze the ester exchange reaction, which generally contains a large number of impurity metal ions. In addition, hypochlorite is generally used as an oxidant in the existing synthesis process, which is also easy to introduce a large number of impurity metal ions, and the impurity metal ions will be directly introduced into the electrolyte with the compound shown in Formula I. Compared with the transition metal elements that slowly begin to dissolve with the use of the battery, the impurity metal ions introduced into the electrolyte with the compound shown in Formula I are not only easier to combine with the reduction product of the compound shown in Formula I, but also as the initial component in the electrolyte, it also has a time advantage in combining with the reduction product of the compound shown in Formula I, thereby not only reducing the electrochemical stability of the battery, but also affecting the ability of the polycyclic compound described in Formula I to inhibit the deposition of the dissolved transition metal ions on the negative electrode surface. Taking the sodium ions and / or potassium ions that may be introduced by using an alkaline catalyst as an example, during battery formation, driven by the external potential difference, the cations will migrate to the negative electrode, because the atomic radius of Na and K is larger than that of Li, and is also larger than transition metal elements such as Fe, Ni, and Mn, and is easier to combine with the reduction product of the polycyclic compound shown in Formula I, occupying the complexing site of the reduction product of the polycyclic compound shown in Formula I; at the same time, due to the low dissolution of the positive electrode transition metal ions during the formation of the SEI film, while Na + and K + In a free state, it is easier to migrate to the negative electrode and occupy the complexation site of the polycyclic compound shown in Formula I, resulting in a reduction in the complexation sites of the transition metal dissolved during battery storage / cycling for the same amount of the polycyclic compound shown in Formula I, thereby reducing the ability to inhibit the deposition of the already dissolved transition metal at the negative electrode.
[0078] In the present application, by using a polycyclic compound containing a compound shown in Formula I and having a metal ion content of ≤10ppm as an additive in an electrolyte, the problem that the improvement effect of the compound shown in Formula I on the electrochemical performance of the battery is reduced due to the presence of impurity metal ions, and the problem that the complexing sites and stabilizing effect of the compound shown in Formula I on the dissolved transition metal ions are reduced due to the high content of impurity metal ions can be effectively reduced, thereby effectively improving the improvement effect of the polycyclic compound on the electrochemical performance of the battery.
[0079] In some specific embodiments of the present application, when R 1 , R 2 When at least one of them is not H, when synthesizing the compound represented by formula I, an alcohol raw material containing corresponding substitution positions and substituent types can be obtained in advance, and then the alcohol raw material can be used to synthesize the compound represented by formula I through processes such as ester exchange reaction and condensation reaction.
[0080] In some specific embodiments of the present application, based on the mass of the polycyclic compound, the content of metal ions can be ≤5ppm, thereby further reducing the problem of the decrease in the improvement effect of the compound shown in Formula I on the electrochemical performance of the battery due to the presence of impurity metal ions, and further improving the improvement effect of the polycyclic compound on the electrochemical performance of the battery. Further, based on the mass of the polycyclic compound, the content of metal ions can be ≤1ppm, thereby further improving the improvement effect of the polycyclic compound on the electrochemical performance of the battery.
[0081] In some specific embodiments of the present application, the polycyclic compound may further include: chloride ions, and the content of chloride ions may be ≤10ppm based on the mass of the polycyclic compound, for example, 10ppm, 9ppm, 8ppm, 7ppm, 6ppm, 5ppm, 4ppm, 3ppm, 2ppm or 1ppm, etc. The free chloride ions in the electrolyte have a great influence on the battery performance, not only easily inducing corrosion of the positive electrode foil (such as aluminum foil), but also easily leading to the dissolution of transition metal ions of the positive electrode of the battery, which not only leads to a decrease in the structural stability of the positive electrode active material, but also the dissolved transition metal ions are easily deposited on the surface of the negative electrode, resulting in the continuous decomposition and regeneration of the SEI film, and the continuous consumption of active lithium. The dissolution of transition metal ions, the decomposition and regeneration of the SEI film will promote the decomposition of the electrolyte, which is easy to cause the battery capacity to decay, the polarization to increase due to the thickening of the SEI film or the consumption of the electrolyte and the blocking of the lithium insertion and removal channel by the byproducts, and the increase in the risk of short circuits, which has a great impact on low-temperature discharge, high-temperature storage and cycle performance. In the present application, by controlling the content of chloride ions in the polycyclic compound to meet the given range, the increase in the free chlorine content in the electrolyte caused by the use of the polycyclic compound can be effectively reduced, thereby reducing the risk of corrosion of the positive electrode foil and dissolution of transition metal ions in the positive electrode sheet due to the increase in the free chlorine content of the electrolyte, thereby improving the effect of the compound shown in Formula I on inhibiting the dissolution of transition metal ions in the active material of the positive electrode sheet.
[0082] In some specific embodiments of the present application, the content of chloride ions can be ≤5ppm based on the mass of the polycyclic compound. This can further reduce the content of free chlorine introduced into the electrolyte with the polycyclic compound, thereby reducing the risk of corrosion of the positive electrode foil and the dissolution of transition metal ions in the positive electrode sheet, and improving the effect of the compound shown in Formula I on inhibiting the dissolution of transition metal ions in the positive electrode sheet active material. Further, based on the mass of the polycyclic compound, the content of chloride ions can be ≤1ppm, which can further improve the effect of the compound shown in Formula I on inhibiting the dissolution of transition metal ions in the positive electrode sheet active material.
[0083] In some specific embodiments of the present application, based on the mass of the polycyclic compound, the content of metal ions may be ≤5ppm, and the content of chloride ions may be ≤5ppm; further, the content of metal ions may be ≤1ppm, and the content of chloride ions may be ≤1ppm. Thus, the problem of the reduced effect of the compound shown in Formula I on the electrochemical performance of the battery due to the presence of impurity metal ions and chloride ions can be further reduced, and the effect of the polycyclic compound on the electrochemical performance of the battery can be further improved.
[0084] In some specific embodiments of the present application, the polycyclic compounds may also include: chlorine-containing organic matter. Based on the mass of the polycyclic compounds, the total content of chlorine-containing organic matter may be ≤300ppm, for example, ≤300ppm, ≤280ppm, ≤250ppm, ≤220ppm, ≤200ppm, ≤180ppm, ≤150ppm, ≤120ppm, ≤100ppm, ≤80ppm, ≤50ppm, ≤40ppm, ≤30ppm, ≤20ppm, ≤10ppm or ≤5ppm, and the like. The free chloride ions in the electrolyte have a great influence on the battery performance. At present, most of the technicians in this field are committed to reducing the content of free chloride ions in the electrolyte, but in actual situations, the performance is still not optimal. The inventors of this application found that the conventional method of detecting chloride ions in the electrolyte cannot detect chlorine-containing organics of certain specific structures, because these chlorine-containing organics of specific structures are difficult to remove chlorine under existing test conditions, so that they exist in the form of chloride ions. Therefore, the existing test method cannot detect them, causing the technicians in this field to ignore the control of the content of chlorine-containing organics. And it is precisely these chlorine-containing polycyclic compounds with specific structures that have a greater negative impact on the performance of the electrolyte. The reason may be that: the battery cell usually contains trace amounts of water and some residual alkaline substances. If there are too many chlorine-containing organic impurities in the electrolyte additive, after applying it to the electrolyte, during the operation of the battery, under high temperature and high pressure conditions, especially under the action of residual alkaline substances, the chlorine-containing organic impurities are prone to hydrolysis, resulting in an increase in the free chlorine content in the electrolyte, which is not only easy to induce corrosion of the positive electrode foil (such as aluminum foil), but also easy to cause the transition metal of the battery positive electrode. The dissolution of metal ions will not only lead to a decrease in the structural stability of the positive electrode active material, but also the dissolved transition metal ions are easy to deposit on the negative electrode surface, resulting in the continuous decomposition and regeneration of the SEI film, and the continuous consumption of active lithium. The dissolution of transition metal ions, the decomposition and regeneration of the SEI film will promote the decomposition of the electrolyte, which will easily lead to battery capacity decay, increased polarization due to SEI film thickening or electrolyte consumption and by-products blocking the lithium insertion and extraction channels, and increased short circuit risks. The impact on low-temperature discharge, high-temperature storage and cycle performance is relatively large. Even under the requirements of relevant standards, the moisture content in the battery cell is also controlled, but the requirements for free chloride ions in the standard are more stringent than those for moisture. That is to say, even if the moisture content in the battery cell is not much, under the action of moisture that exceeds the free chloride ion standard, once the chlorine-containing organic matter is hydrolyzed, it will easily cause the free chloride ion content to exceed the standard, thereby deteriorating the performance.In the present application, the content of chlorine-containing organic matter in the polycyclic compound is made to meet the given range, which can further reduce the content of chlorine-containing organic matter introduced into the electrolyte with the polycyclic compound and the increase in the content of free chloride ions in the electrolyte that may be caused by the introduction of the polycyclic compound, thereby further reducing the risk of transition metal ion dissolution in the positive electrode plate and improving the effect of the polycyclic compound on the electrochemical performance of the battery.
[0085] In some specific embodiments of the present application, R 1 , R 2 can be any one of H, F, and fluoromethyl, which is not only conducive to the synthesis of the polycyclic compound shown in Formula I, but also can further avoid the introduction of chlorine-containing polycyclic compounds in additives, and reduce the free chlorine content that may be generated after the polycyclic compounds are introduced into the electrolyte. 1 , R 2 When at least one of them is F, the terminal group of the hexanol can be first substituted with fluorine or fluoromethyl, which makes the terminal group more active and easier to replace. The hexanol with fluorine or fluoromethyl terminal group can then be mixed with raw materials such as carbonate to carry out ester exchange reaction, as well as subsequent condensation reaction and oxidation reaction.
[0086] In some specific embodiments of the present application, chlorine-containing organic matter may include, but is not limited to, chlorine-containing organic matter without cyclic sulfate groups and cyclic carbonate groups, chlorine-containing organic matter containing only cyclic carbonate groups, chlorine-containing organic matter containing only cyclic sulfate groups, and chlorine-containing organic matter containing 1 to 2 cyclic carbonate groups and 1 cyclic sulfate group. Among them, in the synthesis process of the compound shown in Formula I, chlorine-containing organic matter may be produced due to excessive use of hexavalent alcohol, insufficient process conditions for transesterification and condensation reactions, etc. The several types of chlorine-containing organic impurities given are common impurities in the target product when the compound shown in Formula I is prepared using hexavalent alcohol, carbonate and thionyl chloride as raw materials. Reducing the content of the chlorine-containing organic matter is conducive to further improving the improvement effect of polycyclic compounds on the electrochemical performance of the battery.
[0087] In some specific embodiments of the present application, chlorine-containing organic impurities may include: , , One or more of the following, for example, R 1 , R 2 Taking H as an example, chlorine-containing organic matter can include , , One or more of the above. The three chlorine-containing organic substances are common chlorine-containing organic impurities in the target product when the compound shown in Formula I is prepared using hexavalent alcohol, carbonate and thionyl chloride as raw materials. The above chlorine-containing organic substances are easily hydrolyzed to form free chlorine, which increases the risk of corrosion of the positive electrode foil and dissolution of transition metal ions in the positive electrode sheet. Reducing the content of the three chlorine-containing organic substances is conducive to further reducing the increase in the free chlorine content in the electrolyte that may be caused by the introduction of polycyclic compounds, reducing the risk of dissolution of transition metal ions in the positive electrode sheet, and improving the effect of polycyclic compounds on the electrochemical performance of the battery. Further, based on the mass of the polycyclic compound, , , The total content of can be ≤50ppm, for example, ≤45ppm, ≤40ppm, ≤35ppm, ≤30ppm, ≤20ppm, ≤10ppm or ≤5ppm, etc. This can further improve the problem of reduced improvement effect of the compound represented by formula I on the electrochemical performance of the battery due to chlorine-containing organic impurities.
[0088] In some specific embodiments of the present application, the polycyclic compound may further include: other organic matter, and the other organic matter is selected from one or more of the following six compounds: , , , , , , for example, with R 1 , R 2 Taking H as an example, other organic substances can be one or more of the following six compounds: , , , , , . Based on the mass of the polycyclic compound, the total content of other organic matter can be ≤500ppm, for example, ≤450ppm, 400ppm, 350ppm, ≤300ppm, 250ppm, ≤200ppm, 150ppm, ≤100ppm, ≤50ppm or ≤30ppm, etc. The given polycyclic compounds are also common impurities in the target product when the compound shown in formula I is prepared using hexavalent alcohol, carbonate and thionyl chloride as raw materials. The total content of the six compounds meets the given range, which is conducive to further reducing the risk of reducing the improvement effect of the compound shown in formula I on the electrochemical performance of the battery due to the presence of impurities, and improving the improvement effect of the polycyclic compound on the electrochemical performance of the battery.
[0089] Furthermore, based on the mass of the polycyclic compound, the total content of other organic matter may be ≤200 ppm, and optionally ≤100 ppm, thereby further improving the effect of the polycyclic compound on the electrochemical performance of the battery.
[0090] In some specific embodiments of the present application, based on the mass of the polycyclic compound, , , , , , , , , The total content of can be ≤800ppm, for example, ≤700ppm, ≤600ppm, ≤500ppm, ≤300ppm, ≤200ppm, ≤100ppm, ≤50ppm or ≤30ppm. Further, the total content of the 9 polycyclic compounds can be ≤300ppm or ≤100ppm. Thus, the risk of the compound shown in Formula I decreasing the effect of improving the electrochemical performance of the battery due to the presence of impurities can be further reduced, and the effect of improving the electrochemical performance of the battery by the polycyclic compounds can be improved.
[0091] In some specific embodiments of the present application, R 1 , R 2 can be independently H, that is, the compound represented by formula I may include: . The polycyclic compound has a strong polarity, and its interaction with other non-polar molecules is weak, the friction and collision between molecules are small, and it has better stability than other sulfate polycyclic compounds; in addition, compared with other sulfate polycyclic compounds, the polycyclic compound also has better thermal stability, not only can it be stored at room temperature without low-temperature storage, it can operate stably in a wide voltage range, and has good cycle life and capacity retention rate. It also has better high-temperature performance and can maintain relatively stable electrochemical performance under high temperature environment, thereby extending the service life of the battery. In addition, the oxidation and reduction potentials of the polycyclic compound are both ahead of conventional electrolyte solvents. During the battery formation process, it will be oxidized at the positive electrode and reduced at the negative electrode before the solvent, and then it is easy to form a dense CEI film at the positive electrode and a dense SEI film at the negative electrode. Therefore, it is conducive to further improving the improvement effect of polycyclic compounds on the electrochemical performance of batteries.
[0092] In some specific embodiments of the present application, based on the mass of the polycyclic compound, the total content of chlorine-containing organic matter, metal ions and chloride ions can be ≤300 ppm, for example, it can be 300 ppm, 250 ppm, 200 ppm, 150 ppm, 100 ppm, 80 ppm, 50 ppm or 30 ppm, etc. The conventional synthesis process of the compound shown in Formula I inevitably contains impurities, and it is difficult to obtain a product with high purity and low impurity content. In particular, the existing synthesis method using sulfonyl chloride as a reaction raw material and using an alkaline catalyst to catalyze the transesterification reaction generally contains a large amount of chlorine-containing organic matter, impure metal ions and chloride ions. In addition, hypochlorite is generally used as an oxidant in the existing synthesis process, which is also easy to introduce a large amount of impurity metal ions and chloride ions. The impurity metal ions not only reduce the electrochemical stability of the battery, but also affect the ability of the polycyclic compound described in Formula I to inhibit the deposition of the dissolved transition metal ions on the negative electrode surface, and free chlorine is easy to cause the dissolution of transition metal ions in the positive electrode active material. In addition, the chlorine-containing organic impurities are easily hydrolyzed under the action of residual alkaline substances and the battery operating environment, and the free chlorine content in the electrolyte is increased, which is easy to cause the dissolution of transition metal ions in the positive electrode active material, reducing the improvement effect of the compound shown in Formula I on the electrochemical performance of the battery. In the present application, by using a polycyclic compound that meets the given conditions as an additive in the electrolyte, it is possible to effectively reduce the problem that the presence of impurity metal ions can easily lead to a decrease in the improvement effect of the compound shown in Formula I on the electrochemical performance of the battery, and it is also possible to effectively reduce the increase in the free chlorine content in the electrolyte caused by the introduction of the polycyclic compound, thereby reducing the risk of corrosion of the positive electrode foil and dissolution of transition metal ions in the positive electrode sheet due to the increase in the free chlorine content of the electrolyte, as well as the problem of reducing the complexing sites and stabilizing effect of the compound shown in Formula I on the already dissolved transition metal ions due to the high content of impurity metal ions, thereby effectively improving the problem that the compound shown in Formula I causes a decrease in the improvement effect on the electrochemical performance of the battery due to the presence of impurities, thereby further improving the improvement effect of the polycyclic compound on the electrochemical performance of the battery.
[0093] In some specific embodiments of the present application, based on the mass of the polycyclic compound, the total content of chlorine-containing organic matter, metal ions and chloride ions may be ≤150ppm. Further, based on the mass of the polycyclic compound, the total content of chlorine-containing organic matter, metal ions and chloride ions may be ≤100ppm. This can further solve the problem that the improvement effect of the compound shown in Formula I on the electrochemical performance of the battery due to the presence of impurity ions is reduced, and the improvement effect of the polycyclic compound on the electrochemical performance of the battery is improved.
[0094] In some specific embodiments of the present application, based on the mass of the polycyclic compound, the content of the compound shown in Formula I can be ≥99wt%, for example, it can be 99wt%, 99.2wt%, 99.4wt%, 99.5wt%, 99.7wt%, 99.9wt%, 99.92wt%, 99.95wt%, 99.97wt% or 99.99wt%, etc. Make the purity of the compound shown in Formula I meet the given range, the improvement effect of the polycyclic compound on the electrochemical performance of the battery can be further improved. Further, based on the mass of the polycyclic compound, the content of the compound shown in Formula I can be ≥99.9wt%, for example, it can be 99.9wt%, 99.91wt%, 99.92wt%, 99.93wt%, 99.94wt%, 99.5wt%, 99.96wt%, 99.97wt%, 99.8wt% or 99.99wt%, etc. This can further improve the improvement effect of the polycyclic compound on the electrochemical performance of the battery.
[0095] At present, in the common synthesis process of the compound shown in Formula I, there are problems such as poor selectivity of the target product, low yield, and more impurities in the generated target product. For example, there is currently a method of transesterifying hexavalent alcohol and carbonate under catalyst catalysis, and then adding sulfonyl chloride for recrystallization to obtain the target product, but the selectivity of this method is poor, the yield is low, and the impurities generated are more. In addition, the use of sulfonyl chloride as a reaction raw material is also prone to cause more chlorine-containing organic impurities to be present in the synthesized target product, especially when an alkaline catalyst is used to catalyze the transesterification reaction and / or hypochlorous acid (salt) is used as an oxidant, it is also easy to introduce more chlorine-containing inorganic salts into the synthesized target product. Taking sodium hypochlorite as an oxidant, for example, it is very easy to introduce more sodium ions and chloride ions into the synthesized target product, and the removal effect of sodium ions and chloride ions using a common water washing process is not ideal. In addition, there are still problems such as large solvent usage, cumbersome process, and unfavorable for industrial production in the existing synthesis process. Therefore, it is urgent to seek a method with high conversion rate, high yield, and relatively simple reaction steps, which is suitable for industrial production of polycyclic sulfates.
[0096] Based on the same inventive concept as the first aspect of the present application, it is expected to obtain a polycyclic compound product containing a compound shown in formula I and a metal ion content of ≤10ppm. The present application proposes a method for preparing a polycyclic compound with high conversion efficiency, high yield and low chlorine-containing organic impurities.
[0097] In a second aspect of the present application, a method for preparing a polycyclic compound is provided, comprising:
[0098] (1) mixing a hexahydric alcohol, a monohydric alcohol, a carbonate and an alkaline catalyst to carry out an ester exchange reaction to obtain a compound 1;
[0099] (2) dissolving the compound 1 in a solvent and reacting the mixture with thionyl chloride to obtain a compound 2;
[0100] (3) mixing the condensation reaction product with an aqueous sodium hypochlorite solution and subjecting it to oxidation treatment to obtain a reaction product containing compound 2;
[0101] (4) subjecting the reaction product obtained in step (3) to azeotropic treatment with a non-aqueous solvent;
[0102] (5) filtering the product after the azeotropic treatment, and performing a desolvation treatment on the liquid phase product to obtain a compound represented by formula I,
[0103] Wherein, the compound represented by Formula I is soluble in the non-aqueous solvent and NaCl is insoluble in the non-aqueous solvent, and the structural formulas of the hexavalent alcohol, the compound 1, and the compound 2 are respectively:
[0104] , , , R 1 , R 2 Each is independently any one of H, F, alkyl and fluoroalkyl.
[0105] During the preparation process, the use of alkaline catalysts and sodium hypochlorite will inevitably introduce metal ions. In addition, the use of thionyl chloride and sodium hypochlorite will also introduce chloride ions. Impure metal ions and chloride ions will be directly introduced into the electrolyte along with the compound shown in Formula I. Free chloride ions are likely to cause the dissolution of transition metal ions in the active material of the positive electrode plate. Moreover, relative to the transition metal elements that slowly begin to dissolve with the use of the battery, the impurity metal ions introduced into the electrolyte along with the compound shown in Formula I are not only easier to combine with the compound shown in Formula I, but also, as the initial component in the electrolyte, they also have a greater time advantage in combining with the compound shown in Formula I, thereby not only reducing the electrochemical stability of the battery, but also affecting the ability of the polycyclic compound described in Formula I to inhibit the deposition of the dissolved transition metal ions on the surface of the negative electrode, reducing the compound shown in Formula I. In order to improve the electrochemical performance of the battery, the present invention relates to an azeotropic treatment of the reaction product obtained by oxidation treatment with a non-aqueous solvent to remove water from the product after oxidation treatment. Since there is a certain matching relationship between the impurity metal cations and the chloride ions existing as anions, as the water content gradually decreases, the impurity metal cations and chloride ions that match each other combine to form inorganic salts (such as NaCl). Since the inorganic salts cannot be dissolved in the selected non-aqueous solvent, they appear in the non-aqueous solvent in the form of precipitation, while the polycyclic compound shown in the target product formula 1 is still dissolved in the non-aqueous solvent. Therefore, the inorganic salts (such as NaCl) can be removed by filtration. As a result, not only the residual metal ion content in the target product shown in formula I can be greatly reduced, such as the metal ion content can be reduced to less than a few ppm, but also the chloride ion content can be reduced.
[0106] In summary, the method for preparing a polycyclic compound in the above embodiment of the present application not only has high selectivity and high conversion rate for the compound shown in Formula I, but also has low impurity content of metal ions and chloride ions, which is conducive to obtaining the target product shown in Formula I with a metal ion content of ≤10ppm. The target product shown in Formula I obtained can be used in the electrolyte to effectively reduce the content of impurity metal ions and chloride ions in the electrolyte, reduce the risk of dissolution of transition metal ions in the active material of the positive electrode sheet due to the presence of chloride ions, and improve the problem of reducing the complexing site and stabilizing effect of the compound shown in Formula I on the already dissolved transition metal ions due to the high content of impurity metal ions, thereby effectively improving the problem of the decrease in the improvement effect of the compound shown in Formula I on the electrochemical performance of the battery due to the presence of impurities, and improving the improvement effect of the obtained polycyclic compound on the electrochemical performance of the battery. It should be noted that the method for preparing a polycyclic compound in the second aspect of the present application and the polycyclic compound in the first aspect of the present application are based on the same inventive concept, and the characteristics and effects described for the polycyclic compound in the first aspect of the present application are also applicable to the method for preparing a polycyclic compound in the second aspect of the present application, which will not be repeated here.
[0107] In some specific embodiments of the present application, the transesterification reaction can be carried out under heating and pressurization conditions.
[0108] For example, Figure 1 Shows For hexavalent alcohol, Carbonate, H 3 C-OH is a monohydric alcohol and combined with thionyl chloride As raw materials to prepare the target product The flowchart also shows the intermediate products, target products and possible impurity components such as chlorine-containing organic matter and other organic polycyclic compounds in the preparation process.
[0109] In a specific embodiment, the transesterification reaction is carried out at a temperature of 65 to 100° C. and under pressure and controlled to be less than 2.5 MPa for 0.5 to 6 hours to obtain compound 1. In step (1), the temperature of the transesterification reaction can be, for example, 65° C., 70° C., 75° C., 80° C., 85° C., 90° C., 95° C. or 100° C., the pressure can be, for example, 0.2 MPa, 0.4 MPa, 0.6 MPa, 0.8 MPa, 1 MPa, 1.2 MPa, 1.4 MPa, 1.6 MPa, 1.8 MPa, 2 MPa, 2.2 MPa or 2.5 MPa, and the time can be 0.5 to 6 hours, for example, 0.5 h, 1 h, 2 h, 3 h, 4 h, 5 h or 6 h.
[0110] refer to Figure 1 It is understood that in step (1), the reaction activity of the hydroxyl groups at the terminal positions (1 and 6) of the hexamethylene alcohol is suppressed by using a monohydric alcohol and controlling the pressure to be less than 2.5 MPa, and then the reaction temperature is raised to 65-100°C, which is higher than the boiling point of the monohydric alcohol (methanol has the lowest boiling point in China, 65°C, used in this application), so as to increase the reaction activity of the hydroxyl groups at the middle positions (2, 3, 4, and 5) of the hexamethylene alcohol, so that the activity of the hydroxyl groups at the middle positions of the hexamethylene alcohol is much higher than that of the terminal hydroxyl groups. At the same time, due to the heating and pressurizing conditions, the hydroxyl groups at the 2 and 3 positions are more likely to participate in the reaction. The product to be generated reacts with the 4- and 5-hydroxyl groups, and the product generated by the 3- and 4-hydroxyl groups (i.e., compound 1) has good symmetry and better stability. Therefore, under this condition, the selectivity for compound 1 and the conversion efficiency of compound 1 in the ester exchange reaction can be improved, and an intermediate product having compound 1 can be obtained with high conversion rate and high selectivity. Compared with the conventional process for synthesizing the target product shown in formula I, which has low selectivity and easy generation of by-products, the process of step (1) of the present application can not only effectively reduce the residual hexavalent alcohol content in the ester exchange reaction product, but also reduce the impurities. , The content of 2-hydroxy-2-nitropropene is 0.0447W, which is beneficial to further reduce the impurities that may exist in the condensation reaction product of step (2). , , , The formation of, and possible impurities produced in the subsequent oxidation reaction , In addition, in step (1), no additional organic solvent is used in the transesterification reaction, and carbonate and monohydric alcohol serve as both reactants and solvents, which is not only environmentally friendly but also easy to operate.
[0111] Too low pressure during the transesterification reaction (e.g. negative pressure) may result in a large amount of monohydric alcohol in the reaction system being removed, which is not conducive to reducing the reaction rate of the transesterification reaction and inhibiting impurities. The production of; however, the pressure during the transesterification reaction is too high. As the reaction proceeds, if the methanol content in the system is too high, the transesterification reaction is easily hindered, resulting in a lower conversion rate and an increase in residual raw materials. In the present application, by controlling the temperature, pressure and time of the transesterification reaction to meet the above ranges, a higher raw material conversion rate and a suitable transesterification reaction rate can be taken into account, thereby obtaining compound 1 with higher selectivity and yield and lower impurity content.
[0112] In some specific embodiments of the present application, reference is made to Figure 1 It is understood that in step (1), the temperature of the transesterification reaction may be 70-90°C and the pressure may be 0.5-2.2 MPa. More preferably, the temperature of the transesterification reaction may be 75-85°C and the pressure may be 1-2 MPa. This is beneficial to further balance a higher raw material conversion rate and a suitable transesterification reaction rate, thereby obtaining compound 1 with higher selectivity and yield and lower impurity content.
[0113] In some specific embodiments of the present application, by performing an ester exchange reaction under heating and pressurization conditions and combining subsequent azeotropic and filtering treatments, not only is the impurity content generated low, but the problems of low reaction conversion rate, complicated reaction steps, large amount of impurity generation, and inconvenience for industrial production in the synthesis of the compound shown in Formula I can be effectively improved. At the same time, it is also beneficial to obtain a target product with a total content of chlorine-containing organic impurities of ≤300ppm, a content of metal ions of ≤10ppm, a content of chloride ions of ≤10ppm, and a purity of ≥99wt% of the compound shown in Formula I. The target product shown in Formula I obtained is used in an electrolyte to effectively reduce the chlorine content in the electrolyte. The content of organic matter, chloride ions and impurity metal ions can effectively reduce the increase in the free chlorine content in the electrolyte caused by the introduction of the polycyclic compound, thereby reducing the risk of transition metal ions dissolving out of the positive electrode sheet due to the increase in the free chlorine content of the electrolyte, and can also improve the problem of reducing the complexing sites and stabilizing effect of the compound shown in formula I on the already dissolved transition metal ions due to the high content of impurity metal ions, thereby effectively improving the problem of the reduced improvement effect of the compound shown in formula I on the electrochemical performance of the battery due to the presence of impurities, and improving the improvement effect of the prepared polycyclic compound on the electrochemical performance of the battery when it is used as an additive in the electrolyte.
[0114] In some specific embodiments of the present application, in step (1), after the ester exchange reaction is completed, it can also include: decompression treatment to remove low-boiling point components, which is beneficial to improve the purity of the compound shown in Formula I in the final product and reduce the impurity content. As some specific examples, the decompression treatment can be a decompression distillation treatment. Optionally, the pressure of the decompression treatment can be -90~80kPa (i.e., 90~80kPa lower than the standard atmospheric pressure), for example, it can be -90kPa, -85kPa, -80kPa, etc., and the temperature of the decompression treatment can be 30~60℃, for example, it can be 35℃, 40℃, 45℃, 50℃, 55℃, etc., which is further beneficial to remove low-boiling point components.
[0115] In some specific embodiments of the present application, in step (1), the molar ratio of carbonate to hexahydric alcohol can be 3:1 to 5:1, such as 3 / 1, 3.5 / 1, 4 / 1, 4.5 / 1 or 5 / 1. Based on the amount of hexahydric alcohol, appropriately increasing the amount of carbonate is beneficial to speeding up the process of transesterification reaction, improving the conversion rate of raw materials, reducing the content of unreacted hexahydric alcohol in the intermediate product, and thus helping to reduce impurities in the final product. , In the present application, by controlling the amount of carbonate to meet the given range, the transesterification reaction can have a suitable reaction rate, which can improve the utilization rate of raw materials and the yield of compound 1 and reduce the impurities in the final product. , The content of carbonate can also reduce the excessively fast transesterification reaction when a large amount of carbonate is added, which leads to the reaction of the terminal hydroxyl groups of the hexyl alcohol to generate impurities. and The risk of subsequent impurities can be further reduced. , , The content.
[0116] In some specific embodiments of the present application, reference is made to Figure 1 It is understood that in step (1), the molar ratio of the monohydric alcohol to the hexhydric alcohol may be 10:1 to 20:1, for example, 10 / 1, 12 / 1, 14 / 1, 16 / 1, 18 / 1, 20 / 1, etc. Further preferably, the molar ratio of the monohydric alcohol to the hexhydric alcohol may be 12:1 to 18:1, and even more preferably, the molar ratio of the monohydric alcohol to the hexhydric alcohol may be 14:1 to 16:1. Controlling the relative amounts of the monohydric alcohol and the hexhydric alcohol to meet the above range can not only meet the demand for the monohydric alcohol to be used as a solvent to dissolve the reaction raw materials, but also reduce the risk of a large inhibitory effect on the ester exchange reaction when the amount of the monohydric alcohol is large, which is conducive to the smooth progress of the ester exchange reaction, and can also make the ester exchange reaction have a suitable reaction rate, reduce the low selectivity of the ester exchange reaction when the amount of the monohydric alcohol is small, and increase the reaction of the terminal hydroxyl group of the hexhydric alcohol to generate impurities. and The risk of subsequent impurities can be further reduced. , , The content.
[0117] In some specific embodiments of the present application, in step (1), based on the mass of the hexavalent alcohol, the amount of the alkaline catalyst can be 0.01-5wt%, for example, 0.01wt%, 0.1wt%, 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, etc. Controlling the amount of the alkaline catalyst within the above range is not only conducive to the smooth progress of the transesterification reaction, but also reduces the risk of increasing the amount of thionyl chloride used in the subsequent condensation reaction due to excessive use of the alkaline catalyst, thereby generating more sulfur dioxide.
[0118] In some specific embodiments of the present application, in step (1), the amount of the alkaline catalyst can be 0.02-0.5wt% based on the mass of the hexavalent alcohol. More preferably, the amount of the alkaline catalyst can be 0.02-0.1wt% based on the mass of the hexavalent alcohol. In the present application, in order to facilitate industrialization, it is expected to simplify the post-processing process of each reaction step. In view of the use of an alkaline catalyst in the transesterification reaction in step (1), the system after the reaction is easily alkaline. If the neutralization or purification process is not performed, the alkaline catalyst will enter the condensation reaction process and consume the thionyl chloride in the second step, affecting the condensation reaction. However, if the alkaline catalyst is removed, the post-processing process of step (1) will be relatively complicated, for example, it is necessary to add an acidic substance such as oxalic acid to adjust the pH value, and then perform post-processing steps such as filtration and recrystallization. In the present application, by further reducing the amount of alkaline catalyst used, the steps of adjusting pH, filtering, recrystallization, etc. after step (1) can be simplified. However, if the content of the catalyst is reduced, it is easy to affect the reaction rate, etc. The present application can make up for the defects caused by the reduction of the amount of catalyst by heating and pressurizing treatment, thereby achieving the purpose of simplifying the post-treatment process. On this basis, by further adjusting the relative amounts of hexahydric alcohol, monohydric alcohol, and carbonate, as well as the reaction temperature and pressure conditions to meet the above ranges, the defects caused by the reduction of the amount of catalyst can be further made up, thereby achieving the purpose of simplifying the post-treatment process.
[0119] In some specific embodiments of the present application, in step (1), when the hexahydric alcohol Medium R 1 , R 2 When at least one of them is not H, when synthesizing the target product shown in formula I, a hexahydric alcohol raw material containing corresponding substitution positions and substituent types can be obtained in advance, and then the hexahydric alcohol raw material can be used to synthesize the compound shown in formula I through processes such as ester exchange reaction and condensation reaction.
[0120] In some specific embodiments of the present application, reference is made to Figure 1 It is understood that in step (1), the hexavalent alcohol may include but is not limited to one or more of mannitol, sorbitol, and galactitol. Selecting the given type of hexavalent alcohol can produce a polycyclic compound with better stability. .
[0121] In some specific embodiments of the present application, in step (1), the carbonate may include, but is not limited to, one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and diphenyl carbonate.
[0122] In some specific embodiments of the present application, in step (1), the monohydric alcohol may include, but is not limited to, one or more of methanol, ethanol, propanol, isopropanol, butanol, and tert-butanol.
[0123] In some specific embodiments of the present application, in step (1), the alkaline catalyst may include, but is not limited to, one or more of sodium hydroxide, potassium hydroxide, potassium carbonate, sodium carbonate, lithium carbonate, sodium methoxide, sodium ethoxide, sodium tert-butoxide, potassium tert-butoxide, triethylamine, and pyridine.
[0124] In some specific embodiments of the present application, in step (2), after the condensation reaction is completed, it can also include: reflux deacidification treatment, which can not only reduce the residual HCl produced by the condensation reaction, but also reduce the sodium hypochlorite required for the subsequent oxidation reaction, thereby reducing the free chlorine content that may be introduced into the electrolyte later. In some specific embodiments, the temperature of the reflux deacidification can be 40~80℃, for example, 40℃, 50℃, 60℃, 70℃ or 80℃. In some specific embodiments, the temperature of the reflux deacidification can be 10~50min, for example, 15min, 20min, 30min, 40min or 50min. Meeting the reflux deacidification treatment conditions is conducive to further reducing the residual HCl produced by the condensation reaction.
[0125] In some embodiments of the present application, in step (2), the chloride ion content in the condensation reaction product after the reflux deacidification treatment is 100-200 ppm. Since the molar ratio of chloride ions to sodium ions in sodium hypochlorite is 1:1, and after the post-treatment of step (4) and step (5), when the chloride ions and metal ions are precipitated and removed in the form of chloride (such as sodium chloride), the chloride ions and metal ions are also removed in a 1:1 relationship. However, the alkaline catalyst in step (1) and the sodium hypochlorite in step (3) will introduce metal ions, that is, the actual content of metal ions will be higher than the content of chloride ions introduced in step (3). Therefore, the chloride ion content in the condensation reaction product is controlled within 100-200 ppm by reflux deacidification treatment, which is not only conducive to saving the time used for deacidification, but also the chloride ions remaining in this step can be matched with the metal ions in steps (4) and step (5), and finally removed simultaneously in the form of chloride (such as sodium chloride or potassium chloride), which is more conducive to reducing the content of metal ions and chloride ions at the same time.
[0126] In some specific embodiments of the present application, reference is made to Figure 1 It is understood that in step (2), compound 1 can be dissolved in a solvent and then thionyl chloride can be added dropwise to carry out the condensation reaction. In this way, thionyl chloride is slowly added to the mixed solution to react with compound 1, which can significantly reduce the side reactions that may be caused by the relative excess of thionyl chloride, thereby better inhibiting the formation of impurities. Generation of.
[0127] In some specific embodiments of the present application, in step (2), the temperature of the condensation reaction may be 20-100°C, for example, 20-60°C, 20°C, 25°C, 30°C, 50°C, 60°C, 80°C or 100°C. Controlling the temperature of the condensation reaction to meet the given conditions is beneficial to reducing the increase in the reactivity of thionyl chloride caused by excessively high reaction temperature, resulting in the formation of chlorine-containing impurities (such as ) can also reduce the risk of increased reaction temperature, decreased reaction rate, increased reaction time, and decreased production efficiency, and can better balance the reaction efficiency and the purity of the final product.
[0128] In some specific embodiments of the present application, in step (2), the molar ratio of compound 1 to thionyl chloride can be 1: (2~3), for example, 1 / 2, 1 / 2.2, 1 / 2.5, 1 / 2.8, 1 / 3, etc., and the addition time of thionyl chloride can be 0.5~2h, for example, 0.5h, 0.8h, 1h, 1.5h or 2h, etc. By controlling the addition amount of thionyl chloride to meet the given range, it is not only conducive to reducing the risk of a decrease in the conversion rate of the hexavalent alcohol due to a relative shortage of thionyl chloride, but also the risk of the purity and yield of the target product of compound 2 and formula I being reduced due to the uncomplete reaction of hydroxyl groups, and also conducive to reducing the risk of an increase in chlorine-containing impurities when the amount of thionyl chloride is large. Further, by making the addition time of thionyl chloride meet the given range, a suitable thionyl chloride addition rate can be obtained, which can not only increase the reaction rate, but also reduce the risk of an increase in chlorine-containing impurities due to an excessively fast addition rate of thionyl chloride. In this way, the reaction rate can be taken into consideration while also helping to improve the purity of compound 2 and the final product and reduce the impurity content.
[0129] In some specific embodiments of the present application, in step (2), the solvent may include, but is not limited to, one or more of ether solvents, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), tetrahydrofuran, and ester solvents.
[0130] In some specific embodiments of the present application, in step (2), the solvent is a solvent that can azeotropize with water. In this way, after the condensation reaction is completed, there is no need to perform a solvent removal step, and the solvent can directly participate in the reaction of step (3), so that the reaction product obtained in step (3) contains water and solvent, and no additional solvent needs to be added in step (4) to perform azeotropic treatment.
[0131] In some specific embodiments of the present application, reference is made to Figure 2It is understood that in step (3), the molar ratio of compound 2 to sodium hypochlorite can be 1:(2-2.5), for example, 1 / 2, 1 / 2.1, 1 / 2.2, 1 / 2.3, 1 / 2.4 or 1 / 2.5, etc. Controlling the content of the oxidant to meet the given range is conducive to fully oxidizing compound 2, improving the yield and purity of the target product shown in formula I, and can also reduce the chlorine-containing impurities and / or inorganic salt impurities that may be introduced when the amount of the oxidant is large.
[0132] In some specific embodiments of the present application, the solvent in step (2) is a solvent that cannot be azeotropic with water. In this way, after the condensation reaction is completed, a solvent removal step is also included to remove the solvent in step (2). At the same time, before the oxidation treatment in step (3), a non-aqueous solvent is added to dissolve the condensation reaction product to facilitate the oxidation treatment with the sodium hypochlorite aqueous solution. The oxidation product after the oxidation treatment contains water and non-aqueous solvent, and the azeotropic reaction can be carried out by heating operation. The non-aqueous solvent includes one or more of chloroform, toluene, alcohol solvents, ether solvents, and ester solvents. The temperature for the azeotropic reaction and the amount of addition are selected according to the characteristics of each solvent, and the amount of addition is based on the ability to dissolve the product of the condensation reaction. For example, ether, the azeotropic temperature is 34~35℃, and the addition amount is 20~25 times the mass of the hexamethylene alcohol; acetonitrile, the azeotropic temperature is 76~82℃, and the addition amount is 8~10 times the mass of the hexamethylene alcohol; ethyl acetate, the azeotropic temperature is 70~77℃, and the addition amount is 12~15 times the mass of the hexamethylene alcohol; toluene, the azeotropic temperature is 85~110℃, and the addition amount is 19~22 times the mass of the hexamethylene alcohol; tetrahydrofuran, the azeotropic temperature is 63~65℃, and the addition amount is 10~15 times the mass of the hexamethylene alcohol; dichloroethane, the azeotropic temperature is 72~84℃, and the addition amount is 19~23 times the mass of the hexamethylene alcohol; chloroform, the azeotropic temperature is 56~62℃, and the addition amount is 18~20 times the mass of the hexamethylene alcohol; dimethyl carbonate, the azeotropic temperature is 85~90℃, and the addition amount is 15~20 times the mass of the hexamethylene alcohol. This is conducive to further reducing the content of chloride ions and metal ion impurities in the target product shown in Formula I. The non-aqueous solvent can be selected from one or more of ethanol and ether, and the solubility of the inorganic salt in the non-aqueous solvent is low, which is conducive to further reducing the content of chloride ions and metal ion impurities in the target product shown in Formula I. As some specific examples, the non-aqueous solvent can be ether, which can further reduce the content of chloride ion impurities and metal ion impurities, and is also conducive to achieving separation of the target product and the non-aqueous solvent.
[0133] In some specific embodiments of the present application, in step (5), the desolvation treatment may include one or more of distillation, extraction, and chromatography, which can further facilitate the effective separation of the target product and the non-aqueous solvent.
[0134] In the third aspect of the present application, a polycyclic compound prepared by the method for preparing a polycyclic compound is proposed, wherein the prepared polycyclic compound comprises: a compound shown in Formula I and a metal ion, wherein the content of the metal ion is ≤10ppm based on the mass of the polycyclic compound. The characteristics and effects described for the preparation of the polycyclic compound are also applicable to the polycyclic compound, and will not be repeated here.
[0135] In the fourth aspect of the present application, a use of the polycyclic compound and the method for preparing the polycyclic compound in the field of electrolyte and battery is proposed. The features and effects described for the polycyclic compound and the method for preparing the polycyclic compound are also applicable to this use, and will not be described in detail here.
[0136] In the fifth aspect of the present application, an electrolyte is proposed, comprising: an electrolyte additive, wherein the electrolyte additive comprises the above-mentioned polycyclic compound, or a polycyclic compound prepared by the above-mentioned method for preparing a polycyclic compound. It should be noted that the characteristics and effects described for the above-mentioned polycyclic compound and the above-mentioned method for preparing a polycyclic compound are also applicable to the electrolyte, and are not described one by one here. In general, the use of the electrolyte in a battery can better improve the electrochemical performance of the battery.
[0137] Typically, the electrolyte also includes an electrolyte salt and an organic solvent. Optionally, the electrolyte can be used in a lithium battery. Taking a lithium battery as an example, the electrolyte salt can be a lithium salt. Among them, the organic solvent is the main component of the electrolyte and is an important carrier for ion transmission. It can make the organic solvent have a higher solubility of lithium salt, so that the electrolyte has a higher ionic conductivity. After the lithium salt is dissolved in the organic solvent, lithium ions can be released. The lithium ions and the organic solvent form a solvation structure, which is conducive to the rapid migration of lithium ions.
[0138] In some specific embodiments of the present application, based on the total mass of the electrolyte, the content of the electrolyte additive can be 0.1~5wt%, for example, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, etc., so that the electrolyte can be used in the battery to achieve a good improvement in the electrochemical performance of the battery.
[0139] In some specific embodiments of the present application, the organic solvent may include a carbonate solvent and / or a carboxylate solvent, thereby improving the dispersion uniformity and ion conductivity of the electrolyte.
[0140] In some specific embodiments of the present application, the organic solvent may include at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, propyl propionate and butyl propionate. The organic solvent in the given range can make the electrolyte have a higher ionic conductivity after dissolving the lithium salt, which is conducive to further improving the electrochemical performance of the battery.
[0141] In some specific embodiments of the present application, the composition of the organic solvent can be flexibly adjusted according to the actual situation of the battery system, for example, as some specific examples, the organic solvent can include ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a mass ratio of 1: (0.5-2): (0.5-2). The organic solvent can be suitable for a layered transition metal oxidant as a positive electrode active material (for example, a chemical formula of Li a Ni b Co c M1 d M2 e O f R g A battery system comprising a positive electrode active material, wherein 1≤a≤1.2, 0.6≤b≤1, 0≤c≤1, 0≤d≤1, 0≤e≤0.2, b+c+d+e=1, 1≤f≤2, 0≤g≤1, f+g=2; M1 includes Mn and / or Al, M2 includes at least one of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb, and R includes at least one of N, F, S, and Cl).
[0142] In some specific embodiments of the present application, the lithium salt may include lithium hexafluorophosphate (LiPF 6 ), lithium bis(fluorosulfonyl)imide (LiFSI), lithium tetrafluoroborate (LiBF 4 ) and lithium bis(trifluoromethanesulfonyl imide) (C 2 F 6 LiNO 4 S 2 )
[0143] In some specific embodiments of the present application, the molar concentration of the lithium salt in the electrolyte can be 0.8mol / L~2mol / L, for example, 0.8mol / L, 0.9mol / L, 1.0mol / L, 1.1mol / L, 1.2mol / L, 1.3mol / L, 1.4mol / L, 1.5mol / L, 1.6mol / L, 1.7mol / L, 1.8mol / L, 1.9mol / L or 2mol / L, etc. The cost of lithium salt in the electrolyte accounts for a high proportion, and controlling the concentration of lithium salt in the electrolyte to meet the given range is beneficial to fully dissolving the lithium salt in the organic solvent, and also to making the electrolyte have both high ionic conductivity and low manufacturing cost.
[0144] In some specific embodiments of the present application, in addition to the above components, the electrolyte may optionally include a small amount of other conventional additives or auxiliary agents that can improve certain battery properties. Those skilled in the art can make selections based on actual needs, which will not be described in detail here.
[0145] In the sixth aspect of the present application, a battery is proposed, comprising: the above-mentioned electrolyte. It should be noted that the characteristics and effects described for the electrolyte in the third aspect of the present application are also applicable to the battery, and will not be repeated here. In general, the battery has good electrochemical properties. In addition, it should be noted that the type of the battery is not particularly limited, and those skilled in the art can flexibly choose according to actual needs, for example, it can be a secondary battery.
[0146] Typically, a battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery charge and discharge process, active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0147] In some embodiments of the present application, the positive electrode sheet may include a positive electrode current collector and a positive electrode active material layer disposed on the surface of the positive electrode current collector, the positive electrode active material layer includes a positive electrode active material, a conductive agent and a binder, the positive electrode current collector may include a metal foil or a composite positive electrode current collector, for example, the metal foil may be aluminum foil, the composite positive electrode current collector may include a polymer material base and a metal layer formed on at least one side of the surface of the polymer material base, for example, the composite negative electrode current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc.). The positive electrode active material may include the above-mentioned positive electrode active material or a commonly used positive electrode active material in the art. The conductive agent and the binder may be conventional materials in the art.
[0148] In some embodiments of the present application, the negative electrode plate may include a negative electrode current collector and a negative electrode active material layer disposed on the surface of the negative electrode current collector, the negative electrode active material layer may include a negative electrode active material, a conductive agent and a binder, wherein the negative electrode current collector may be a metal foil or a composite current collector, for example, the metal foil may be a copper foil, the composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate, for example, the composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc.). The negative electrode active material may include a commonly used negative electrode active material in the art (such as at least one of commonly used negative electrode active materials such as graphite, silicon-carbon composite materials, silicon materials, lithium metal, lithium titanate, etc.). The conductive agent and the binder may be conventional materials in the art.
[0149] In some embodiments of the present application, the isolation membrane can adopt an isolation membrane that is well known in the art and can be used in batteries and is stable to the electrolyte used. For example, its material can include but is not limited to at least one of polyolefins, aromatic polyamides, polytetrafluoroethylene, and polyether sulfone, such as a polyethylene diaphragm, a polypropylene diaphragm, a PE ceramic coated diaphragm, etc., and the specific material can be flexibly selected according to needs.
[0150] The embodiments of the present application are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. In addition, unless otherwise explicitly stated, all reagents used in the following embodiments are commercially available or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.
[0151] Example 1
[0152] 1. Preparation of polycyclic compounds:
[0153] (i) Mannitol, dimethyl carbonate, methanol and sodium hydroxide were added into a reactor at a molar ratio of 1:3.5:15:0.0005, reacted at 1.5 MPa and 85°C for 1 hour, and low-boiling materials were removed under reduced pressure at (-85±5) kPa and 50°C to obtain a dry product mainly composed of compound 1. The structural formula of compound 1 is , in this embodiment, ;
[0154] (ii) The dried product was dissolved in 50 g of dichloromethane, and thionyl chloride was added dropwise to the dried product solution at room temperature for 1.5 h. The mixture was stirred for 2.5 h. The molar ratio of thionyl chloride to thionyl chloride is 1:2.1; reflux and deacidify at 40°C for 30 minutes to obtain a reaction product, which includes compound 2. The structural formula of compound 2 is , in this embodiment, ;
[0155] (iii) removing dichloromethane from the reaction product of step (2) by distillation under reduced pressure, adding toluene in an amount 20 times the mass of mannitol to dissolve the solid matter, and then adding a 12% sodium hypochlorite aqueous solution to carry out an oxidation reaction, wherein the molar ratio of sodium hypochlorite to compound 2 in the reaction product is 2:1.
[0156] (iv) separating the layers, raising the temperature of the organic phase to 100° C., and removing the residual water in the organic phase by azeotropy;
[0157] (v) filtering off the precipitated inorganic salt, taking the liquid product and distilling it under reduced pressure at -80 kPa and 50° C. to remove the solvent, to obtain the final product of formula I , in this embodiment, .
[0158] 2. Preparation of positive electrode
[0159] The positive electrode active material LiNi 0.6 Co 0.1 Mn 0.3 O 2 The binder polyvinylidene fluoride (PVDF) and the conductive agent conductive carbon black are mixed evenly in a weight ratio of 97:1.2:1.8, and N-methylpyrrolidone (NMP) is added and stirred under the action of a vacuum mixer until the mixed system becomes a positive electrode slurry with uniform fluidity; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, and the coating amount is 20.2g / m 2After drying at 85°C, cold pressing is performed, and trimming, cutting, and slitting are performed. After slitting, it is dried at 85°C under vacuum conditions for 4 hours, and the pole ears are welded to obtain the positive electrode sheet.
[0160] 3. Preparation of negative electrode sheet
[0161] The negative electrode active material graphite is mixed with the conductive agent conductive carbon black, the thickener carboxymethyl cellulose (CMC), and the adhesive styrene butadiene rubber (SBR) in a mass ratio of 95.8:1.2:1.5:1.5, and deionized water is added to obtain the negative electrode slurry under the action of a vacuum mixer; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil, and the coating amount is 13.0g / m 2 After drying at 85°C, cold pressing is performed, and edge trimming, cutting, and slitting are performed. After slitting, it is dried at 85°C under vacuum conditions for 4 hours, and the tabs are welded to obtain the negative electrode sheet.
[0162] 4. Preparation of electrolyte
[0163] In a glove box filled with argon (water content <10ppm, oxygen content <1ppm), ethylene carbonate, ethyl methyl carbonate and diethyl carbonate were mixed in a mass ratio of 3:5:2 as an organic solvent, lithium hexafluorophosphate was used as a lithium salt, and the final product obtained in step 1 was used as an electrolyte additive. The lithium salt concentration was configured to be 1 mol / L, and the mass proportion of the electrolyte additive in the electrolyte was 1wt% of the electrolyte.
[0164] 5. Preparation of isolation film
[0165] A polyethylene isolation film with a thickness of 8 μm was selected.
[0166] 6. Lithium-ion battery preparation
[0167] The prepared positive electrode sheet, negative electrode sheet and isolation film are stacked in order, the isolation film is placed between the positive electrode sheet and the negative electrode sheet, and then rolled and flattened and put into an aluminum foil packaging bag, which is vacuum-baked at 75°C for 48 hours to obtain a battery cell, and the above-mentioned electrolyte is injected into the battery cell in a glove box, and the preparation of the lithium-ion battery is completed after packaging, formation, aging and capacity separation.
[0168] Examples 2 to 18 and Comparative Examples 1 to 6
[0169] The differences between Examples 2 to 18 and Comparative Examples 1 to 6 and Example 1 are shown in Tables 1 to 5 (Tables 1 and 2 show some differences between Examples 1 to 18 and Comparative Examples 1 to 5, and Tables 3, 4 and 5 show some differences and test results between Examples 1 to 18 and Comparative Examples 1 to 6). The difference between Comparative Example 1 and Example 1 is that steps (iv) to (v) are performed as follows: inorganic salts are removed by washing with water, and after the oxidation reaction is completed, the layers are separated, the organic phase is taken, and the washing and extraction layers are performed with deionized water, and after repeating for 3 times, the solvent is removed at (-85±5) kPa and 30°C to obtain the final product.
[0170] The structure, purity, impurity content, and battery cycle performance of the polycyclic compounds obtained in Examples 1 to 18 and Comparative Examples 1 to 6 were tested. The test method is as follows, and the test results are shown in Tables 3 to 5. Figure 2 and Figure 3 shown.
[0171] (1) Perform NMR testing on the final product of the polycyclic compound using a nuclear magnetic resonance (NMR) spectrometer to determine the polycyclic compound structure of the final product; perform liquid chromatography testing on the final product of the polycyclic compound using a high performance liquid chromatograph to quantitatively analyze the components of the final product; perform metal ion and chloride ion content testing using ion chromatography; and perform content analysis on chlorine-containing organic impurities using high performance liquid chromatography.
[0172] (2) Initial charge and discharge efficiency: The charge capacity at the time of formation is recorded as C 化成 , charge the formed battery to 4.4V at room temperature using a 0.1C constant current and constant voltage, and record the charging capacity as C 充 , leave it for 5 minutes, and then discharge it at 0.1C to 2.75V. The discharge capacity is C 放 , first charge and discharge efficiency (%) = C 放 / (C 化成 +C 充 )×100%.
[0173] (3) Cycle performance test: Charge the formed battery to 4.4V at room temperature using a constant current and constant voltage of 1.0C, and discharge it to 2.75V at 1.0C, and measure the initial discharge capacity of the battery; perform 800 charge and discharge cycles, and measure the discharge capacity of the battery after 800 charge and discharge cycles. Calculate the cycle capacity retention rate based on the cycle capacity retention rate (%) = (800th cycle discharge capacity / 1st cycle discharge capacity) × 100%.
[0174] (4) High temperature storage performance test:
[0175] At 25°C, the battery was charged to 4.4V at 1.0C constant current, charged to a cut-off current of 0.05C at 4.4V constant voltage, and then discharged to 2.75V at 1C constant current. The discharge capacity is recorded as C 1 Remove the battery and use a thickness tester to test its initial thickness. 1 At 25°C, charge at 1.0C constant current to 4.4V, charge at 4.4V constant voltage to a cut-off current of 0.05C, then transfer the battery to an explosion-proof oven at 60°C for 30 days. Use a thickness tester to test the thickness after 30 days as T. 2 Then the battery is discharged to 2.75V at a constant current of 1.0C, and the discharge capacity is recorded as C 2 . Storage at 60℃ for 30 days Capacity retention rate = C 2 / C 1 *100%, 60℃ storage for 30 days Battery expansion rate = 100%*(T 2 -T 1 ) / T 1 .
[0176]
[0177] Results and Conclusions:
[0178] Combining Examples 1 to 18, Comparative Examples 1 to 5 and Table 1, it can be seen that the purity of the compound represented by Formula I in the final product prepared by the method of the above embodiment of the present invention is high, and the metal ion content is low, generally below 10 ppm. Taking Example 1 as an example, Figure 2 and Figure 3 The nuclear magnetic hydrogen spectrum and carbon spectrum of the final product obtained in Example 1 are shown, and its structural formula is shown in Table 2, with high purity and a metal ion content of 1ppm. In addition, it can be seen from Examples 1 to 7 that, under the same other conditions, the transesterification reaction is carried out under heating and pressurization conditions, which can also improve the selectivity and yield of the target product, reduce the content of chlorine-containing organic matter and other compounds, and appropriately increase the pressure. It is also beneficial to further improve the selectivity and yield of the target product. Further, it can be seen from Examples 1 to 18 and Comparative Examples 1 to 6 that the final product (i.e., polycyclic compound) with a metal ion content of less than 10ppm obtained in the above embodiment is used as an electrolyte additive in the electrolyte, which is also beneficial to further improve the electrochemical performance of the battery.
[0179] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0180] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. A method for preparing a polycyclic compound as shown in Formula I, characterized in that: include: (1) mixing a hexahydric alcohol, a monohydric alcohol, a carbonate and an alkaline catalyst to carry out an ester exchange reaction to obtain a compound 1; (2) dissolving the compound 1 in a solvent and reacting the mixture with thionyl chloride to obtain a reaction product containing the compound 2; (3) mixing the condensation reaction product with an aqueous sodium hypochlorite solution for oxidation treatment; (4) subjecting the reaction product obtained in step (3) to azeotropic treatment with a non-aqueous solvent; (5) filtering the product after the azeotropic treatment, and performing a desolvation treatment on the liquid phase product to obtain a compound represented by formula I, Wherein, the compound represented by formula I is soluble in the non-aqueous solvent and NaCl is insoluble in the non-aqueous solvent, and the structural formulas of the hexavalent alcohol, the compound 1, the compound 2, and the compound represented by formula I are, in order: , , , , R1 and R2 are independently any one of H, F, alkyl and fluoroalkyl, and the alkyl and fluoroalkyl are independently an alkyl having 1 to 10 carbon atoms and a fluoroalkyl having 1 to 10 carbon atoms; The transesterification reaction is carried out under heating and pressurizing conditions. The temperature of the transesterification reaction is 65-100° C., the pressure is pressurized and is 0.2 MPa-2.5 MPa, and the time is 0.5-6 hours.
2. The method according to claim 1, characterized in that Step (1) satisfies at least one of the following conditions: (B) after the transesterification reaction is completed, the process further comprises: reducing pressure to remove low boiling point components; (C) the molar ratio of the carbonate to the hexahydric alcohol is (3:1) to (5:1); (D) the molar ratio of the monohydric alcohol to the hexahydric alcohol is (10:1) to (20:1); (E) Based on the mass of the hexavalent alcohol, the amount of the alkaline catalyst is 0.01-5wt%; (F) the hexavalent alcohol includes one or more of mannitol, sorbitol, and galactitol; (G) the carbonate ester includes one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and diphenyl carbonate; (H) the monohydric alcohol includes one or more of methanol, ethanol, propanol and butanol; (I) The alkaline catalyst includes one or more of sodium hydroxide, potassium hydroxide, potassium carbonate, sodium carbonate, lithium carbonate, sodium methoxide, sodium ethoxide, sodium tert-butoxide, potassium tert-butoxide, triethylamine, and pyridine.
3. The method according to claim 1 or 2, characterized in that: Step (2) satisfies at least one of the following conditions: (a) after the condensation reaction is completed, the step further includes: reflux deacidification treatment; (β) After dissolving compound 1 in a solvent, thionyl chloride is added dropwise to carry out the condensation reaction, wherein the thionyl chloride is added for 0.5 to 2 hours, and the condensation reaction lasts for 1 to 4 hours; (γ) the condensation reaction temperature is 20 to 100°C; (δ) the molar ratio of the compound 1 to the thionyl chloride is 1:(2-3); (ζ) The solvent is a solvent that can form an azeotrope with water.
4. The method according to claim 3, characterized in that The solvent includes one or more of ether solvents, N,N-dimethylformamide, N,N-dimethylacetamide, and ester solvents.
5. The method according to claim 3, characterized in that: After the condensation reaction is completed, the method further comprises: reflux deacidification treatment, wherein the temperature of the reflux deacidification treatment is 40-80° C., and / or the time of the reflux deacidification treatment is 10-50 min, and / or the chloride ion content in the condensation reaction product after the reflux deacidification treatment is 100-200 ppm.
6. The method according to any one of claims 1 or 2, characterized in that: At least one of the following conditions is met: (①) In step (3), the molar ratio of the compound 2 to the sodium hypochlorite is 1:(2-2.5); (②) In step (5), the non-aqueous solvent includes one or more of chloroform, toluene, alcohol solvents, ether solvents, and ester solvents; (③) In step (5), the desolvation treatment includes one or more of distillation, extraction, and chromatography; (④) The solvent in step (2) is a solvent that can azeotrope with water, and the non-aqueous solvent in step (4) is the solvent in step (2); (⑤) The solvent in step (2) cannot be azeotropic with water, and the condensation reaction comprises a solvent removal step to remove the solvent in step (2) after completion of the condensation reaction; and the non-aqueous solvent in step (4) is added before the oxidation treatment in step (3), and the non-aqueous solvent is added to dissolve the condensation reaction product to facilitate the oxidation treatment with the sodium hypochlorite aqueous solution; the non-aqueous solvent is subjected to the azeotropic treatment with the reaction product obtained in step (4) and step (3); (⑥) the amount of the non-aqueous solvent added is sufficient to dissolve the condensation reaction product; (⑦) The azeotropic treatment is achieved by increasing the temperature.
7. The method according to claim 2, characterized in that Step (1) satisfies at least one of the following conditions: (i) the temperature of the transesterification reaction is 75-85°C and the pressure is 1-2Mpa; (ii) the molar ratio of the monohydric alcohol to the hexahydric alcohol is (12:1) to (18:1); (iii) Based on the mass of the hexavalent alcohol, the amount of the alkaline catalyst is 0.02-0.5wt%.
8. The method according to claim 7, characterized in that Step (1) satisfies at least one of the following conditions: 1) The molar ratio of the monohydric alcohol to the hexahydric alcohol is (14:1) to (16:1); 2) Based on the mass of the hexavalent alcohol, the amount of the alkaline catalyst is 0.02-0.1 wt %.
Citation Information
Cited By
Preparation method of mannitol carbonate sulfate
CN120441561A