A nano-TiC particle modified 6 series aluminum alloy and its preparation method and application
By adding nano-TiC particles and supplementing with nano-Si to the aluminum alloy, the microstructure of the aluminum alloy is optimized, the problem of insufficient strength and hot cracking of the aluminum alloy under high load conditions is solved, and its mechanical properties and thermal stability are improved.
Patent Information
- Application Number
- CN202410776356.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-17
AI Technical Summary
Conventional aluminum alloys have insufficient strength and plasticity under high load conditions, and deformed alloys are prone to hot cracking during die-casting and liquid die forging processes. Existing technologies have shortcomings in improving strength and improving hot cracking problems.
Nano-TiC particles are added to the 6 series aluminum alloy. By remelting the aluminum liquid and adding co-solvent and nano-TiC particles in batches, the microstructure is optimized, the grain structure is refined, the strength and toughness are improved, and the nano-Si particles are used to assist in dispersing the nano-TiC particles. TiC particles, control particle size and addition amount, inhibit thermal cracking.
Significantly improve the yield strength, tensile strength and elongation of aluminum alloy, reduce the risk of hot cracking, enhance the high temperature stability and creep resistance of the material, solve the problem of hot cracking, and optimize the microstructure and mechanical properties.
Smart Images

Figure CN118360515B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alloy materials and processing thereof, and in particular to a nano-TiC particle-modified 6-series aluminum alloy and a preparation method thereof. Background Art
[0002] The α-Al and eutectic phase grains in conventional cast aluminum alloys are coarse, and the alloy strength and plasticity are low. However, the rapid growth in the application of aluminum alloys in the automotive and 3C electronics industries has also put forward higher requirements on their performance, especially when used as structural parts. The performance requirements are more stringent. Conventional cast aluminum alloys cannot meet the requirements of bearing high loads in terms of strength and plasticity. The industry hopes to use deformed alloys with high performance, but deformed alloys are prone to thermal cracking when produced using die casting and liquid die forging processes.
[0003] The existing technology often uses three methods, namely, in-situ endogenous method, powder metallurgy synthesis and adding nanoparticles, to enhance the performance of aluminum alloys and improve the hot cracking problem. The Chinese patent application with patent publication number CN111118355A uses rare earth element Er to modify the hypoeutectic casting Al-Mg2Si alloy to refine the α-Al and eutectic phases, but the alloy strength is limited and the hot cracking problem of the deformed alloy cannot be solved. The Chinese patent application with publication number CN112662909A discloses a die-cast aluminum alloy modified by carbide nanoparticles and a preparation method thereof. The method is an in-situ endogenous method through a chemical reaction between an element and a compound. The advantage of this method is that it can directly generate the required reinforcement phase inside the material, so that the interface between the reinforcement and the matrix is clean and pollution-free, and evenly distributed. Its disadvantage is that specific reaction conditions need to be met during the preparation process, and the generation of by-products is difficult to control, and sometimes there are interface problems. Summary of the invention
[0004] In order to overcome the shortcomings of the prior art, the purpose of the present application is to provide a nano-TiC particle modified 6 series aluminum alloy, by adding nano-sized TiC particles to the 6 series deformed aluminum alloy, refining the alloy matrix, eliminating the dendrite structure, enhancing the fluidity of the alloy, improving the strength and plastic toughness of the aluminum alloy material, and inhibiting the problem of hot cracking.
[0005] To solve the above problems, the technical solutions adopted in this application are as follows:
[0006] The embodiment of the present application provides a 6-series aluminum alloy modified with nano-TiC particles, which is an aluminum alloy modified by adding nano-TiC particles to the aluminum liquid after remelting of 6-series aluminum. The amount of the nano-TiC particles added to the aluminum liquid is 0.5wt%-1.0wt%, the particle size of the nano-TiC particles is 30nm-80nm, and the size of the α-Al grains in the modified aluminum alloy is 1-50μm; the second phase compounds of the modified aluminum alloy include Mg2Si, AlSiMnFe, and CuAl2, and the sizes of Mg2Si, AlSiMnFe, and CuAl2 are all 1μm-10μm.
[0007] As a further preferred solution, the addition amount of the nano-TiC particles described in the embodiment of the present application is 0.5wt%-1.0wt%.
[0008] As a further preferred solution, nano-Si particles are added to the nano-TiC particles described in the embodiments of the present application, and the mass ratio of nano-TiC particles to nano-Si is (8-12):1.
[0009] As a further preferred solution, the nano-TiC particle modified 6 series aluminum alloy described in the embodiment of the present application has a yield strength of 350-370 MPa, a tensile strength of 380-420 MPa, and an elongation after fracture of 8.5%-13% in the T6 state.
[0010] The present application also provides a method for preparing a 6-series aluminum alloy modified with nano-TiC particles, wherein nano-scale TiC particles are selected to modify cast aluminum and deformed aluminum through an external process, thereby optimizing and improving the microstructure of the aluminum alloy, improving the strength and plasticity of the alloy, and suppressing the hot cracking problem of deformed aluminum in the casting process. The preparation method comprises the following steps:
[0011] Aluminum alloy remelting: melting cast aluminum or deformed aluminum alloy at a first preset temperature to obtain aluminum liquid, and controlling the aluminum liquid temperature to maintain at a second preset temperature;
[0012] Adding nano-TiC particles: under the second preset temperature condition, adding the solvent and nano-TiC particles to the above aluminum liquid in batches, stirring the aluminum liquid while adding;
[0013] Refining: After the nano-TiC particles are completely added, a refining agent is added during the stirring process for refining, and then after degassing and slag removal treatment, the alloy is allowed to stand to obtain a nano-TiC particle-modified 6 series aluminum alloy.
[0014] As a further preferred scheme, the preparation method described in the embodiment of the present application also includes the step of treating the nano-TiC particles before adding the nano-TiC particles: adding nano-Si particles to the nano-TiC particles, mixing and dispersing them evenly, and then adding them to the aluminum liquid in batches, and the mass ratio of nano-TiC particles to nano-Si is (8-12):1.
[0015] As a further preferred solution, the first preset temperature described in the embodiment of the present application is 800-820°C; the second preset temperature is 850-900°C.
[0016] As a further preferred scheme, in the preparation method described in the embodiment of the present application, when adding nano-TiC particles, the nano-TiC particles are first mixed with the co-solvent, and the obtained mixture is added in 3-8 times. The stirring speed during the stirring process is 120-200 r / min, and the stirring time after adding the co-solvent and the nano-TiC particles is 2-4 hours.
[0017] As a further preferred scheme, in the preparation method described in the embodiment of the present application, the amount of the refining agent added is 0.5wt%-3.0wt% of the weight of the aluminum liquid; the refining agent includes the following components in mass percentage: CaF2 20wt%-40wt%, MgCl2•KCl 60wt%-80wt%.
[0018] As a further preferred scheme, in the preparation method described in the embodiment of the present application, the degassing method adopts a protective gas degassing method or a dynamic vacuum degassing method.
[0019] The embodiment of the present application also provides an application of a 6-series aluminum alloy modified with nano-TiC particles in the production of a mobile phone mid-plate.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The nano-TiC particle modified 6 series aluminum alloy described in the present application is an aluminum alloy obtained by refining the aluminum liquid after remelting the aluminum alloy with nano-TiC particles. The nano-TiC particles can serve as effective heterogeneous nucleation sites to promote the nucleation process of the aluminum matrix, thereby refining the grain structure, improving the mechanical properties and physical properties of the aluminum alloy, and enhancing its strength and toughness.
[0022] 2. In the nano-TiC particle modified 6 series aluminum alloy described in the present application, the nano-TiC particles can increase the hardness and strength of the aluminum matrix, and optimize the microstructure of the aluminum alloy through interaction with the matrix metal, thereby further improving its mechanical indicators such as tensile strength, yield strength and elongation; at the same time, by optimizing the microstructure and reducing defects and impurities on the grain boundaries, the stability and creep resistance of the aluminum alloy at high temperatures can be improved.
[0023] 3. In the nano-TiC particle modified 6 series aluminum alloy described in the present application, the nano-TiC particles act as additional nucleation points and can promote the transformation of dendrites to equiaxed crystals during the solidification process of the aluminum alloy; this transformation can greatly reduce the hot cracking of the material and better resist crack propagation caused by thermal stress. By optimizing the microstructure of the aluminum alloy and reducing internal stress concentration and defects, its hot cracking resistance can be indirectly improved.
[0024] 4. The preparation method of the nano-TiC particle modified 6 series aluminum alloy described in the present application is to add TiC particles to the remelted aluminum liquid to modify the aluminum alloy by an external addition method. Compared with the internal method: on the one hand, the external addition method can directly add nano-TiC particles to the aluminum liquid; on the other hand, the nano-TiC particles used are usually prepared in advance, and their properties such as size, shape and purity can be better controlled.
[0025] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0027] Figure 1 This is the organizational structure diagram of the 6 series aluminum alloy modified by nano-TiC particles described in Example 1 of the present application.
[0028] Figure 2 This is the organizational structure diagram of the 6 series aluminum alloy modified by nano-TiC particles described in Example 2 of the present application.
[0029] Figure 3 This is the organizational structure diagram of the 6 series aluminum alloy modified with nano-TiC particles described in Example 3 of the present application. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0031] The term "comprising" and other equivalent descriptions involved in the specification and claims of this application are intended to cover non-exclusive inclusions, including both the contents clearly described in the specification and claims, and the steps or units that are not described in the specification and claims but are inherent in the product, method or structure.
[0032] The embodiment of the present application provides a nano-TiC particle modified 6 series aluminum alloy, which is an aluminum alloy modified by adding nano-TiC particles to the aluminum liquid after remelting the 6 series aluminum, wherein the addition amount of the nano-TiC particles is 0.5wt%-1.0wt% of the weight of the aluminum liquid, the particle size of the nano-TiC particles is 30nm-80nm, and the size of the α-Al grains in the modified aluminum alloy is 1-50μm. In this scheme, the nano-TiC particles can serve as effective heterogeneous nucleation sites to promote the nucleation process of the aluminum matrix, thereby refining the grain structure, improving the mechanical properties and physical properties of the aluminum alloy, and improving its strength and toughness. The grain size has a direct impact on the hot cracking sensitivity of the aluminum alloy. Smaller grains mean more grain boundaries, which can absorb and disperse thermal stress, thereby reducing the formation and expansion of cracks. Therefore, when the α-Al grain size is small, the hot cracking of the aluminum alloy material can be reduced. At the same time, grain size also affects the mechanical properties of aluminum alloy materials. More grain boundaries can hinder dislocation movement and crack propagation. Therefore, grain refinement can improve the strength, plasticity and toughness of aluminum alloys. In addition, fine grains can also increase the plastic deformation capacity of the material, making it less likely to break when subjected to stress. Of course, the smaller the grain size, the better. Too small grains may lead to excessive grain boundary area, thereby increasing defects and stress concentration inside the material, which has an adverse effect on performance. Therefore, in this application, regulating the size of α-Al grains by nano-TiC particles is an important factor in solving the technical problems of this application.
[0033] From the perspective of the mechanical properties of aluminum alloys, the smaller the particle size of nano-TiC particles, the larger the specific surface area, and the larger the contact area with the aluminum alloy matrix, thereby enhancing the interfacial bonding between the particles and the matrix; this enhanced interfacial bonding helps to improve the strength, hardness and wear resistance of the aluminum alloy; in addition, the fine nano-TiC particles can be better dispersed in the aluminum alloy matrix, play a role in dispersion strengthening, and further improve the comprehensive mechanical properties of the aluminum alloy. But in fact, in this application, the particle size of nano-TiC particles is not the smaller the better. If the particle size is too small, the distribution of nano-TiC particles in the aluminum alloy may agglomerate, which will reduce the performance of the aluminum alloy; and too small a particle size may also make it difficult to evenly disperse the particles during the preparation process, increasing the difficulty of preparation. Hot cracking mainly occurs during the solidification process of aluminum alloys, due to solidification shrinkage and stress concentration. If the particle size of nano-TiC particles is too large, they may form larger hard points in the aluminum alloy. These hard points may become crack sources when subjected to force, increasing the risk of hot cracking. Fine nano-TiC particles can refine the grains of aluminum alloys, reduce stress concentration at grain boundaries, and thus reduce the tendency of hot cracking; at the same time, nano-TiC particles can also improve the fluidity of aluminum alloys, which helps to reduce defects and cracks during the solidification process. Therefore, in the embodiment of the present application, the particle size of the nano-TiC particles used is 30nm-80nm. Preferably, the particle size of the nano-TiC particles is 40-60nm. In the embodiment of the present application, since the addition of nano-TiC particles can promote the nucleation process during the solidification of aluminum alloys, resulting in the refinement or even disappearance of dendrites, the disappearance of secondary dendrites helps to reduce microscopic defects and stress concentration in aluminum alloys, thereby improving their mechanical properties; at the same time, the reduction of secondary dendrites can also improve the thermal stability of aluminum alloys and reduce the risk of hot cracking. Because secondary dendrites are usually hot cracking sensitive areas, their disappearance helps to reduce the formation and expansion of cracks. Smaller primary dendrite size means more grain boundaries and more uniform microstructure, which helps to improve the strength, plasticity and toughness of aluminum alloys. Grain boundaries can absorb and disperse thermal stress when the material is stressed, reducing the formation and expansion of cracks. If the primary dendrites are refined uniformly enough, the risk of thermal cracking can be effectively reduced. Therefore, in this application, in order to further solve the thermal cracking problem of aluminum alloys and enhance the mechanical properties of aluminum alloys, the secondary dendrites disappear in the organizational structure of the 6-series aluminum alloy modified by nano-TiC particles described in the embodiments of this application.
[0034] In the embodiments of the present application, nano-TiC particles have extremely high hardness and excellent mechanical properties. They can be used as an effective strengthening phase to improve the overall performance of aluminum alloys through dispersion strengthening and interface strengthening mechanisms. The addition of an appropriate amount of nano-TiC particles can significantly improve the strength, hardness and toughness of aluminum alloys; excessive addition may also cause the nano-TiC particles to agglomerate in the aluminum alloy, forming large-sized hard points, which will reduce the plasticity and toughness of the aluminum alloy, resulting in a decrease in the performance of the aluminum alloy. At the same time, the addition of an appropriate amount of nano-TiC particles can refine the grain structure, improve the solidification behavior of the aluminum alloy, and reduce the tendency of hot cracking; if the addition amount is too much, the hard points in the nano-TiC particles may become crack sources during the solidification process, increasing the risk of hot cracking. Therefore, in the present application, in order to obtain an aluminum alloy with enhanced performance and solve the problem of hot cracking at the same time, the addition amount of the nano-TiC particles in the aluminum liquid is controlled to be 0.5wt%-1.0wt%.
[0035] The influence of the grain size of the second phase on the performance of the aluminum alloy is manifested as follows: when the second phase grains are small, it means that the number of grain boundaries increases, which helps to enhance the strength and toughness of the material; and the increase of the second phase particles reduces the density of the aluminum alloy grain boundaries, reduces the number of grain boundaries, and leads to an increase in the degree of grain boundary bending and the range of distribution areas; therefore, the increase of the second phase particles will lead to a decrease in the hardness and strength of the aluminum alloy, and also reduce its toughness and plasticity. The composition of the second phase determines the physical and chemical properties of the aluminum alloy itself, and then affects the overall performance of the aluminum alloy. The Mg2Si phase can improve the hardness and strength of the aluminum alloy, while the Cu-Al2 phase may reduce the ductility of the alloy. The composition of the second phase can adjust the thermal expansion coefficient and thermal conductivity of the aluminum alloy. The thermal physical properties, further reduce the risk of thermal cracking. As a further preferred solution, the second phase compound described in the embodiment of the present application is Mg2Si, AlSiMnFe, CuAl2, and the size of Mg2Si, AlSiMnFe, and CuAl2 in the second phase is 1-10μm.
[0036] As a further preferred solution, the nano-TiC particle-modified 6-series aluminum alloy described in the embodiment of the present application has a yield strength of 350-370 MPa, a tensile strength of 380-420 MPa, and an elongation after fracture of 8.5-13% in the T6 state.
[0037] The present application also provides a method for preparing a 6-series aluminum alloy modified with nano-TiC particles, wherein nano-scale TiC particles are selected to modify cast aluminum and deformed aluminum through an external process, thereby optimizing and improving the microstructure of the aluminum alloy, improving the strength and plasticity of the alloy, and suppressing the hot cracking problem of deformed aluminum in the casting process. The preparation method comprises the following steps:
[0038] Aluminum alloy remelting: melting the aluminum alloy at a first preset temperature to obtain aluminum liquid, and controlling the temperature of the aluminum liquid to maintain at a second preset temperature;
[0039] Adding nano-TiC particles: under the second preset temperature condition, adding the solvent and nano-TiC particles to the aluminum liquid in batches, stirring the melt while adding;
[0040] Refining: After the nano-TiC particles are completely added, a refining agent is added during the stirring process for refining, and then after degassing and slag removal treatment, the alloy is allowed to stand to obtain a nano-TiC particle-modified 6 series aluminum alloy.
[0041] In the above preparation method, the aluminum alloy is remelted to obtain uniform aluminum liquid. During the remelting process, the temperature affects the melting and uniformity of the aluminum alloy. If the temperature is too high, the aluminum alloy may be over-oxidized, resulting in metal loss and increased impurities. If the temperature is too low, the aluminum alloy may not be completely melted, resulting in unmelted particles or impurities remaining in the aluminum liquid, affecting the subsequent addition and dispersion of nano-TiC particles. Moreover, nano-TiC particles need to be effectively dispersed into the aluminum liquid at an appropriate temperature to form a uniform modified alloy; if the temperature is too high, the nano-TiC particles may agglomerate or oxidize and lose their modification effect; and if the temperature is too low, the particles may not be fully dispersed, affecting the modification effect. The remelting temperature will also affect the subsequent refining, degassing and slag removal processes; the refining agent has different activities at different temperatures, so it is necessary to select a suitable temperature to ensure the best refining effect; and the effect of degassing and slag removal is also affected by temperature, and the appropriate temperature is conducive to the discharge and removal of gas and slag. In addition, the remelting temperature will also affect the grain structure and properties of the aluminum alloy. Too high a temperature may cause grain growth, affecting the mechanical properties and thermal stability of the alloy; while too low a temperature may lead to insufficient grain refinement, which will also affect the performance of the alloy. Therefore, considering the important impact of the aluminum alloy remelting temperature on subsequent processes, strict control is required to ensure the preparation of 6 series aluminum alloy modified with nano-TiC particles with excellent performance. In the embodiment of the present application, the first preset temperature is controlled to 800-820°C; the second preset temperature is controlled to 850-900°C. Preferably, in some embodiments, the first preset temperature is 805-815°C; the second preset temperature is preferably 850-860°C.
[0042] Nano-TiC particles can refine grains, improve microstructure and improve the mechanical properties of alloys. Adding a small amount of nano-TiC particles can significantly improve the yield strength and tensile strength of aluminum alloys, while keeping the elongation basically unchanged. However, adding nano-TiC particles to aluminum liquid to modify aluminum alloys will inevitably cause some problems. Due to the extremely small size and high specific surface area of nano-TiC particles, agglomeration is prone to occur, resulting in uneven dispersion in the aluminum alloy matrix. This uneven dispersion state will affect the enhancement effect of nano-TiC particles in aluminum alloys, limiting its performance improvement. In the embodiments of the present application, a variety of solutions are used to solve the agglomeration problem of nano-TiC particles in aluminum liquid.
[0043] One solution to the agglomeration problem of nano TiC particles in aluminum liquid is to add a solvent while adding nano TiC particles to aluminum liquid. The solvent can react chemically with the metal to generate one or more low melting point compounds. These compounds can significantly reduce the melting point of the entire alloy system in a molten state, and improve the fluidity of the metal, which helps the nano TiC particles to flow and mix better in the aluminum liquid, and promotes its uniform dispersion in the aluminum liquid. It is necessary to consider its compatibility with nano TiC particles and aluminum liquid and its specific impact on the performance of aluminum alloys. In the embodiment of the present application, fluorine salt compounds are selected as solvents. Specifically, one or more of potassium fluoroaluminate, potassium fluoride, sodium fluoroaluminate, etc. can be selected but not limited to. These solvents can reduce the contact angle between nano TiC particles and aluminum liquid, have good wettability and compatibility in aluminum liquid, and can also play the role of heterogeneous nucleating agent, refine the grains of the alloy, thereby further promoting the dispersion of nano TiC particles. The amount of solvent will affect the dispersion effect of nano TiC particles in aluminum liquid and the performance of aluminum alloy. An appropriate amount of solvent can significantly improve the dispersion effect of nano-TiC particles in aluminum liquid. The solvent can react chemically with aluminum to generate low-melting-point compounds. These compounds can improve the fluidity of the metal in the molten state and are conducive to the uniform dispersion of nano-TiC particles. Too little solvent may not provide sufficient dispersion force, resulting in particle agglomeration; while too much solvent may introduce too many impurities, affecting the performance of aluminum alloy. And the addition of an appropriate amount of solvent can significantly improve the strength, hardness and toughness of aluminum alloy. Therefore, in the present application, the mass ratio of the added solvent to the nano-TiC particles is (1-2):1, preferably, the mass ratio of the solvent to the nano-TiC particles is (1.2-1.5):1. In a preferred embodiment, the solvent and the nano-TiC particles are first mixed evenly and then added to the aluminum liquid in batches. By mixing the two in advance, the solvent can be wrapped on the surface of the nano-TiC particles, effectively reducing the interaction force between the particles and preventing them from agglomerating. The solvent can reduce the interfacial tension between the aluminum liquid and the nano-TiC particles, making the nano-TiC particles easier to dissolve or disperse in the aluminum liquid.
[0044] Another solution to the agglomeration problem of nano-TiC particles in aluminum liquid is to add a small amount of nano-Si particles to the nano-TiC particles. On the one hand, the surface energy of nano-Si particles is higher when nano-TiC particles and nano-Si are mixed, and they can be adsorbed on the surface of nano-TiC particles, thereby reducing the attraction between nano-TiC particles. Nano-Si particles can play a role similar to a dispersant, effectively reducing the agglomeration of nano-TiC particles; on the other hand, nano-Si can also drive nano-TiC particles to be better dispersed in aluminum liquid through its good affinity with aluminum liquid; in addition, nano-Si has some active sites in aluminum liquid, providing more binding points for nano-TiC particles, thereby enhancing its affinity with aluminum liquid. In the embodiment of the present application, nano-TiC particles and nano-Si are mixed and dispersed evenly and then added to aluminum liquid in batches. During the mixing process of nano-TiC particles and nano-Si, mechanical stirring is used to mix the two, and the stirring speed is 300-500r / min. The appropriate mixing ratio can ensure that the nano-TiC particles and nano-Si particles are evenly dispersed in the aluminum liquid, thereby improving the performance of the composite material. The evenly dispersed nano-particles can significantly refine the grains, improve the density and mechanical properties. In the embodiments of the present application, the inventors found that the ratio of TiC particles to nano-Si particles has an important influence on solving the agglomeration problem of nano-TiC particles, as well as the refinement of aluminum alloy grains, the mechanical properties and thermal stability of aluminum alloy materials. Therefore, in some embodiments of the present application, the mass ratio of the nano-TiC particles to the nano-Si particles is (8-12):1.
[0045] In the present application, nano-TiC particles are added in batches, and each addition is carried out under stirring conditions, which can not only effectively break the agglomeration between nano-TiC particles and promote their uniform dispersion in the aluminum liquid; it can also prevent the temperature from rising suddenly or the reaction is too violent due to the instantaneous addition of a large number of nano-TiC particles, which is conducive to maintaining the stability of the aluminum liquid and ensuring the safety and controllability of the preparation process. In the preparation method described in the embodiment of the present application, when adding nano-TiC particles, they are added in 3-8 times. The stirring speed is a key factor affecting the uniformity of the dispersion of nano-TiC particles in the aluminum liquid. If the stirring speed is too low, the particles cannot be fully dispersed, and agglomeration is inevitable; if the stirring speed is too high, excessive shear force may be generated, destroying the stability of the aluminum liquid, and may even introduce new impurities. In addition, the stirring time will also affect the interaction between the aluminum liquid and the nano-TiC particles. If the stirring time is too short, the nano-particles may not be fully dispersed or reacted, resulting in poor modification effect; and if the stirring time is too long, the preparation cost may increase, and may even cause excessive oxidation or contamination of the aluminum liquid. In order to obtain the best modification effect, in the examples of the present application, the stirring speed during the stirring process is 120-200 r / min, and the stirring time after adding the co-solvent and the nano-TiC particles is 2-4 hours.
[0046] In addition, in the embodiments of the present application, by controlling the addition of nano-Si particles to nano-TiC particles and controlling the mass ratio of nano-TiC particles to nano-Si particles, combined with the control of the addition method of nano-TiC particles and stirring conditions, the alloy matrix and the second phase compound can be effectively refined, the dendritic structure of the aluminum alloy can be eliminated, the fluidity of the alloy can be enhanced, the strength and plastic toughness of the aluminum alloy material can be improved, and the problem of hot cracking can be suppressed.
[0047] In the present application, the addition of a refining agent can further remove impurities and gases in the aluminum liquid and improve the purity of the aluminum alloy. The refining process helps to reduce the occurrence of hot cracking and other defects. When selecting a refining agent, it is necessary to consider factors such as the composition of the aluminum alloy, the impurity removal ability of the refining agent, the impact on nano-TiC particles, the conditions of use and operating requirements, environmental protection and safety, as well as cost and economic benefits. In some embodiments of the present application, the amount of the refining agent used is 0.5wt%-3.0wt% of the melt weight; the refining agent includes the following components in mass percentage: CaF2 20wt%-40wt%, MgCl2•KCl 60wt%-80wt%. In the refining agent used in the embodiments of the present application, CaF2 is mainly used as a degassing agent, which can react with hydrogen in the aluminum liquid to generate hydrogen fluoride gas that is insoluble in the aluminum liquid, thereby effectively removing the hydrogen content in the aluminum liquid. In addition, CaF2 can also react with oxide inclusions in the aluminum liquid to form compounds with lower density, which is convenient for inclusions to float and be removed; when the amount of CaF2 is in the range of 20wt%-40wt%, it can significantly improve the purity of the aluminum alloy, reduce the number of pores and inclusions, and thus improve the mechanical properties and processing properties of the aluminum alloy. During the refining process, MgCl2•KCl can form a protective coating on the surface of the aluminum liquid to prevent the aluminum liquid from contacting with oxygen and water vapor in the air, thereby reducing oxidation and inhalation. MgCl2•KCl can also reduce the melting point of the refining agent, so that it can melt at a lower temperature and be evenly distributed in the aluminum liquid, thereby improving the refining effect. When the amount of MgCl2•KCl is in the range of 60wt%-80wt%, it can ensure that a stable coating is formed on the surface of the aluminum liquid, effectively preventing oxidation and inhalation, and can ensure that the melting point of the refining agent is reduced, and the dispersibility and fluidity of the refining agent are improved.
[0048] Degassing is to remove gases dissolved in the aluminum liquid, such as hydrogen, which may cause defects such as thermal cracking and holes. As a further preferred solution, in the preparation method described in the embodiment of the present application, the degassing method adopts a protective gas degassing method or a dynamic vacuum degassing method. Preferably, in some embodiments of the present application, a protective gas degassing method is adopted, and the protective gas can be selected from nitrogen or an inert gas, such as argon, neon, etc. In the protective gas degassing method, the main function of the protective gas is that on the one hand, the gas needs to cover the surface of the aluminum liquid to prevent the outside air from entering and reacting with the aluminum liquid; on the other hand, the gas also needs to penetrate into the aluminum liquid to help bring out the gas (such as hydrogen) dissolved therein; the flow of the protective gas will drive the rolling of the aluminum liquid, which is conducive to the uniform distribution and rapid rise of the bubbles, so the flow control of the protective gas is an important control condition for the degassing process. On the one hand, if the flow rate of the protective gas is too large, it will cause excessive tumbling of the aluminum liquid, increasing the risk of oxidation and inclusions; if the flow rate is too small, it may not be able to form enough bubbles, affecting the degassing effect; on the other hand, the flow rate of the protective gas determines the size and number of bubbles. If the bubbles are too large, the gas may stay in the aluminum liquid for too short a time and cannot fully capture the dissolved gas; if the bubbles are too small, the rising speed may be too slow, affecting the degassing efficiency. Therefore, in order to avoid the above situations, in the application, the flow rate of the protective gas is controlled to 0.5-1.0m 3 / h.
[0049] The present application also provides an application of a nano-TiC particle modified 6 series aluminum alloy in manufacturing a mobile phone mid-plate. The various performance requirements of the aluminum alloy for making a mobile phone mid-plate are: yield strength of 350-370MPa, tensile strength of 390-420MPa, and elongation after fracture of 8.5%-13%.
[0050] The following are specific embodiments of the present application, and the present application is further limited by the following embodiments.
[0051] Example 1
[0052] like Figure 1 As shown, this embodiment provides a nano-TiC particle modified 6 series aluminum alloy, which is prepared by the following method:
[0053] Aluminum alloy remelting: Aluminum alloy 6013 is melted at 800℃ to obtain aluminum liquid, and the temperature of the aluminum liquid is controlled to be maintained at 850℃;
[0054] Adding nano-TiC particles: under the condition of 850°C, add the pre-mixed mixture of nano-TiC particles and potassium fluoroaluminate (the mass ratio of nano-TiC particles to potassium fluoroaluminate is 1:1.2) into the above aluminum liquid in 5 times, the average particle size of the nano-TiC particles is 60nm, the addition amount is 0.8wt%, and the aluminum liquid is stirred while adding, the stirring speed is 200r / min, and the stirring time after adding the nano-TiC particles is 2 hours;
[0055] Refining: After the nano-TiC particles are completely added, a refining agent is added during the stirring process for refining. The amount of the refining agent added is 0.2wt%. Argon is then used as a protective gas for degassing. The flow rate of the protective gas is 0.8m 3 / h, after refining, scrape off the slag on the surface of the melt and let it stand for 15 minutes to obtain nano-TiC modified aluminum alloy.
[0056] Performance Testing
[0057] 1. The microstructure of the nano-TiC modified aluminum alloy obtained in Example 1 was tested using a metallographic microscope. Figure 1 .
[0058] 2. The mechanical properties of the nano-TiC modified aluminum alloy obtained in the example were tested, and the cracks and bubbles in the castings processed from the nano-TiC modified aluminum alloy were tested. The test items and the methods / standards used for the test are shown in Table 1 below.
[0059] Table 1: Mechanical properties test results of nano-TiC modified aluminum alloy
[0060]
[0061] Furthermore, in order to understand the effect of the particle size of nano-TiC particles on the mechanical properties, cracks and bubbles of the modified aluminum alloy material, on the basis of the scheme of the above-mentioned Example 1, nano-TiC particles of different particle sizes were used to modify the aluminum alloy, and other conditions were the same as those of Example 1. See Table 2 for the experimental conditions and results.
[0062] Table 2: Effect of particle size of nano-TiC particles on the properties of aluminum alloy
[0063]
[0064] The experimental results in Table 2 above show that the smaller the particle size of the nano-TiC particles, the easier it is to agglomerate, and this agglomeration phenomenon will cause the elongation at break of the aluminum alloy material to decrease, and in the actual process of modifying the aluminum alloy, the presence of agglomeration will form a coarse phase structure, which may have an adverse effect on the mechanical properties, corrosion resistance, etc. of the aluminum alloy; and the larger the particle size, the more it will affect the mechanical properties of the aluminum alloy material. The grain refinement effect of the nano-TiC particles can improve the mechanical properties of the aluminum alloy. When the particle size is too large, this enhancement effect will weaken, resulting in a decrease in the mechanical properties of the aluminum alloy. Therefore, based on the comprehensive experimental results, in this application, when the particle size of the nano-TiC particles is 30-80nm, the performance of the aluminum alloy obtained can meet the requirements of the application, and the particle size of the preferred nano-TiC particles is 40-60nm.
[0065] Further, in order to understand the effect of the addition amount of nano-TiC particles on the mechanical properties, cracks and bubbles of the modified aluminum alloy material, on the basis of the scheme of the above-mentioned Example 1, the aluminum alloy was modified by using nano-TiC particles with different addition amounts, and the other conditions were the same as those of Example 1. See Table 3 for the experimental conditions and results.
[0066] Table 3: Effect of the addition amount of nano-TiC particles on the properties of aluminum alloy
[0067]
[0068] When too much nano-TiC particles are added, the appearance of nano-clusters will be aggravated at the grain boundaries of the composite material, and the clusters will reduce the toughness of the composite material, causing the elongation of the material to decrease. The modified aluminum alloy material described in the embodiment of the present application is mainly used for the manufacture of mobile phone mid-plates, which requires an elongation of not less than 8.5%. It can be seen that when the addition amount of nano-TiC particles exceeds 1.0%, the elongation at break does not meet the expected requirements.
[0069] Furthermore, in order to understand the effects of stirring speed and stirring time on the performance, cracks and bubbles of the modified aluminum alloy material, different aluminum alloy remelting temperatures were used based on the scheme of Example 1, and other conditions were the same as those of Example 1. See Table 4 for experimental conditions and results.
[0070] Table 4: Effect of stirring speed on aluminum alloy properties
[0071]
[0072] The experimental results in Table 4 show that when the stirring speed is too low, the clustering of nano-TiC particles cannot be avoided, resulting in a decrease in the elongation of the aluminum alloy material. When the stirring speed is higher than a certain speed, gas will be drawn into the aluminum liquid, resulting in the generation of bubbles. Therefore, in order to meet the application requirements of the mobile phone mid-plate in this application, the stirring speed is selected to be 120-200r / min.
[0073] Example 2
[0074] like Figure 2 As shown, this embodiment provides a nano-TiC particle modified 6 series aluminum alloy, which is prepared by the following method:
[0075] Aluminum alloy remelting: Aluminum alloy 6061 is melted at 810℃ to obtain aluminum liquid, and the temperature of the aluminum liquid is raised and controlled to be maintained at 860℃;
[0076] Adding nano-TiC particles: under the condition of 860°C, a mixture of potassium fluoroaluminate and nano-TiC particles (the mass ratio of potassium fluoroaluminate to nano-TiC particles is 1.8:1) is added to the above aluminum liquid in three times, the average particle size of the nano-TiC particles is 50nm, the addition amount is 0.5wt%, and the aluminum liquid is stirred while adding, the stirring speed is 200r / min, and the stirring time after adding is 2h;
[0077] Refining: After the nano-TiC particles are completely added, refining agent + argon gas is added during the stirring process for refining. The amount of refining agent added is 0.2wt%, and the flow rate of protective gas is 1m 3 / h, after refining, scrape off the slag on the surface of the melt and let it stand for 12 minutes to obtain nano-TiC modified aluminum alloy.
[0078] Performance Testing
[0079] 1. The microstructure of the nano-TiC modified aluminum alloy obtained in Example 2 was tested using a metallographic microscope. Figure 2 .
[0080] 2. The mechanical properties of the nano-TiC modified aluminum alloy obtained in the example were tested. The test items and the methods / standards used for the test are shown in Table 5 below.
[0081] Table 5: Mechanical properties test results of nano-TiC modified aluminum alloy
[0082] Example 3
[0083] like Figure 3 As shown, this embodiment provides a nano-TiC particle modified 6 series aluminum alloy, which is prepared by the following method:
[0084] Aluminum alloy remelting: Aluminum alloy 6210 is melted at 820℃ to obtain aluminum liquid, and the aluminum liquid temperature is controlled to be maintained at 870℃;
[0085] Adding nano-TiC particles: under the condition of 870°C, nano-TiC particles (nano-Si particles are added to the nano-TiC particles, and the mass ratio of nano-TiC particles to nano-Si particles is 10:1) are added to the above aluminum liquid in 8 times, the average particle size of the nano-TiC particles is 60nm, the addition amount is 1.0wt%, and the aluminum liquid is stirred while adding, the stirring speed is 200r / min, and the stirring time after adding is 2h;
[0086] Refining: After the nano-TiC particles are completely added, refining agent + argon gas is added during the stirring process for refining. The amount of refining agent added is 0.2wt%, and the flow rate of argon gas is 0.5m 3 / h, after refining, scrape off the slag on the surface of the melt and let it stand for 12 minutes to obtain nano-TiC modified aluminum alloy.
[0087] Performance Testing
[0088] 1. The microstructure of the nano-TiC modified aluminum alloy obtained in Example 3 was tested by metallographic microscopy. Figure 3 .
[0089] 2. The mechanical properties of the nano-TiC modified aluminum alloy obtained in the example were tested. The test items and the methods / standards used for the test are shown in Table 6 below.
[0090] Table 6: Mechanical properties test results of nano-TiC modified aluminum alloy
[0091]
[0092] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.
Claims
1. A method for preparing a 6-series aluminum alloy modified with nano-TiC particles, characterized in that: The following steps are involved: Aluminum alloy remelting: melt the 6 series aluminum alloy at a first preset temperature to obtain aluminum liquid, and control the temperature of the aluminum liquid to maintain at a second preset temperature, wherein the first preset temperature is 800-820°C; and the second preset temperature is 850-900°C; Adding nano-TiC particles: adding nano-Si particles to the nano-TiC particles, mixing and dispersing them uniformly, and then mixing them with a solvent. The obtained mixture is added to the above-mentioned aluminum liquid in 3-8 times, while stirring the aluminum liquid, the stirring speed is 120-200r / min, and the stirring time after adding the solvent and nano-TiC particles is 2-4 hours; the amount of the nano-TiC particles added to the aluminum liquid is 0.5wt%-1.0wt%, the particle size of the nano-TiC particles is 30nm-80nm, the mass ratio of the nano-TiC particles to the nano-Si particles is (8-12):1, and the mass ratio of the solvent to the nano-TiC particles is (1-2):1; Refining: After the nano-TiC particles are completely added, a refining agent is added during the stirring process for refining, and then after degassing and slag removal, the alloy is allowed to stand to obtain a TiC nano-modified aluminum alloy; The size of α-Al grains in the TiC nano-modified aluminum alloy is 1-50 μm, and the second phase compounds include Mg2Si, AlSiMnFe, and CuAl2. The sizes of Mg2Si, AlSiMnFe, and CuAl2 are all 1 μm-10 μm.
2. The preparation method according to claim 1, characterized in that: The amount of the refining agent added is 0.5wt%-3.0wt% of the weight of the aluminum liquid; the refining agent includes the following components in mass percentage: CaF2 20wt%-40wt%, MgCl2•KCl 60wt%-80wt%.
3. The preparation method according to claim 1, characterized in that: The degassing method is a protective gas degassing method or a dynamic vacuum degassing method.
4. A 6-series aluminum alloy modified with nano-TiC particles obtained by the preparation method according to any one of claims 1 to 3, characterized in that: The invention discloses an aluminum alloy obtained by adding nano-TiC particles mixed with nano-Si particles to aluminum liquid after remelting 6 series aluminum, wherein the mass ratio of nano-TiC particles to nano-Si particles is (8-12):1; the amount of the nano-TiC particles added to the aluminum liquid is 0.5wt%-1.0wt%, and the particle size of the nano-TiC particles is 30nm-80nm; the size of α-Al grains in the modified aluminum alloy is 1-50μm, and the second phase compounds in the modified aluminum alloy include Mg2Si, AlSiMnFe, and CuAl2, and the sizes of Mg2Si, AlSiMnFe, and CuAl2 are all 1μm-10μm.
5. The nano-TiC particle modified 6 series aluminum alloy according to claim 4, characterized in that: The modified aluminum alloy has a yield strength of 350-370 MPa, a tensile strength of 380-420 MPa, and an elongation after fracture of 8.5%-13% in the T6 state.
6. Use of the nano-TiC particle modified 6 series aluminum alloy as claimed in claim 4 or 5 in manufacturing a mobile phone mid-plate.
Citation Information
Patent Citations
Rare earth element erbium-modified cast hypoeutectic Al-Mg2Si alloy and preparation method thereof
CN111118355A
Die-casting aluminum alloy modified by carbide nanoparticles and preparation method thereof
CN112662909A
Hot rolling process of 6xxx aluminum alloy
CN109136628A
Preparation method of reinforced aluminum alloy plate with nano-endogenous TiC particles
CN109468485A
Preparation method of novel particle-reinforced 6XXX aluminum alloy plate strip
CN114101610A