A smart thermal control-infrared stealth integrated coating and its preparation method, spacecraft

By using a structure consisting of a layered metal bonding layer, a thermochromic radiation layer, and a heat-sensitive layer, the shortcomings of thermal control coatings in terms of infrared stealth and service life are solved. This results in a coating with high bonding strength and infrared stealth function in temperature-changing environments, extending service life and reducing maintenance frequency.

CN118389983BActive Publication Date: 2026-11-10BEIJING MINING & METALLURGICAL TECH GRP CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410490678.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-23
Publication Date
2026-11-10
Estimated Expiration
2044-04-23

AI Technical Summary

Technical Problem

Existing thermal control coatings are difficult to simultaneously meet infrared stealth requirements and extend service life, and require frequent maintenance.

Method used

The structure employs a stacked configuration of a metal bonding layer, a thermochromic radiation layer, and a heat-sensitive layer. The metal bonding layer comprises an MCrAlY alloy, the thermochromic radiation layer comprises a lanthanum manganate ceramic, and the heat-sensitive layer comprises a low-emission, low-absorption metal. The coating is prepared using supersonic spraying, plasma spraying, and magnetron sputtering processes to ensure the bonding strength and thermal expansion coefficient matching between the layers.

Benefits of technology

It achieves high bonding strength and infrared stealth function of coating in temperature-changing environments, can autonomously adjust emissivity, adapt to changes in space temperature, extend service life and reduce maintenance frequency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118389983B_ABST
    Figure CN118389983B_ABST
Patent Text Reader

Abstract

This application provides an integrated intelligent thermal control and infrared stealth coating, its preparation method, and a spacecraft, relating to the field of thermal control coatings. The coating comprises a stacked metal bonding layer, a thermochromic radiation layer, and a heat-sensitive layer. The metal bonding layer comprises an MCrAlY alloy, where M includes nickel and / or cobalt. The thermochromic radiation layer comprises a lanthanum manganate ceramic system, and the heat-sensitive layer comprises one or more of Pt, Ag, Cu, and Al. This coating possesses infrared stealth capabilities. Through the combined use of multiple layers, including the metal bonding layer, the thermochromic radiation layer, and the heat-sensitive layer, it reduces radiation absorption and effectively adjusts emissivity with temperature changes, adapting to the temperature variations in the space environment. Its unique temperature sensing characteristics effectively respond to temperature changes, control interlayer heat transfer within the coating, and rapidly adjust emissivity changes, meeting multifunctional requirements. Furthermore, the coating is thin and lightweight, effectively saving energy and resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of thermal control coatings, and more particularly to an integrated coating with intelligent thermal control and infrared stealth functions, its preparation method, and spacecraft. Background Technology

[0002] With the continuous development of science and technology, research on spacecraft thermal control technology has become increasingly in-depth. Spacecraft are exposed to radiation from celestial bodies, including the Sun and Earth, in the harsh thermal environment of space, with temperature differences reaching over 200 degrees Celsius. Therefore, to ensure the normal operation of spacecraft payload equipment and control the heat flux density of internal precision instruments, thermal control coatings are needed to regulate temperature on the spacecraft surface, significantly reducing energy consumption and greatly benefiting the extension of the spacecraft's service life. Lanthanum-strontium-manganese-oxygen ceramic materials, due to their metal-insulator phase transition characteristics, have become one of the main means of passive temperature control.

[0003] Meanwhile, with the rapid development of infrared detection technology in recent years, especially the advent of high-precision, high-resolution infrared detection and remote sensing equipment, more severe challenges have been posed to military defense systems. Research on infrared stealth methods and materials has received high attention and focus. Therefore, during spacecraft operation in orbit, it is necessary to cope with infrared reconnaissance and guidance, and improve the infrared stealth performance and survivability of equipment in the space environment. Due to their low emissivity at infrared wavelengths, metallic materials can be used as the main raw material for infrared stealth coatings.

[0004] However, current thermal control coatings still face challenges such as how to meet infrared stealth requirements, improve service life, and reduce maintenance frequency. Summary of the Invention

[0005] The purpose of this application is to provide an integrated coating with intelligent thermal control and infrared stealth functions, its preparation method, and a spacecraft, in order to solve the above-mentioned problems.

[0006] To achieve the above objectives, the first aspect of this application provides an integrated coating with intelligent thermal control and infrared stealth functions, comprising a stacked metal bonding layer, a thermochromic radiation layer, and a heat-sensitive layer;

[0007] The metal bonding layer comprises an MCrAlY alloy;

[0008] The thermochromic radiation layer comprises lanthanum manganate-based ceramics.

[0009] The heat-sensitive layer comprises a metal with low emission and low absorption properties;

[0010] M in the MCrAlY alloy includes nickel and / or cobalt;

[0011] The composition of the lanthanum manganate system ceramic includes La. 1-xA x MnO3, wherein A includes one or more of Sr, Ba and Ca, and x ranges from 0.1 to 0.3;

[0012] The metal includes one or more of Pt, Ag, Cu, and Al.

[0013] Optionally, the integrated coating with intelligent thermal control and infrared stealth functions satisfies at least one of the following conditions:

[0014] A. The thickness of the metal bonding layer is 50μm-150μm;

[0015] B. The thickness of the thermochromic radiation layer is 100μm-200μm;

[0016] C. The thickness of the heat-sensitive layer is 200nm-300nm.

[0017] Optionally, the porosity of the thermochromic radiation layer is 10%-15%.

[0018] A second aspect of this application provides a method for preparing the integrated coating with intelligent thermal control and infrared stealth functions, comprising:

[0019] The MCrAlY alloy is first sprayed onto the substrate using a supersonic spraying process and / or a plasma spraying process to obtain the metal bonding layer.

[0020] The lanthanum manganate system ceramic is subjected to the plasma spraying process to be second-sprayed onto the metal bonding layer, and then sintered to obtain the thermochromic radiation layer.

[0021] Under vacuum conditions, the metal is sputtered onto the thermochromic radiation layer using a magnetron sputtering process, and then annealed to obtain the integrated coating with intelligent thermal control and infrared stealth functions.

[0022] Optionally, the preparation method of the integrated intelligent thermal control and infrared stealth coating satisfies at least one of the following conditions:

[0023] A. During the first spraying, the spraying distance in the supersonic spraying process is 300mm-400mm, the powder feeding rate is 3r / min-5r / min, the kerosene is 4L / h-6L / h, and the oxygen is 1500L / min-2000L / min;

[0024] B. During the first spraying, the spraying distance in the plasma spraying process is 130mm-150mm, the power is 35kW-42kW, the powder feeding rate is 1.5r / min-2.5r / min, and the operating current is 530A-550A.

[0025] Optionally, the power of the second spraying is 20kw-30kw, the working current of the second spraying is 600A-700A, the powder feeding rate of the second spraying is 2r / min-9r / min, and the distance of the second spraying is 170mm-190mm.

[0026] Optionally, the sputtering gas pressure is 0.8Pa-1.5Pa, the sputtering power is 100W-200W, and the sputtering turntable speed is 3r / min-5r / min.

[0027] Optionally, the sintering temperature is 850℃-900℃, and the sintering holding time is 0.5h-1h.

[0028] Optionally, the preparation method of the integrated intelligent thermal control and infrared stealth coating satisfies at least one of the following conditions:

[0029] A. The annealing temperature is 300℃-400℃, and the annealing time is 2h-4h;

[0030] B. The vacuum level is 1.0 × 10⁻⁶. -4 Pa-1.0×10 -3 Pa.

[0031] A third aspect of this application provides a spacecraft including the aforementioned integrated coating for intelligent thermal control and infrared stealth functions.

[0032] Compared with the prior art, the beneficial effects of this application include:

[0033] The intelligent thermal control-infrared stealth integrated coating provided in this application includes a multi-layer coating structure comprising a metal bonding layer, a thermochromic radiation layer, and a heat-sensitive layer. The metal bonding layer increases the bonding strength between the thermochromic radiation layer and the substrate, as well as the matching degree of interlayer thermal expansion coefficients. The thermochromic radiation layer is made of perovskite oxide with metal-insulator state transition characteristics, capable of autonomously adjusting its emissivity range according to changes in phase transition temperature, thus achieving intelligent thermal control. The heat-sensitive layer not only complements the emissivity regulation of the thermochromic radiation layer, but its material also features low emissivity and low absorption, enabling the coating to possess infrared stealth capabilities. Through the combined use of the metal bonding layer, thermochromic radiation layer, and heat-sensitive layer, radiation absorption can be reduced while effectively adjusting emissivity with temperature changes, adapting to temperature variations in the space environment. Its unique temperature sensing characteristics effectively respond to temperature changes, control interlayer heat transfer within the coating, and rapidly adjust emissivity changes, meeting multi-functional requirements. Furthermore, the coating is thin and lightweight, effectively saving energy and resources.

[0034] The method for preparing the integrated intelligent thermal control and infrared stealth coating provided in this application involves preparing an MCrAlY metal bonding layer on the surface of an aluminum alloy substrate using supersonic spraying and / or plasma spraying; then, spraying a lanthanum manganate system material onto the surface of the metal bonding layer using plasma spraying, followed by heat treatment to obtain a thermochromic radiation layer; finally, under vacuum conditions, sputtering a metal with low emissivity characteristics onto the surface of the thermochromic radiation layer using magnetron sputtering, followed by annealing to obtain the integrated intelligent thermal control and infrared stealth coating. This process is not limited by the shape of the substrate, can prepare large-area coatings with uniform composition, and offers high controllability, high spraying efficiency, and readily available raw materials, making it suitable for large-scale industrial production.

[0035] The spacecraft provided in this application has intelligent thermal control performance while meeting the requirements for infrared stealth, which greatly extends the service life of its internal precision instruments and reduces the number of maintenance operations. Attached Figure Description

[0036] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments will be briefly described below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation on the scope of this application.

[0037] Figure 1 This is a schematic diagram of the integrated intelligent thermal control and infrared stealth coating prepared in Example 1;

[0038] Figure 2 The graph shows the emissivity of the integrated intelligent thermal control and infrared stealth coating prepared in Example 1 as a function of temperature. Detailed Implementation

[0039] As used in this article:

[0040] "Prepared from" is synonymous with "comprising". The terms "comprising", "including", "having", "containing", or any other variations thereof as used herein are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements, but may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.

[0041] The conjunction "composed of..." excludes any unspecified elements, steps, or components. If used in a claim, this phrase makes the claim closed, excluding materials other than those described, except for associated conventional impurities. When the phrase "composed of..." appears in a clause of the body of a claim rather than immediately following it, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0042] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range “1–5” is disclosed, the described range should be interpreted as including ranges “1–4”, “1–3”, “1–2”, “1–2 and 4–5”, “1–3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range.

[0043] In these embodiments, unless otherwise specified, the portions and percentages are all by weight.

[0044] "Parts by mass" refers to the basic unit of measurement that expresses the mass ratio of multiple components. One part can represent any unit mass, such as 1g or 2.689g. If we say that component A has "a" parts by mass and component B has "b" parts by mass, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it can mean that the mass of component A is aK and the mass of component B is bK (K is any number representing a multiplier). It is important to understand that, unlike the number of parts by mass, the sum of the mass parts of all components is not limited to 100 parts.

[0045] "And / or" is used to indicate that one or both of the described situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0046] The first aspect of this application provides an integrated coating with intelligent thermal control and infrared stealth functions, including a stacked metal bonding layer, a thermochromic radiation layer and a heat-sensitive layer;

[0047] The metal bonding layer comprises an MCrAlY alloy;

[0048] The thermochromic radiation layer comprises lanthanum manganate-based ceramics.

[0049] The heat-sensitive layer comprises a metal with low emission and low absorption properties;

[0050] M in the MCrAlY alloy includes nickel and / or cobalt;

[0051] The composition of the lanthanum manganate system ceramic includes La. 1-x A x MnO3, wherein A includes one or more of Sr, Ba and Ca, and x ranges from 0.1 to 0.3;

[0052] In some embodiments, x can be any value between 0.1, 0.15, 0.2, 0.25, 0.3, or 0.1-0.3;

[0053] The metal includes one or more of Pt, Ag, Cu, and Al.

[0054] It should be noted that the metal bonding layer provided in this application can form a good interlayer bond with the aluminum alloy substrate commonly used in spacecraft, ensuring the service life and bonding strength of the coating under temperature alternation environment.

[0055] In some embodiments, the integrated intelligent thermal control-infrared stealth coating satisfies at least one of the following conditions:

[0056] A. The thickness of the metal bonding layer is 50μm-150μm;

[0057] Optionally, the thickness of the metal bonding layer can be any value between 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm or 50μm-150μm;

[0058] It is important to note that when the thickness of the metal bonding layer is 50μm-150μm, it can effectively increase the bonding strength between the thermochromic radiation layer and the substrate, while also improving the difference in the coefficient of thermal expansion between the layer and the substrate, so that it will not break or peel off in the use environment with alternating temperatures, thus extending the service life of the coating.

[0059] B. The thickness of the thermochromic radiation layer is 100μm-200μm;

[0060] Optionally, the thickness of the thermochromic radiation layer can be any value between 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm or 100 μm-200 μm;

[0061] It is worth noting that the coating structure can maintain optimal thermochromic radiation characteristics and bonding with the metal bonding layer and heat-sensitive layer when the thickness of the thermochromic radiation layer is 100μm-200μm. If it is too thick, the interlayer bonding of the coating will be weak and it will be easy to peel off in the alternating hot and cold environment; if it is too thin, the emissivity change value of the coating will be reduced.

[0062] C. The thickness of the heat-sensitive layer is 200nm-300nm.

[0063] Optionally, the thickness of the heat-sensitive layer can be any value between 200nm, 210nm, 220nm, 230nm, 240nm, 250nm, 260nm, 270nm, 280nm, 290nm, 300nm, or 200nm-300nm.

[0064] It is worth noting that when the thickness of the heat-sensitive layer is 200nm-300nm, it can play a supplementary role in the emissivity regulation of the thermochromic radiation layer. The heat-sensitive layer is made of metal, which has the characteristics of low emission and low absorption, giving the coating infrared stealth function. In addition, by changing the thickness of this layer, the upper and lower limits of the emissivity of the entire coating as a function of temperature can be adjusted, so that the range of emissivity variation can be shifted to a lower trend.

[0065] This can be understood as follows: metallic materials have a much higher thermal conductivity and lower emissivity than ceramics, enabling them to rapidly conduct changes in ambient temperature to the thermochromic radiation layer while maintaining low absorption and low emission characteristics. When the thickness of the heat-sensitive layer is between 200nm and 300nm, the coating exhibits low absorption and low emission characteristics, with very little change in emissivity near the phase transition temperature of the thermochromic radiation layer. However, when the thickness of the heat-sensitive layer is thinner (nanometer-scale), the emissivity of the entire coating is more significantly affected by the thermochromic radiation layer, and its range of emissivity variation will adjust with changes in the phase transition temperature. The phase transition temperature, in turn, changes with the doping elements and doping content of the lanthanum manganate system. For example, the emissivity of a single thermochromic radiation layer can change from 0.45 to 0.80 at -180℃ to 180℃. After adding a heat-sensitive layer with a thickness of about 200nm, the overall emissivity will decrease by about 0.1-0.2, that is, the emissivity changes from 0.35 to 0.70 at -180℃ to 180℃. However, when the thickness of the heat-sensitive layer reaches less than 200nm, especially at the micrometer level, the emissivity changes from 0.25 to 0.45 at -180℃ to 180℃.

[0066] In some embodiments, the porosity of the thermochromic radiation layer is 10%-15%.

[0067] Optionally, the porosity of the thermochromic radiation layer can be any value between 10%, 11%, 12%, 13%, 14%, 15%, or 10%-15%.

[0068] It is worth noting that when the porosity of the thermochromic radiation layer is 10%-15%, it helps the coating to extend its lifespan under alternating hot and cold environments and reduces the possibility of premature failure and peeling due to thermal stress.

[0069] A second aspect of this application provides a method for preparing the integrated coating with intelligent thermal control and infrared stealth functions, comprising:

[0070] The MCrAlY alloy is first sprayed onto the substrate using a supersonic spraying process and / or a plasma spraying process to obtain the metal bonding layer.

[0071] The lanthanum manganate system ceramic is subjected to the plasma spraying process to be second-sprayed onto the metal bonding layer, and then sintered to obtain the thermochromic radiation layer.

[0072] Under vacuum conditions, the metal is sputtered onto the thermochromic radiation layer using a magnetron sputtering process, and then annealed to obtain the integrated coating with intelligent thermal control and infrared stealth functions.

[0073] In some embodiments, the preparation method of the integrated intelligent thermal control-infrared stealth coating satisfies at least one of the following conditions:

[0074] A. During the first spraying, the spraying distance in the supersonic spraying process is 300mm-400mm, the powder feeding rate is 3r / min-5r / min, the kerosene is 4L / h-6L / h, and the oxygen is 1500L / min-2000L / min;

[0075] Optionally, during the first spraying, the spray distance in the supersonic spraying process can be any value between 300mm, 310mm, 320mm, 330mm, 340mm, 350mm, 360mm, 370mm, 380mm, 390mm, 400mm, or 300mm-400mm, and the powder feed rate can be 3r / min, 3.5r / min, 4r / min, 4.5r / min, 5r / min, or 3r / min. The speed can be any value between 1 / min and 5 r / min; for kerosene, it can be any value between 4 L / h, 4.5 L / h, 5 L / h, 5.5 L / h, 6 L / h, or between 4 L / h and 6 L / h; for oxygen, it can be any value between 1500 L / min, 1600 L / min, 1700 L / min, 1800 L / min, 1900 L / min, 2000 L / min, or between 1500 L / min and 2000 L / min.

[0076] B. During the first spraying, the spraying distance in the plasma spraying process is 130mm-150mm, the power is 35kW-42kW, the powder feeding rate is 1.5r / min-2.5r / min, and the operating current is 530A-550A.

[0077] Optionally, during the first spraying, the spray distance in the plasma spraying process can be any value between 130mm, 135mm, 140mm, 145mm, 150mm, or 130mm-150mm; the power can be any value between 35kW, 36kW, 37kW, 38kW, 39kW, 40kW, 41kW, 42kW, or 35kW-42kW; the powder feeding rate can be any value between 1.5r / min, 1.6r / min, 1.7r / min, 1.8r / min, 1.9r / min, 2.0r / min, 2.1r / min, 2.2r / min, 2.3r / min, 2.4r / min, 2.5r / min, or 1.5r / min-2.5r / min; and the operating current can be any value between 530A, 535A, 540A, 545A, 550A, or 530A-550A.

[0078] In some embodiments, the power of the second spraying is 20kW-30kW, the operating current of the second spraying is 600A-700A, the powder feeding rate of the second spraying is 2r / min-9r / min, and the spraying distance is 170mm-190mm.

[0079] Optionally, the power of the second spraying can be any value between 20kW, 21kW, 22kW, 23kW, 24kW, 25kW, 26kW, 27kW, 28kW, 29kW, 30kW, or 20kW-30kW, and the operating current can be 600A, 610A, 620A, 630A, 640A, 650A, 660A, 670A, 680A, 690A, 700A, or 600A. The powder feeding rate can be any value between -700A and 2r / min, 3r / min, 4r / min, 5r / min, 6r / min, 7r / min, 8r / min, 9r / min or any value between 2r / min and 9r / min, and the second spraying distance can be any value between 170mm, 175mm, 180mm, 185mm, 190mm or any value between 170mm and 190mm.

[0080] In some embodiments, the sputtering gas pressure is 0.8 Pa to 1.5 Pa, the sputtering power is 100 W to 200 W, and the sputtering rotary table speed is 3 r / min to 5 r / min.

[0081] Optionally, the sputtering gas pressure can be any value between 0.8Pa, 0.9Pa, 1.0Pa, 1.1Pa, 1.2Pa, 1.3Pa, 1.4Pa, 1.5Pa, or 0.8Pa-1.5Pa; the sputtering power can be any value between 100W, 110W, 120W, 130W, 140W, 150W, 160W, 170W, 180W, 190W, 200W, or 100W-200W; and the sputtering rotary table speed can be any value between 3r / min, 3.5r / min, 4r / min, 4.5r / min, 5r / min, or 3r / min-5r / min.

[0082] In some embodiments, the sintering temperature is 850℃-900℃, and the sintering holding time is 0.5h-1h.

[0083] Optionally, the sintering temperature can be any value between 850℃, 860℃, 870℃, 880℃, 890℃, 900℃ or 850℃-900℃, and the sintering holding time can be any value between 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h or 0.5h-1h.

[0084] It should be noted that when the sintering temperature is 850℃-900℃ and the holding time is 0.5h-1h, the crystallinity of the lanthanum manganate system material can be enhanced, the diffraction peak broadening phenomenon caused by the spraying process can be improved, and the thermochromic radiation characteristics of the material can be ensured.

[0085] In some embodiments, the preparation method of the integrated intelligent thermal control-infrared stealth coating satisfies at least one of the following conditions:

[0086] A. The annealing temperature is 300℃-400℃, and the annealing time is 2h-4h;

[0087] Optionally, the annealing temperature can be any value between 300℃, 310℃, 320℃, 330℃, 340℃, 350℃, 360℃, 370℃, 380℃, 390℃, 400℃ or 300℃-400℃, and the annealing time can be any value between 2h, 2.5h, 3h, 3.5h, 4h or 2h-4h.

[0088] It should be noted that when the annealing temperature is 300℃-400℃ and the time is 2h-4h, the crystallinity of the film can be improved, its electrical properties can be enhanced, and thus its infrared radiation performance can be optimized.

[0089] B. The vacuum level is 1.0 × 10⁻⁶. -4 Pa-1.0×10 -3 Pa.

[0090] Optionally, the vacuum level can be 1.0 × 10⁻⁶. -4 Pa, 2.0×10 -4 Pa, 3.0 × 10 -4 Pa, 4.0 × 10 - 4 Pa, 5.0 × 10 -4 Pa, 6.0×10 -4 Pa, 7.0×10 -4 Pa, 8.0×10 -4 Pa, 9.0 × 10 -4 Pa, 1.0×10 -3 Pa or 1.0 × 10 -4 Pa-1.0×10 -3 Any value between Pa.

[0091] A third aspect of this application provides a spacecraft including the aforementioned integrated coating for intelligent thermal control and infrared stealth functions.

[0092] The implementation schemes of this application will be described in detail below with reference to specific embodiments. However, those skilled in the art will understand that the following embodiments are only for illustrating this application and should not be regarded as limiting the scope of this application. Unless otherwise specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments used without specified manufacturers are all conventional products that can be purchased commercially.

[0093] Example 1

[0094] The first aspect of this embodiment provides an integrated coating with intelligent thermal control and infrared stealth functions, which consists of a stacked metal bonding layer, a thermochromic radiation layer, and a heat-sensitive layer.

[0095] The metal bonding layer is an MCrAlY alloy, where M is nickel, and its thickness is 80 μm.

[0096] The thermochromic radiation layer is a lanthanum manganate-based ceramic with the composition La. 1-x A x MnO3, A is Sr, x is 0.2, thickness is 150 μm, porosity is 10%, and phase transition temperature is in the range of 273±10 K;

[0097] The heat-sensitive layer is a metal with low emission and low absorption characteristics, specifically Al, with a thickness of 200 nm.

[0098] The second aspect of this embodiment provides a method for preparing an integrated coating with intelligent thermal control and infrared stealth functions, including:

[0099] MCrAlY alloy powder was sprayed onto an aluminum alloy substrate using a supersonic spraying process. The spraying distance was 300 mm, the powder feed rate was 3 r / min, the kerosene was 4.5 L / h, and the oxygen was 1700 L / min, resulting in a metal bonding layer.

[0100] Lanthanum manganate ceramics were sprayed onto a metal bonding layer using a plasma spraying process. The spraying power was 30 kW, the working current was 630 A, the powder feeding rate was 2.5 r / min, and the spraying distance was 170 mm. A thermochromic radiation layer was obtained by sintering at a temperature of 870 °C and a holding time of 0.5 h.

[0101] Under vacuum conditions, the vacuum level is 1.0 × 10⁻⁶. -4 At a pressure of 0.8 Pa, the above-mentioned metal was sputtered onto the thermochromic radiation layer using magnetron sputtering. The sputtering gas pressure was 0.8 Pa, the power was 120 W, and the turntable speed was 3 r / min. The resulting coating, which integrates intelligent thermal control and infrared stealth functions, was annealed at a temperature of 300 °C for 4 hours.

[0102] The integrated coating structure with intelligent thermal control and infrared stealth functions prepared in this embodiment is as follows: Figure 1 As shown.

[0103] The emissivity of the integrated intelligent thermal control and infrared stealth coating as a function of temperature was tested, and the test results are as follows: Figure 2 As shown, the emissivity change of this integrated intelligent thermal control and infrared stealth coating was tested within a temperature range of -180℃ to 180℃, and the measured emissivity change value was 0.389.

[0104] Example 2

[0105] The first aspect of this embodiment provides an integrated coating with intelligent thermal control and infrared stealth functions, which consists of a stacked metal bonding layer, a thermochromic radiation layer, and a heat-sensitive layer.

[0106] The metal bonding layer is an MCrAlY alloy, where M is nickel-cobalt, and its thickness is 100 μm.

[0107] The thermochromic radiation layer is a lanthanum manganate-based ceramic with the composition La. 1-x A x MnO3, A is Ba, x is 0.15, thickness is 100 μm, porosity is 13%;

[0108] The heat-sensitive layer is a metal with low emission and low absorption characteristics, specifically Cu, with a thickness of 250 nm.

[0109] The second aspect of this embodiment provides a method for preparing an integrated coating with intelligent thermal control and infrared stealth functions, including:

[0110] MCrAlY alloy powder was sprayed onto an aluminum alloy substrate using a supersonic spraying process. The spraying distance was 350 mm, the powder feed rate was 4 r / min, the kerosene was 5 L / h, and the oxygen was 1800 L / min, resulting in a metal bonding layer.

[0111] Lanthanum manganate ceramics were sprayed onto a metal bonding layer using a plasma spraying process. The spraying power was 25 kW, the working current was 650 A, the powder feeding rate was 3.5 r / min, and the spraying distance was 180 mm. A thermochromic radiation layer was obtained by sintering at a temperature of 850 °C and a holding time of 1 h.

[0112] Under vacuum conditions, the vacuum level is 0.8 × 10⁻⁶. -3 At a pressure of 1.0 Pa, the above-mentioned metal was sputtered onto the thermochromic radiation layer using magnetron sputtering. The sputtering gas pressure was 1.0 Pa, the power was 150 W, and the turntable speed was 4 r / min. The resulting coating, which integrates intelligent thermal control and infrared stealth functions, was annealed at a temperature of 350 °C for 3 h.

[0113] The emissivity change of the integrated coating for intelligent thermal control and infrared stealth functions was tested in the temperature range of -180℃ to 180℃, and the measured emissivity change value was 0.386.

[0114] Example 3

[0115] The first aspect of this embodiment provides an integrated coating with intelligent thermal control and infrared stealth functions, which consists of a stacked metal bonding layer, a thermochromic radiation layer, and a heat-sensitive layer.

[0116] The metal bonding layer is an MCrAlY alloy, where M is cobalt, and its thickness is 150 μm.

[0117] The thermochromic radiation layer is a lanthanum manganate-based ceramic with the composition La. 1-x A x MnO3, where A is Ca, x is 0.1, thickness is 200 μm, and porosity is 15%;

[0118] The heat-sensitive layer is a metal with low emission and low absorption characteristics, specifically a PtAg alloy, with a thickness of 300 nm.

[0119] The second aspect of this embodiment provides a method for preparing an integrated coating with intelligent thermal control and infrared stealth functions, including:

[0120] MCrAlY alloy powder was sprayed onto an aluminum alloy substrate using a supersonic spraying process. The spraying distance was 400 mm, the powder feed rate was 4.5 r / min, the kerosene was 6 L / h, and the oxygen was 2000 L / min, resulting in a metal bonding layer.

[0121] Lanthanum manganate ceramics were sprayed onto a metal bonding layer using a plasma spraying process. The spraying power was 30 kW, the working current was 675 A, the powder feeding rate was 5.5 r / min, and the spraying distance was 190 mm. A thermochromic radiation layer was obtained by sintering at a temperature of 900 ℃ and a holding time of 0.5 h.

[0122] Under vacuum conditions, the vacuum level is 1.0 × 10⁻⁶. -3 At a pressure of 1.5 Pa, the above-mentioned metal was sputtered onto the thermochromic radiation layer using magnetron sputtering. The sputtering gas pressure was 1.5 Pa, the power was 200 W, and the turntable speed was 5 r / min. The resulting coating, which integrates intelligent thermal control and infrared stealth functions, was annealed at a temperature of 400 °C for 2 hours.

[0123] The emissivity change of the integrated coating for intelligent thermal control and infrared stealth functions was tested in the temperature range of -180℃ to 180℃, and the measured emissivity change value was 0.379.

[0124] Comparative Example 1

[0125] This comparative example provides a coating that differs from Example 1 in that it does not have a heat-sensitive layer, while other conditions are the same as in Example 1.

[0126] The emissivity change of the coating was tested in the temperature range of -180℃ to 180℃, and the measured emissivity change value was 0.284.

[0127] Comparative Example 2

[0128] This comparative example provides a coating that differs from Example 1 in that the metal bonding layer thickness in this comparative example is 45 μm, while other conditions are the same as in Example 1. This coating is prone to detachment during the preparation of the thermochromic radiation layer and the heat-sensitive layer due to the large difference in the thermal expansion coefficients between the metal and ceramic materials.

[0129] The emissivity change of the coating was tested in the temperature range of -180℃ to 180℃, and the measured emissivity change value was 0.374.

[0130] Comparative Example 3

[0131] This comparative example provides a coating that differs from Example 1 in that the thickness of the thermochromic radiation layer in this comparative example is 50 μm, while other conditions are the same as in Example 1.

[0132] The emissivity change of the coating was tested in the temperature range of -180℃ to 180℃, and the measured emissivity change value was 0.235.

[0133] Comparative Example 4

[0134] This comparative example provides a coating that differs from Example 1 in that the porosity of the thermochromic radiation layer in this comparative example is 5%, while other conditions are the same as in Example 1.

[0135] The emissivity change of the coating was tested in the temperature range of -180℃ to 180℃, and the measured emissivity change value was 0.195.

[0136] Comparative Example 5

[0137] This comparative example provides a coating that differs from Example 1 in that the composition of the thermochromic radiation layer in this comparative example is La. 1-x A x The x value in MnO3 is 0.6, and other conditions are the same as in Example 1.

[0138] The emissivity change of the coating was tested in the temperature range of -180℃ to 180℃, and the measured emissivity change value was 0.105.

[0139] Comparative Example 6

[0140] This comparative example provides a coating that differs from Example 1 in that the heat-sensitive layer in this comparative example is Fe, while other conditions are the same as in Example 1.

[0141] The emissivity change of the coating in the temperature range of -180℃ to 180℃ was tested, and the emissivity change value was measured to be 0.102.

[0142] Comparative Example 7

[0143] This comparative example provides a coating that differs from Example 1 in that the thickness of the heat-sensitive layer in this comparative example is 100 nm, while other conditions are the same as in Example 1.

[0144] The emissivity change of the coating was tested in the temperature range of -180℃ to 180℃, and the measured emissivity change value was 0.233.

[0145] Comparative Example 8

[0146] This comparative example provides a method for preparing a coating, which differs from Example 1 in that the sintering temperature of this comparative example is 700°C, while other conditions are the same as in Example 1.

[0147] The emissivity change of the coating was tested in the temperature range of -180℃ to 180℃, and the measured emissivity change value was 0.125.

[0148] Comparative Example 9

[0149] This comparative example provides a method for preparing a coating, which differs from Example 1 in that the annealing temperature in this comparative example is 250°C, while other conditions are the same as in Example 1.

[0150] The emissivity change of the coating was tested in the temperature range of -180℃ to 180℃, and the measured emissivity change value was 0.114.

[0151] Comparative Example 10

[0152] This comparative example provides a coating that differs from Example 1 in that the metal bonding layer in this comparative example is a NiAlY alloy, while other conditions are the same as in Example 1. This coating is prone to peeling within a temperature range of -180℃ to 180℃.

[0153] The emissivity variation reflects the coating's ability to regulate radiation under alternating temperature environments. The coating can autonomously adjust its emissivity according to temperature, effectively preventing temperature fluctuations caused by external factors. The high emissivity of the coating in high-temperature environments helps dissipate excess heat from the spacecraft through radiation, ensuring that internal precision instruments are not damaged by overheating. Conversely, the low emissivity of the coating in sub-zero temperatures ensures that the spacecraft radiates less heat outward, maintaining a stable temperature for the devices to operate stably.

[0154] As can be seen from the above embodiments and comparative examples, the intelligent thermal control-infrared stealth integrated coating prepared in Example 1 has the largest emissivity change value of 0.389 in the temperature range of -180℃ to 180℃.

[0155] As shown in Comparative Example 1, when no heat-sensitive layer is set, the emissivity change value of the integrated coating of intelligent thermal control and infrared stealth function decreases in the temperature range of -180℃ to 180℃, and it cannot meet the functional requirements of infrared stealth.

[0156] As can be seen from Comparative Examples 2, 3 and 7, if the thickness of each layer of the integrated coating for intelligent thermal control and infrared stealth is too thin, it will affect the bonding between the coating and the substrate and the thermochromic radiation characteristics.

[0157] As can be seen from Comparative Examples 5 and 6, when the composition of the thermochromic radiative layer La... 1-x A x When x in MnO3 is 0.6, x exceeds the doping ratio range for the transition from the insulating state to the metallic state, resulting in a small change in emissivity within the temperature range of -180℃ to 180℃. When the heat-sensitive layer is Fe, its oxidation resistance is inferior to that of Pt, Ag, Cu, and Al, and its emissivity in the medium and low temperature range cannot meet the requirements for infrared stealth.

[0158] Comparative Examples 8 and 9 show that when the heat treatment temperature of the coating is not high enough, the proportion of amorphous phase in the material is too high, which weakens the thermochromic radiation properties of the material. Appropriate sintering and annealing temperatures help to enhance the crystallinity of the material and optimize its thermochromic radiation properties.

[0159] As can be seen from Comparative Example 10, when the metal bonding layer is a NiAlY alloy, the integrated coating of intelligent thermal control and infrared stealth function is prone to peeling when used in a hot and cold alternating environment.

[0160] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.

[0161] Furthermore, those skilled in the art will understand that although some embodiments herein include certain features included in other embodiments but not others, combinations of features from different embodiments are intended to be within the scope of this application and form different embodiments. For example, in the foregoing claims, any of the claimed embodiments can be used in any combination. The information disclosed in this background section is intended only to enhance the understanding of the general background of this application and should not be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.

Claims

1. An integrated coating for intelligent thermal control and infrared stealth functions, characterized in that, It includes a stacked metal bonding layer, a thermochromic radiation layer, and a heat-sensitive layer; The metal bonding layer comprises an MCrAlY alloy; The thermochromic radiation layer comprises lanthanum manganate-based ceramics. The heat-sensitive layer comprises a metal with low emission and low absorption properties; M in the MCrAlY alloy includes nickel and / or cobalt; The composition of the lanthanum manganate system ceramic includes La. 1-x A x MnO3, wherein A includes one or more of Sr, Ba and Ca, and x ranges from 0.1 to 0.3; The metal includes one or more of Pt, Ag, Cu, and Al; The thickness of the heat-sensitive layer is 200nm-300nm; The porosity of the thermochromic radiation layer is 10%-15%.

2. The integrated coating for intelligent thermal control and infrared stealth functions according to claim 1, characterized in that, At least one of the following conditions must be met: A. The thickness of the metal bonding layer is 50μm-150μm; B. The thickness of the thermochromic radiation layer is 100μm-200μm.

3. A method for preparing an integrated coating with intelligent thermal control and infrared stealth functions as described in claim 1 or 2, characterized in that, include: The MCrAlY alloy is first sprayed onto the aluminum alloy substrate using a supersonic spraying process and / or a plasma spraying process to obtain the metal bonding layer. The lanthanum manganate system ceramic is subjected to the plasma spraying process to be second-sprayed onto the metal bonding layer, and then sintered to obtain the thermochromic radiation layer. Under vacuum conditions, the metal is sputtered onto the thermochromic radiation layer using a magnetron sputtering process, and then annealed to obtain the integrated coating with intelligent thermal control and infrared stealth functions. The sintering temperature is 850℃-900℃, and the sintering holding time is 0.5h-1h; The annealing temperature is 300℃-400℃, and the annealing time is 2h-4h.

4. The method for preparing the integrated coating with intelligent thermal control and infrared stealth functions according to claim 3, characterized in that, At least one of the following conditions must be met: A. During the first spraying, the spraying distance in the supersonic spraying process is 300mm-400mm, the powder feeding rate is 3r / min-5r / min, the kerosene is 4L / h-6L / h, and the oxygen is 1500L / min-2000L / min; B. During the first spraying, the spraying distance in the plasma spraying process is 130mm-150mm, the power is 35kW-42kW, the powder feeding rate is 1.5r / min-2.5r / min, and the operating current is 530A-550A.

5. The method for preparing the integrated coating with intelligent thermal control and infrared stealth functions according to claim 3, characterized in that, The power of the second spraying is 20kw-30kw, the working current of the second spraying is 600A-700A, the powder feeding rate of the second spraying is 2r / min-9r / min, and the spraying distance of the second spraying is 170mm-190mm.

6. The method for preparing the integrated coating with intelligent thermal control and infrared stealth functions according to claim 3, characterized in that, The sputtering gas pressure is 0.8Pa-1.5Pa, the sputtering power is 100W-200W, and the sputtering rotary table speed is 3r / min-5r / min.

7. The method for preparing the integrated coating with intelligent thermal control and infrared stealth functions according to any one of claims 3-6, characterized in that, The vacuum level is 1.0 × 10⁻⁶. -4 Pa-1.0×10 -3 Pa.

8. A spacecraft, characterized in that, It includes the integrated coating with intelligent thermal control and infrared stealth functions as described in claim 1 or 2.

Citation Information

Patent Citations

  • Thermochromism coating with variable emissivity and preparation method thereof

    CN103386786A