A biomineral crystal material and preparation method thereof, and a sleep-aiding technology pillow
By modifying the combination of natural mineral crystal materials with TiO2/Fe3O4 intercalated montmorillonite and aromatic essential oil, combined with infrared waves and magnetic fields, the problem of rapid release of ingredients and odor concentration in existing sleep aid pillows is solved, and the essential oil is realized Slow release and improve sleep quality to alleviate insomnia and air pollution.
Patent Information
- Application Number
- CN202410869073.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-01
AI Technical Summary
The active ingredients of natural crystals in the existing sleep aid pillow are released quickly, used for a short time, and the odor concentration of Chinese medicine ingredients is over, resulting in discomfort, making it difficult to effectively relieve insomnia and improve sleep quality for a long time.
Using modified natural mineral crystal materials, spherical particles are prepared by mixing with TiO2/Fe3O4 intercalated montmorillonite, adsorbing aromatic essential oil and sodium alginate embedding on the surface, combining infrared waves and magnetic fields to release negative ions and slowly releasing essential oil molecules. , improve durability and sleep quality.
It realizes the slow release of essential oils, extends service life, improves sleep quality, and uses infrared waves and magnetic fields to soothe air, purifies the air, relieves headaches and insomnia, and improves indoor air quality.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials, and in particular to a biomineral crystal material and a preparation method thereof, and a sleep-aiding technology pillow. Background Art
[0002] With the continuous improvement of living standards, people are paying more and more attention to hygienic, safe and healthy products. As people's pace of life is accelerating and the pressure of life is relatively high, the number of people with poor sleep quality or even insomnia is gradually increasing. There are also many people who suffer from mental weakness caused by poor sleep quality and insomnia, so sleep-aiding pillows came into being.
[0003] Natural crystal is a quartz crystal mineral. Its main chemical component is silicon dioxide, with the chemical formula SiO2. It is also known as water crystal, water jade, and water jade. Well-developed single crystals are hexagonal pyramids, so they are usually blocky or granular aggregates. Natural crystals can affect physical health by generating electromagnetic fields and regulating the human aura, which is the so-called "mineral therapy". Secondly, natural crystals can also collect negative ions from the outside and release them into the surrounding environment, thereby improving indoor air quality and relieving symptoms such as headaches and insomnia.
[0004] However, directly adding natural crystals into pillows does not have a good sleep-aiding effect, so they need to be modified.
[0005] Chinese patent document CN110101268A discloses a filling material and a sleeping pillow for a sleeping aid, which is made by mixing mugwort, dragon vine, rhubarb, lavender and chrysanthemum, making full use of the advantages of each component, and can effectively improve insomnia, help sleep, and help people with dreaminess, difficulty falling asleep, and sleep discomfort to soothe nerves, relieve fatigue, and achieve an ideal deep sleep state. However, the Chinese medicine ingredients are directly placed in the pillow, the effective ingredients are released quickly, the effective use time is shortened, and there is a short-term excessive concentration of odor, which brings discomfort to people. Summary of the invention
[0006] The purpose of the present invention is to provide a biomineral crystal material and a preparation method thereof and a sleep-aiding technology pillow, which can slowly release essential oil molecules and improve durability. At the same time, the spherical particles are also convenient for stimulating acupuncture points, which helps to improve sleep quality. At the same time, by releasing infrared waves and forming a magnetic field, as well as releasing negative ions into the surrounding environment, organic pollutants, formaldehyde, etc. in the air are purified, indoor air quality is improved, and symptoms such as headaches and insomnia are relieved, and the pillow has broad application prospects.
[0007] The technical solution of the present invention is achieved in this way:
[0008] The invention provides a method for preparing a biomineral crystal material. The surface of a natural mineral crystal is modified and then mixed with doped TiO2 / Fe3O4 intercalated montmorillonite to obtain a modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite. The surface is then modified with polydopamine, aromatic essential oil is adsorbed, and the spherical biomineral crystal material is obtained by embedding with sodium alginate.
[0009] As a further improvement of the present invention, the following steps are included:
[0010] S1. Surface modification of natural mineral crystals: ball-milling natural mineral crystals, adding them to ethanol, adding a silane coupling agent, heating and stirring to react, filtering, washing, and drying to obtain surface-modified natural mineral crystal powder;
[0011] S2. Preparation of TiO2 / Fe3O4 doped intercalated montmorillonite modified crystal powder: adding butyl titanate to ethanol to form solution A, dissolving melamine, ferric chloride and ferrous chloride in water to obtain solution B, adding solution B dropwise to solution A, stirring to obtain a pillaring agent, adding dropwise to the montmorillonite suspension, adding ammonia water dropwise at the same time, adding the surface modified natural mineral crystal powder obtained in step S1, heating and stirring to react, standing for aging, microwave heating and drying, washing, ball milling, calcining, and obtaining TiO2 / Fe3O4 doped intercalated montmorillonite modified crystal powder;
[0012] S3. Preparation of modified crystal powder: adding the TiO2 / Fe3O4 intercalated montmorillonite modified crystal powder obtained in step S2 to water, adding dopamine hydrochloride and a catalyst, heating and stirring the reaction, filtering, washing, and drying to obtain modified crystal powder;
[0013] S4 essential oil adsorption: the modified crystal powder obtained in step S3 is added to petroleum ether, the composite aromatic essential oil is added, the solvent is evaporated to obtain a modified crystal powder adsorbing essential oil;
[0014] S5. Preparation of biomineral crystal material: Add the modified crystal powder adsorbing essential oil obtained in step S4 into water, add sodium alginate and an emulsifier to obtain an aqueous phase, drop the aqueous phase into fish oil, emulsify, drop calcium chloride solution, solidify at room temperature, filter, wash, and dry to obtain the biomineral crystal material.
[0015] As a further improvement of the present invention, the ball milling time in step S1 is 0.5-1.5h, the mass ratio of the natural mineral crystals to the silane coupling agent is 50:4-7, the silane coupling agent is selected from at least one of KH550, KH560, KH580, KH590, KH602, and KH792, and the heating and stirring reaction temperature is 40-50°C and the time is 1-3h.
[0016] Preferably, the silane coupling agent is a mixture of KH550 and KH580 in a mass ratio of 7-10:3-5.
[0017] As a further improvement of the present invention, the mass ratio of butyl titanate, melamine, ferric chloride, ferrous chloride, montmorillonite, and surface modified natural mineral crystal powder in step S2 is 5-7:0.5-1:3.4-3.5:1.2-1.3:30-50:100, the temperature of the heating and stirring reaction is 65-75°C, the time is 2-4h, the ball milling time is 1-2h, and the calcination temperature is 450-550°C, and the time is 1-3h.
[0018] As a further improvement of the present invention, the mass ratio of the doped TiO2 / Fe3O4 intercalated montmorillonite modified crystal powder, dopamine hydrochloride and catalyst in step S3 is 20-30:14-18:1-2, the temperature of the heating and stirring reaction is 40-50°C, the time is 2-3h, and the catalyst is a Tris-HCl solution with a pH of 8.5-9.
[0019] As a further improvement of the present invention, the mass ratio of the modified crystal powder and the composite aromatic essential oil in step S4 is 100:15-22, the composite aromatic essential oil is selected from at least two of lemon essential oil, bergamot essential oil, rose essential oil, clove essential oil, lavender essential oil, and wormwood essential oil, and the preparation method of the essential oil is the essential oil obtained by subjecting the raw materials to supercritical fluid extraction.
[0020] Preferably, the composite aromatic essential oil is a mixture of rose essential oil and wormwood essential oil in a mass ratio of 5-7:3-4.
[0021] As a further improvement of the present invention, the mass ratio of the modified crystal powder for adsorbing essential oil, sodium alginate and emulsifier in step S5 is 10-13:17-20:1-2, the emulsifier is selected from at least one of Tween-20, Tween-40, Tween-60, Tween-80 and Tween-85, and the time for room temperature curing is 20-30 min.
[0022] The present invention further protects a biomineral crystal material obtained by the above preparation method.
[0023] The present invention further protects the use of the above-mentioned biomineral crystal material in the preparation of a sleep-aiding product.
[0024] The present invention further protects a technological sleep-aiding pillow, in which the pillow core is filled with the above-mentioned biological mineral crystal material, and the filling amount is 0.01-100wt%.
[0025] The present invention has the following beneficial effects:
[0026] The present invention uses natural mineral crystals to affect physical health by generating electromagnetic fields, regulating the human body's aura, etc., which is the so-called "mineral therapy". Secondly, natural mineral crystals can also collect negative ions from the outside and release them into the surrounding environment, thereby improving indoor air quality and relieving symptoms such as headaches and insomnia. At the same time, natural mineral crystals are modified by silane coupling agents. After modification with KH550 and KH580, the surface of the crystal powder has thiol and amino groups, which can form hydrogen bonds with hydroxyl groups on the surface of montmorillonite and Van der Waals forces, so that the montmorillonite is fixed on the surface of the crystal powder.
[0027] In the preparation of doped TiO2 / Fe3O4 intercalated montmorillonite, the anatase TiO2 not only has good adsorption performance, but also has good photocatalytic performance. Under the doping effect of melamine, TiO2 is doped with N and C atoms, and at the same time, the mercapto group of the silane coupling agent is also doped with S elements, thereby changing the electronic transition energy level of TiO2, so that it can be photocatalytic within the wavelength range of visible light, and has good effects of degrading organic pollutants, purifying formaldehyde, and antibacterial and anti-mite. In addition, magnetic Fe3O4 can also form a magnetic field and emit infrared waves, so that people can have magnetic therapy and infrared wave soothing effects during sleep. At the same time, the interlayer spacing of the montmorillonite doped with TiO2 / Fe3O4 intercalation is increased, which not only maintains the layered structure before intercalation, but also has a layer peeling phenomenon in the structure, thereby increasing the specific surface area of the montmorillonite, thereby helping to improve its adsorption performance, purifying ambient air, and increasing the adsorption rate of aromatic essential oils, and also increasing the sustained release effect of the adsorbed aromatic essential oils.
[0028] The present invention further modifies the surface of the prepared doped TiO2 / Fe3O4 intercalated montmorillonite modified crystal powder with polydopamine, so that the surface has abundant active groups such as hydroxyl, amino, carboxyl, etc., which can interact with the molecules of aromatic essential oils in various ways, thereby improving the adsorption of essential oil molecules, thereby improving its sustained release effect, thereby improving the sleep-inducing effect of the essential oils and the durability of their use.
[0029] The rose essential oil and wormwood essential oil absorbed by the invention not only have a good sleep-inducing effect, but also have antibacterial, anti-moth, anti-mildew and anti-mite effects, thereby improving the durability of the technological pillow and having a synergistic effect.
[0030] The modified crystal powder for adsorbing essential oil is modified by embedding with sodium alginate to obtain spherical embedded particles, which can slowly release the essential oil and improve its durability. Meanwhile, the spherical particles are also convenient for stimulating acupuncture points and help improve sleep quality.
[0031] The technological pillow prepared by adding the biomineral crystal material prepared by the present invention can slowly release essential oil molecules and improve the durability of use. At the same time, the spherical particles are also convenient for stimulating acupuncture points, which helps to improve sleep quality. At the same time, by releasing infrared waves and forming a magnetic field, as well as releasing negative ions into the surrounding environment, organic pollutants, formaldehyde, etc. in the air are purified, indoor air quality is improved, and symptoms such as headaches and insomnia are relieved. The pillow has broad application prospects. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The preparation method of rose and wormwood essential oil is to obtain the essential oil by extracting rose and wormwood through supercritical fluid.
[0034] The natural mineral crystals are mixed ore containing natural mineral crystals and rare earth concentrates in a mass ratio of 10:5. The natural mineral crystals were purchased from Lianyungang Haisheng Quartz Technology Co., Ltd., and the rare earth concentrates were purchased from China North Rare Earth Group High-Tech Co., Ltd.
[0035] Example 1
[0036] This embodiment provides a method for preparing a biomineral crystal material, which specifically includes the following steps:
[0037] S1. Surface modification of natural mineral crystals: 50 parts by weight of natural mineral crystals were ball-milled for 0.5 h, added to 200 parts by weight of ethanol, 4 parts by weight of silane coupling agent were added, heated to 40°C, stirred for 1 h, filtered, washed, and dried to obtain surface-modified natural mineral crystal powder;
[0038] The silane coupling agent is a mixture of KH550 and KH580, with a mass ratio of 7:3;
[0039] S2. Preparation of modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite: 5 parts by weight of butyl titanate were added to 100 parts by weight of ethanol to form a solution A, 0.5 parts by weight of melamine, 3.4 parts by weight of ferric chloride, and 1.2 parts by weight of ferrous chloride were dissolved in 70 parts by weight of water to obtain a solution B, and solution B was added dropwise to solution A, stirred for 10 minutes to obtain a pillaring agent, which was added dropwise to 200 parts by weight of a suspension containing 30 parts by weight of montmorillonite, and 10 parts by weight of 25wt% ammonia water were added dropwise at the same time. Under nitrogen protection, 100 parts by weight of the surface-modified natural mineral crystal powder obtained in step S1 was added, heated to 65°C, stirred for 2h, allowed to stand for aging for 1h, dried by 500W microwave heating, washed, ball milled for 1h, and calcined at 450°C for 1h to obtain modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite;
[0040] S3. Preparation of modified crystal powder: 20 parts by weight of the doped TiO2 / Fe3O4 intercalated montmorillonite modified crystal powder obtained in step S2 was added to 100 parts by weight of water, 14 parts by weight of dopamine hydrochloride and 1 part by weight of a catalyst were added, heated to 40 ° C, stirred for 2 h, filtered, washed, and dried to obtain a modified crystal powder;
[0041] The catalyst is a Tris-HCl solution with a pH of 8.5;
[0042] S4 essential oil adsorption: 100 parts by weight of the modified crystal powder obtained in step S3 was added to 100 parts by weight of petroleum ether, 15 parts by weight of the composite aromatic essential oil was added, and the solvent was evaporated to obtain a modified crystal powder adsorbed essential oil;
[0043] The composite aromatic essential oil is a mixture of rose essential oil and wormwood essential oil, with a mass ratio of 5:3;
[0044] S5. Preparation of biomineral crystal material: add 10 parts by weight of the modified crystal powder for adsorbing essential oil obtained in step S4 to 200 parts by weight of water, add 17 parts by weight of sodium alginate and 1 part by weight of Tween-20 to obtain an aqueous phase, add the aqueous phase dropwise to 500 parts by weight of fish oil, emulsify at 10,000 r / min for 15 minutes, add dropwise 10 parts by weight of 3wt% calcium chloride solution, cure at room temperature for 20 minutes, filter, wash, and dry to obtain the biomineral crystal material.
[0045] Example 2
[0046] This embodiment provides a method for preparing a biomineral crystal material, which specifically includes the following steps:
[0047] S1. Surface modification of natural mineral crystals: 50 parts by weight of natural mineral crystals were ball-milled for 1.5 h, added to 200 parts by weight of ethanol, added with 7 parts by weight of silane coupling agent, heated to 50 ° C, stirred for 3 h, filtered, washed, and dried to obtain surface-modified natural mineral crystal powder;
[0048] The silane coupling agent is a mixture of KH550 and KH580, with a mass ratio of 10:5;
[0049] S2. Preparation of modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite: 7 parts by weight of butyl titanate was added to 100 parts by weight of ethanol to form a solution A, 1 part by weight of melamine, 3.5 parts by weight of ferric chloride, and 1.3 parts by weight of ferrous chloride were dissolved in 70 parts by weight of water to obtain a solution B, and solution B was added dropwise to solution A, stirred for 10 minutes to obtain a pillaring agent, which was added dropwise to 200 parts by weight of a suspension containing 50 parts by weight of montmorillonite, and 20 parts by weight of 28wt% ammonia was added dropwise at the same time. Under nitrogen protection, 100 parts by weight of the surface-modified natural mineral crystal powder obtained in step S1 was added, heated to 75°C, stirred for 4h, allowed to stand for aging for 1h, dried by 500W microwave heating, washed, ball milled for 2h, and calcined at 550°C for 3h to obtain modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite;
[0050] S3. Preparation of modified crystal powder: 30 parts by weight of the doped TiO2 / Fe3O4 intercalated montmorillonite modified crystal powder obtained in step S2 was added to 100 parts by weight of water, 18 parts by weight of dopamine hydrochloride and 2 parts by weight of a catalyst were added, heated to 50 ° C, stirred for 3 h, filtered, washed, and dried to obtain a modified crystal powder;
[0051] The catalyst is a Tris-HCl solution with a pH of 9;
[0052] S4 essential oil adsorption: 100 parts by weight of the modified crystal powder obtained in step S3 was added to 100 parts by weight of petroleum ether, 22 parts by weight of the composite aromatic essential oil was added, and the solvent was evaporated to obtain a modified crystal powder adsorbed essential oil;
[0053] The composite aromatic essential oil is a mixture of rose essential oil and wormwood essential oil, with a mass ratio of 74;
[0054] S5. Preparation of biomineral crystal material: add 13 parts by weight of the modified crystal powder for adsorbing essential oil obtained in step S4 to 200 parts by weight of water, add 20 parts by weight of sodium alginate and 2 parts by weight of Tween-40 to obtain an aqueous phase, add the aqueous phase dropwise to 500 parts by weight of fish oil, emulsify at 10,000 r / min for 15 minutes, add dropwise 10 parts by weight of 3wt% calcium chloride solution, cure at room temperature for 30 minutes, filter, wash, and dry to obtain the biomineral crystal material.
[0055] Example 3
[0056] This embodiment provides a method for preparing a biomineral crystal material, which specifically includes the following steps:
[0057] S1. Surface modification of natural mineral crystals: 50 parts by weight of natural mineral crystals were ball-milled for 1 hour, added to 200 parts by weight of ethanol, 5 parts by weight of silane coupling agent were added, heated to 45°C, stirred for reaction for 2 hours, filtered, washed, and dried to obtain surface-modified natural mineral crystal powder;
[0058] The silane coupling agent is a mixture of KH550 and KH580, with a mass ratio of 8:4;
[0059] S2. Preparation of modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite: 6 parts by weight of butyl titanate were added to 100 parts by weight of ethanol to form solution A, 0.7 parts by weight of melamine, 3.46 parts by weight of ferric chloride, and 1.26 parts by weight of ferrous chloride were dissolved in 70 parts by weight of water to obtain solution B, solution B was added dropwise to solution A, stirred for 10 min, a pillaring agent was obtained, and added dropwise to 200 parts by weight of a suspension containing 40 parts by weight of montmorillonite, and 15 parts by weight of 26wt% ammonia water were added dropwise, and under nitrogen protection, 100 parts by weight of the surface-modified natural mineral crystal powder obtained in step S1 was added, heated to 70°C, stirred for reaction for 3h, allowed to stand for aging for 1h, dried by 500W microwave heating, washed, ball milled for 1.5h, and calcined at 500°C for 2h to obtain modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite;
[0060] S3. Preparation of modified crystal powder: 25 parts by weight of the doped TiO2 / Fe3O4 intercalated montmorillonite modified crystal powder obtained in step S2 was added to 100 parts by weight of water, 16 parts by weight of dopamine hydrochloride and 1.5 parts by weight of a catalyst were added, heated to 45 ° C, stirred for 2.5 h, filtered, washed, and dried to obtain a modified crystal powder;
[0061] The catalyst is a Tris-HCl solution with a pH of 8.7;
[0062] S4 essential oil adsorption: 100 parts by weight of the modified crystal powder obtained in step S3 was added to 100 parts by weight of petroleum ether, 19 parts by weight of the composite aromatic essential oil was added, and the solvent was evaporated to obtain a modified crystal powder adsorbed essential oil;
[0063] The composite aromatic essential oil is a mixture of rose essential oil and wormwood essential oil, with a mass ratio of 6:3.5;
[0064] S5. Preparation of biomineral crystal material: add 11 parts by weight of the modified crystal powder for adsorbing essential oil obtained in step S4 to 200 parts by weight of water, add 180 parts by weight of sodium alginate and 1.2 parts by weight of Tween-85 to obtain an aqueous phase, add the aqueous phase dropwise to 500 parts by weight of fish oil, emulsify at 10,000 r / min for 15 minutes, add dropwise 10 parts by weight of 3wt% calcium chloride solution, cure at room temperature for 25 minutes, filter, wash, and dry to obtain the biomineral crystal material.
[0065] Example 4
[0066] Compared with Example 3, the difference is that the silane coupling agent is a single KH550.
[0067] Example 5
[0068] Compared with Example 3, the difference is that the silane coupling agent is a single KH580.
[0069] Comparative Example 1
[0070] Compared with Example 3, the difference is that step S1 is not performed.
[0071] The details are as follows:
[0072] S1. Preparation of modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite: 6 parts by weight of butyl titanate were added to 100 parts by weight of ethanol to form solution A, 0.7 parts by weight of melamine, 3.46 parts by weight of ferric chloride and 1.26 parts by weight of ferrous chloride were dissolved in 70 parts by weight of water to obtain solution B, solution B was added dropwise to solution A, stirred for 10 minutes to obtain a pillaring agent, and then added dropwise to 200 parts by weight of a suspension containing 40 parts by weight of montmorillonite, and 15 parts by weight of 26wt% ammonia water were added dropwise at the same time, and 100 parts by weight of natural mineral crystal powder were added under nitrogen protection, heated to 70°C, stirred for reaction for 3h, allowed to stand for aging for 1h, dried by 500W microwave heating, washed, ball milled for 1.5h, and calcined at 500°C for 2h to obtain modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite;
[0073] S2. Preparation of modified crystal powder: 25 parts by weight of the doped TiO2 / Fe3O4 intercalated montmorillonite modified crystal powder obtained in step S1 was added to 100 parts by weight of water, 16 parts by weight of dopamine hydrochloride and 1.5 parts by weight of catalyst were added, heated to 45 ° C, stirred for 2.5h, filtered, washed and dried to obtain modified crystal powder;
[0074] The catalyst is a Tris-HCl solution with a pH of 8.7;
[0075] S3 essential oil adsorption: 100 parts by weight of the modified crystal powder obtained in step S2 was added to 100 parts by weight of petroleum ether, 19 parts by weight of the composite aromatic essential oil was added, and the solvent was evaporated to obtain a modified crystal powder adsorbed essential oil;
[0076] The composite aromatic essential oil is a mixture of rose essential oil and wormwood essential oil, with a mass ratio of 6:3.5;
[0077] S4. Preparation of biomineral crystal material: add 11 parts by weight of the modified crystal powder for adsorbing essential oil obtained in step S3 to 200 parts by weight of water, add 180 parts by weight of sodium alginate and 1.2 parts by weight of Tween-85 to obtain an aqueous phase, add the aqueous phase dropwise to 500 parts by weight of fish oil, emulsify at 10,000 r / min for 15 minutes, add dropwise 10 parts by weight of 3wt% calcium chloride solution, cure at room temperature for 25 minutes, filter, wash, and dry to obtain the biomineral crystal material.
[0078] Comparative Example 2
[0079] Compared with Example 3, the difference is that melamine is not added in step S2.
[0080] The details are as follows:
[0081] S2. Preparation of TiO2 / Fe3O4 intercalated montmorillonite modified crystal powder: add 6 parts by weight of butyl titanate to 100 parts by weight of ethanol to form solution A, dissolve 3.46 parts by weight of ferric chloride and 1.26 parts by weight of ferrous chloride in 70 parts by weight of water to obtain solution B, add solution B dropwise into solution A, stir for 10 minutes to obtain a pillaring agent, add dropwise into 200 parts by weight of a suspension containing 40 parts by weight of montmorillonite, and at the same time, add dropwise 15 parts by weight of 26wt% ammonia water, and under nitrogen protection, add 100 parts by weight of the surface modified natural mineral crystal powder obtained in step S1, heat to 70°C, stir to react for 3 hours, let stand for aging for 1 hour, dry with 500W microwave heating, wash, ball mill for 1.5 hours, and calcine at 500°C for 2 hours to obtain TiO2 / Fe3O4 intercalated montmorillonite modified crystal powder.
[0082] Comparative Example 3
[0083] Compared with Example 3, the difference is that ferric chloride and ferrous chloride are not added in step S2.
[0084] The details are as follows:
[0085] S2. Preparation of modified crystal powder of doped TiO2 intercalated montmorillonite: add 10.72 parts by weight of butyl titanate to 100 parts by weight of ethanol to form solution A, dissolve 0.7 parts by weight of melamine in 70 parts by weight of water to obtain solution B, add solution B dropwise to solution A, stir for 10 minutes to obtain a pillaring agent, add dropwise to 200 parts by weight of a suspension containing 40 parts by weight of montmorillonite, and at the same time add dropwise 15 parts by weight of 26wt% ammonia water, under nitrogen protection, add 100 parts by weight of the surface modified natural mineral crystal powder obtained in step S1, heat to 70°C, stir to react for 3 hours, let stand for aging for 1 hour, dry with 500W microwave heating, wash, ball mill for 1.5 hours, and calcine at 500°C for 2 hours to obtain modified crystal powder of doped TiO2 intercalated montmorillonite.
[0086] Comparative Example 4
[0087] Compared with Example 3, the difference is that step S2 is not performed.
[0088] The details are as follows:
[0089] S1. Surface modification of natural mineral crystals: 50 parts by weight of natural mineral crystals were ball-milled for 1 hour, added to 200 parts by weight of ethanol, 5 parts by weight of silane coupling agent were added, heated to 45°C, stirred for reaction for 2 hours, filtered, washed, and dried to obtain surface-modified natural mineral crystal powder;
[0090] The silane coupling agent is a mixture of KH550 and KH580, with a mass ratio of 8:4;
[0091] S2. Preparation of modified crystal powder: 25 parts by weight of the surface-modified natural mineral crystal powder obtained in step S1 was added to 100 parts by weight of water, 16 parts by weight of dopamine hydrochloride and 1.5 parts by weight of a catalyst were added, heated to 45 ° C, stirred for 2.5 h, filtered, washed, and dried to obtain a modified crystal powder;
[0092] The catalyst is a Tris-HCl solution with a pH of 8.7;
[0093] S3 essential oil adsorption: 100 parts by weight of the modified crystal powder obtained in step S2 was added to 100 parts by weight of petroleum ether, 19 parts by weight of the composite aromatic essential oil was added, and the solvent was evaporated to obtain a modified crystal powder adsorbed essential oil;
[0094] The composite aromatic essential oil is a mixture of rose essential oil and wormwood essential oil, with a mass ratio of 6:3.5;
[0095] S4. Preparation of biomineral crystal material: add 11 parts by weight of the modified crystal powder for adsorbing essential oil obtained in step S3 to 200 parts by weight of water, add 180 parts by weight of sodium alginate and 1.2 parts by weight of Tween-85 to obtain an aqueous phase, add the aqueous phase dropwise to 500 parts by weight of fish oil, emulsify at 10,000 r / min for 15 minutes, add dropwise 10 parts by weight of 3wt% calcium chloride solution, cure at room temperature for 25 minutes, filter, wash, and dry to obtain the biomineral crystal material.
[0096] Comparative Example 5
[0097] Compared with Example 3, the difference is that step S3 is not performed.
[0098] The details are as follows:
[0099] S1. Surface modification of natural mineral crystals: 50 parts by weight of natural mineral crystals were ball-milled for 1 hour, added to 200 parts by weight of ethanol, 5 parts by weight of silane coupling agent were added, heated to 45°C, stirred for reaction for 2 hours, filtered, washed, and dried to obtain surface-modified natural mineral crystal powder;
[0100] The silane coupling agent is a mixture of KH550 and KH580, with a mass ratio of 8:4;
[0101] S2. Preparation of modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite: 6 parts by weight of butyl titanate were added to 100 parts by weight of ethanol to form solution A, 0.7 parts by weight of melamine, 3.46 parts by weight of ferric chloride, and 1.26 parts by weight of ferrous chloride were dissolved in 70 parts by weight of water to obtain solution B, solution B was added dropwise to solution A, stirred for 10 min, a pillaring agent was obtained, and added dropwise to 200 parts by weight of a suspension containing 40 parts by weight of montmorillonite, and 15 parts by weight of 26wt% ammonia water were added dropwise, and under nitrogen protection, 100 parts by weight of the surface-modified natural mineral crystal powder obtained in step S1 was added, heated to 70°C, stirred for reaction for 3h, allowed to stand for aging for 1h, dried by 500W microwave heating, washed, ball milled for 1.5h, and calcined at 500°C for 2h to obtain modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite;
[0102] S3 essential oil adsorption: 100 parts by weight of the doped TiO2 / Fe3O4 intercalated montmorillonite modified crystal powder obtained in step S2 was added to 100 parts by weight of petroleum ether, 19 parts by weight of the composite aromatic essential oil was added, the solvent was evaporated to obtain a modified crystal powder adsorbed essential oil;
[0103] The composite aromatic essential oil is a mixture of rose essential oil and wormwood essential oil, with a mass ratio of 6:3.5;
[0104] S4. Preparation of biomineral crystal material: add 11 parts by weight of the modified crystal powder for adsorbing essential oil obtained in step S3 to 200 parts by weight of water, add 180 parts by weight of sodium alginate and 1.2 parts by weight of Tween-85 to obtain an aqueous phase, add the aqueous phase dropwise to 500 parts by weight of fish oil, emulsify at 10,000 r / min for 15 minutes, add dropwise 10 parts by weight of 3wt% calcium chloride solution, cure at room temperature for 25 minutes, filter, wash, and dry to obtain the biomineral crystal material.
[0105] Comparative Example 6
[0106] Compared with Example 3, the difference is that step S4 is not performed.
[0107] The details are as follows:
[0108] S1. Surface modification of natural mineral crystals: 50 parts by weight of natural mineral crystals were ball-milled for 1 hour, added to 200 parts by weight of ethanol, 5 parts by weight of silane coupling agent were added, heated to 45°C, stirred for reaction for 2 hours, filtered, washed, and dried to obtain surface-modified natural mineral crystal powder;
[0109] The silane coupling agent is a mixture of KH550 and KH580, with a mass ratio of 8:4;
[0110] S2. Preparation of modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite: 6 parts by weight of butyl titanate were added to 100 parts by weight of ethanol to form solution A, 0.7 parts by weight of melamine, 3.46 parts by weight of ferric chloride, and 1.26 parts by weight of ferrous chloride were dissolved in 70 parts by weight of water to obtain solution B, solution B was added dropwise to solution A, stirred for 10 min, a pillaring agent was obtained, and added dropwise to 200 parts by weight of a suspension containing 40 parts by weight of montmorillonite, and 15 parts by weight of 26wt% ammonia water were added dropwise, and under nitrogen protection, 100 parts by weight of the surface-modified natural mineral crystal powder obtained in step S1 was added, heated to 70°C, stirred for reaction for 3h, allowed to stand for aging for 1h, dried by 500W microwave heating, washed, ball milled for 1.5h, and calcined at 500°C for 2h to obtain modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite;
[0111] S3. Preparation of modified crystal powder: 25 parts by weight of the doped TiO2 / Fe3O4 intercalated montmorillonite modified crystal powder obtained in step S2 was added to 100 parts by weight of water, 16 parts by weight of dopamine hydrochloride and 1.5 parts by weight of a catalyst were added, heated to 45 ° C, stirred for 2.5 h, filtered, washed, and dried to obtain a modified crystal powder;
[0112] The catalyst is a Tris-HCl solution with a pH of 8.7;
[0113] S4. Preparation of biomineral crystal material: add 11 parts by weight of the modified crystal powder obtained in step S3 to 200 parts by weight of water, add 180 parts by weight of sodium alginate and 1.2 parts by weight of Tween-85 to obtain an aqueous phase, add the aqueous phase dropwise into 500 parts by weight of fish oil, emulsify at 10,000 r / min for 15 minutes, add dropwise 10 parts by weight of 3wt% calcium chloride solution, cure at room temperature for 25 minutes, filter, wash, and dry to obtain the biomineral crystal material.
[0114] Comparative Example 7
[0115] Compared with Embodiment 3, the difference is that step S5 is not performed.
[0116] The details are as follows:
[0117] S1. Surface modification of natural mineral crystals: 50 parts by weight of natural mineral crystals were ball-milled for 1 hour, added to 200 parts by weight of ethanol, 5 parts by weight of silane coupling agent were added, heated to 45°C, stirred for reaction for 2 hours, filtered, washed, and dried to obtain surface-modified natural mineral crystal powder;
[0118] The silane coupling agent is a mixture of KH550 and KH580, with a mass ratio of 8:4;
[0119] S2. Preparation of modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite: 6 parts by weight of butyl titanate were added to 100 parts by weight of ethanol to form solution A, 0.7 parts by weight of melamine, 3.46 parts by weight of ferric chloride, and 1.26 parts by weight of ferrous chloride were dissolved in 70 parts by weight of water to obtain solution B, solution B was added dropwise to solution A, stirred for 10 min, a pillaring agent was obtained, and added dropwise to 200 parts by weight of a suspension containing 40 parts by weight of montmorillonite, and 15 parts by weight of 26wt% ammonia water were added dropwise, and under nitrogen protection, 100 parts by weight of the surface-modified natural mineral crystal powder obtained in step S1 was added, heated to 70°C, stirred for reaction for 3h, allowed to stand for aging for 1h, dried by 500W microwave heating, washed, ball milled for 1.5h, and calcined at 500°C for 2h to obtain modified crystal powder of doped TiO2 / Fe3O4 intercalated montmorillonite;
[0120] S3. Preparation of modified crystal powder: 25 parts by weight of the doped TiO2 / Fe3O4 intercalated montmorillonite modified crystal powder obtained in step S2 was added to 100 parts by weight of water, 16 parts by weight of dopamine hydrochloride and 1.5 parts by weight of a catalyst were added, heated to 45 ° C, stirred for 2.5 h, filtered, washed, and dried to obtain a modified crystal powder;
[0121] The catalyst is a Tris-HCl solution with a pH of 8.7;
[0122] S4 essential oil adsorption: 100 parts by weight of the modified crystal powder obtained in step S3 was added to 100 parts by weight of petroleum ether, 19 parts by weight of the composite aromatic essential oil was added, the solvent was evaporated to obtain a modified crystal powder adsorbed essential oil, that is, a biomineral crystal material;
[0123] The composite aromatic essential oil is a mixture of rose essential oil and wormwood essential oil, with a mass ratio of 6:3.5.
[0124] Test Example 1
[0125] The biomineral crystal materials prepared in Examples 1-5 and Comparative Examples 1-7 of the present invention were measured for their dual-band infrared emissivity of 3μm-5μm and 8μm-14μm at room temperature using an IR-2 dual-band emissivity measuring instrument. The results are shown in Table 1.
[0126] Table 1
[0127]
[0128] It can be seen from the above table that the biomineral crystal materials prepared in Examples 1-3 of the present invention have high infrared emissivity in the dual bands of 3 μm-5 μm and 8 μm-14 μm.
[0129] Test Example 2
[0130] The specific surface area and pore distribution of the products obtained in step S2 of Examples 1-5 and Comparative Examples 1-3 of the present invention and the product obtained in step S1 of Comparative Example 4 were measured using a TriStarⅡ 3020 specific surface area and porosity analyzer. The results are shown in Table 2.
[0131] Table 2
[0132]
[0133] It can be seen from the above table that the product obtained in step S2 of Examples 1-3 of the present invention has a larger specific surface area and pore volume.
[0134] Test Example 3
[0135] 130 SPF grade Kunming mice were randomly divided into a blank group, examples 1-5 and comparative examples 1-7, with 10 mice in each group. During the feeding period, the mice were free to eat and drink water, the temperature was 25±2°C, and the humidity was 50±10%. After one week of adaptive feeding, the biomineral crystal materials obtained in examples 1-5 and comparative examples 1-7 were mixed with cotton in a mass ratio of 2:8 and filled into a non-woven bag to prepare a pillow. The blank group used all-cotton to fill a non-woven bag to obtain a pillow. The prepared sleep-aiding pillow or pillow was spread on the top cover of the mouse cage, and the top cover was kept tight during the test. On the 15th day of the test, the mice were placed in batches in the mouse autonomous activity instrument, adapted for 5 minutes, and then the number of autonomous activities of the mice within 5 minutes was recorded. The number of autonomous activities of the animal groups in the test group and the control group was compared, and the results are shown in Table 3.
[0136] Table 3
[0137]
[0138] Note: *Compared with the blank group, P < 0.05.
[0139] It can be seen from the above table that the pillows filled with the biomineral crystal materials prepared in Examples 1-3 of the present invention can significantly reduce the number of mouse activities and promote the sleep of mice.
[0140] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a biomineral crystal material, It is characterized in that The following steps are involved: S1. Surface modification of natural mineral crystals: ball-milling the natural mineral crystals, adding them to ethanol, adding a silane coupling agent, heating and stirring to react, filtering, washing, and drying to obtain surface-modified natural mineral crystal powder; the mass ratio of the natural mineral crystals to the silane coupling agent is 50:4-7, the silane coupling agent is a mixture of KH550 and KH580, and the mass ratio is 7-10:3-5; the natural mineral crystals are mixed ore containing natural mineral crystals and rare earth concentrates, and the mass ratio is 10:5; S2. Doped TiO 2 / Fe 3 O 4 Preparation of intercalated montmorillonite modified crystal powder: adding butyl titanate to ethanol to form solution A, dissolving melamine, ferric chloride and ferrous chloride in water to obtain solution B, dropping solution B into solution A, stirring evenly to obtain a pillaring agent, dropping into the montmorillonite suspension, and simultaneously dropping ammonia water, adding the surface modified natural mineral crystal powder obtained in step S1, heating and stirring to react, standing for aging, microwave heating and drying, washing, ball milling, calcining, and obtaining doped TiO 2 / Fe 3 O 4 Intercalated montmorillonite modified crystal powder; S3. Preparation of modified crystal powder: doped TiO 2 / Fe 3 O 4 Adding intercalated montmorillonite modified crystal powder into water, adding dopamine hydrochloride and a catalyst, heating and stirring to react, filtering, washing, and drying to obtain modified crystal powder; S4 essential oil adsorption: the modified crystal powder obtained in step S3 is added to petroleum ether, the composite aromatic essential oil is added, the solvent is evaporated to obtain a modified crystal powder adsorbing essential oil; S5. Preparation of biomineral crystal material: Add the modified crystal powder adsorbing essential oil obtained in step S4 into water, add sodium alginate and an emulsifier to obtain an aqueous phase, drop the aqueous phase into fish oil, emulsify, drop calcium chloride solution, solidify at room temperature, filter, wash, and dry to obtain the biomineral crystal material.
2. The preparation method according to claim 1, It is characterized in that The ball milling time in step S1 is 0.5-1.5 hours, and the heating and stirring reaction temperature is 40-50° C. and the time is 1-3 hours.
3. The preparation method according to claim 1, It is characterized in that The mass ratio of butyl titanate, melamine, ferric chloride, ferrous chloride, montmorillonite and surface modified natural mineral crystal powder in step S2 is 5-7:0.5-1:3.4-3.5:1.2-1.3:30-50:100, the temperature of the heating and stirring reaction is 65-75°C, the time is 2-4h, the ball milling time is 1-2h, the calcination temperature is 450-550°C, and the time is 1-3h.
4. The preparation method according to claim 1, It is characterized in that The doped TiO 2 / Fe 3 O 4 The mass ratio of intercalated montmorillonite modified crystal powder, dopamine hydrochloride and catalyst is 20-30:14-18:1-2, the temperature of the heating and stirring reaction is 40-50°C, the time is 2-3h, and the catalyst is Tris-HCl solution with pH=8.5-9.
5. The preparation method according to claim 1, It is characterized in that The mass ratio of the modified crystal powder and the composite aromatic essential oil in step S4 is 100:15-22, the composite aromatic essential oil is selected from at least two of rose essential oil, clove essential oil, lavender essential oil, and wormwood essential oil, and the preparation method of the essential oil is to obtain the essential oil by subjecting the raw materials to supercritical fluid extraction.
6. The preparation method according to claim 1, It is characterized in that The mass ratio of the modified crystal powder for adsorbing essential oil, sodium alginate and emulsifier in step S5 is 10-13:17-20:1-2, the emulsifier is selected from at least one of Tween-20, Tween-40, Tween-60, Tween-80 and Tween-85, and the room temperature curing time is 20-30min.
7. A biomineral crystal material obtained by the preparation method according to any one of claims 1 to 6.
8. Use of the biomineral crystal material as claimed in claim 7 in the preparation of sleep aid products.