Secondary batteries and electronic devices

By using a combination of lithium nickel cobalt manganese oxide compound and a specific electrolyte in secondary batteries, the problem of unstable performance of secondary batteries under high and low temperature conditions is solved, the capacity retention rate and lithium ion acceptance are significantly improved, and a better Efficient battery performance.

CN118412437BActive Publication Date: 2024-10-18NINGDE AMPEREX TECHNOLOGY LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410876578.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-18
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

The performance of existing secondary batteries is unstable under high and low temperature conditions, making it difficult to meet the market's demand for high efficiency and stability.

Method used

Lithium nickel cobalt manganate compound is used as the cathode material, combined with an electrolyte of specific proportions of ethylene carbonate, fluoroethylene carbonate, 1,3,6-hexanetrinitrile and lithium salicylate, combined with composite current collector and polymerization The material support layer enhances the capacity retention rate and lithium ion acceptance of secondary batteries under high and low temperatures.

Benefits of technology

Significantly improves the capacity retention rate and lithium ion acceptance of secondary batteries after high and low temperature shock tests, and enhances the stability and performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present application provides a secondary battery and an electronic device, wherein the secondary battery comprises a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the positive electrode sheet comprises a composite current collector and a positive electrode material layer disposed on at least one surface of the composite current collector, wherein the positive electrode material layer comprises a nickel cobalt manganese oxide lithium compound, wherein the molar percentage of the nickel element in the nickel cobalt manganese oxide lithium compound is X based on the total molar amount of metal elements other than lithium, and X>80%; the electrolyte comprises ethylene carbonate, fluoroethylene carbonate, 1,3,6-hexane trinitrile and lithium salicylate, wherein the mass percentage of ethylene carbonate is Y1 based on the mass of the electrolyte, the mass percentage of fluoroethylene carbonate is Y2, and 1≤Y1 / Y2≤35; and the mass percentage of 1,3,6-hexane trinitrile is Y3 based on the mass of the electrolyte, and 0.1%≤Y3≤4%, and 1≤Y2 / Y3≤60. The present application can improve the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical energy storage, and in particular to a secondary battery and an electronic device using the secondary battery. Background Art

[0002] Secondary batteries have developed rapidly in the fields of new energy vehicles and large-scale energy storage. With the diversification of the application fields, usage regions and usage scenarios of terminal products, the market has higher and higher performance requirements for secondary batteries. How to provide a secondary battery with more stable and efficient performance under high and low temperature conversion conditions has become an urgent problem that needs to be solved. Summary of the invention

[0003] The present application provides a secondary battery and an electronic device.

[0004] In a first aspect, the present application provides a secondary battery, comprising a positive electrode plate, a negative electrode plate and an electrolyte, wherein the positive electrode plate comprises a composite current collector and a positive electrode material layer disposed on at least one surface of the composite current collector, wherein the positive electrode material layer comprises a nickel cobalt manganese oxide compound, wherein the molar percentage of nickel element in the nickel cobalt manganese oxide compound is X based on the total molar amount of metal elements other than lithium, and X>80%; the electrolyte comprises ethylene carbonate, fluoroethylene carbonate, 1,3,6-hexane trinitrile and lithium salicylate, wherein the mass percentage of ethylene carbonate is Y1, the mass percentage of fluoroethylene carbonate is Y2, and 1≤Y1 / Y2≤35 based on the mass of the electrolyte; and the mass percentage of 1,3,6-hexane trinitrile is Y3, wherein 0.1%≤Y3≤4%, and 1≤Y2 / Y3≤60 based on the mass of the electrolyte.

[0005] In this application, the composite current collector and the high-nickel ternary positive electrode material work together, and cooperate with the ethylene carbonate and fluoroethylene carbonate in a specific ratio in the electrolyte, which can improve the capacity retention rate and lithium ion acceptance of the secondary battery after the high and low temperature impact test. 1,3,6-hexane trinitrile and lithium salicylate are added to the electrolyte to strengthen the synergistic effect of the composite current collector and the high-nickel ternary positive electrode material and the specific ratio of ethylene carbonate and fluoroethylene carbonate, further improving the capacity retention rate and lithium ion acceptance of the secondary battery after the high and low temperature impact test.

[0006] Based on the first aspect, in some possible implementations, 5%≤Y1≤40%, which can further improve the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests.

[0007] Based on the first aspect, in some possible implementations, 10%≤Y1≤20%, which can further improve the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests.

[0008] Based on the first aspect, in some possible implementations, 0.3%≤Y2≤7%, which can further improve the capacity retention and lithium ion acceptance of the secondary battery after high and low temperature impact tests.

[0009] Based on the first aspect, in some possible embodiments, the composite current collector includes a polymer support layer and a metal conductive layer disposed on at least one surface of the polymer support layer. Meeting the above conditions can further improve the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests.

[0010] Based on the first aspect, in some possible implementations, the polymer support layer includes polyethylene terephthalate and / or polypropylene. Meeting the above conditions can further improve the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests.

[0011] Based on the first aspect, in some possible implementations, the thickness of the polymer support layer is T, 3 μm≤T≤12 μm. Meeting the above conditions can further improve the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests.

[0012] Based on the first aspect, in some possible implementations, the electrolyte further comprises butylene sulfite. Meeting the above conditions can further improve the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests.

[0013] Based on the first aspect, in some possible embodiments, the negative electrode plate includes a negative electrode material layer, the negative electrode material layer includes graphite and silicon material, and the graphite includes artificial graphite and / or natural graphite. The negative electrode is applied to the battery of the present application, and can better cooperate with the positive electrode and the electrolyte to improve the performance of the secondary battery.

[0014] A second aspect of the present application provides an electronic device including a secondary battery. DETAILED DESCRIPTION

[0015] The technical scheme in the embodiment of the present application is described clearly and in detail below. Obviously, the described embodiment is a part of the embodiment of the present application, rather than all the embodiments. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present application. The terms used in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application.

[0016] An embodiment of the present application provides a secondary battery, which includes a housing, an electrode assembly and an electrolyte. The electrode assembly and the electrolyte are both located in the housing.

[0017] The outer shell may be a packaging bag encapsulated by an encapsulation film (such as an aluminum-plastic film), such as a soft-pack battery. In other embodiments, the secondary battery may also be a steel-shell battery, an aluminum-shell battery, or the like.

[0018] The electrode assembly includes a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet. The electrode assembly may be a laminated structure, which is formed by alternating the positive electrode sheet, the separator and the negative electrode sheet. In other embodiments, the electrode assembly may also be a wound structure, which is formed by stacking the positive electrode sheet, the separator and the negative electrode sheet and then winding them.

[0019] The positive electrode plate includes a composite current collector and a positive electrode material layer disposed on at least one surface of the composite current collector, the positive electrode material layer includes a nickel cobalt manganese oxide compound, and the molar percentage of nickel element in the nickel cobalt manganese oxide compound is X based on the total molar amount of metal elements other than lithium, and X>80%;

[0020] The electrolyte includes ethylene carbonate (EC), fluoroethylene carbonate (FEC), 1,3,6-hexanetricarbonitrile and lithium salicylate. Based on the mass of the electrolyte, the mass percentage of ethylene carbonate is Y1, the mass percentage of fluoroethylene carbonate is Y2, and 1≤Y1 / Y2≤35; based on the mass of the electrolyte, the mass percentage of 1,3,6-hexanetricarbonitrile is Y3, 0.1%≤Y3≤4%, and 1≤Y2 / Y3≤60.

[0021] The positive electrode and electrolyte in the secondary battery provided in the present application can work synergistically to improve the stability of the secondary battery, thereby improving the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests. It is speculated that the positive electrode system and electrolyte system in the present application can improve the bonding force between the composite current collector and the high-nickel ternary positive electrode material, and enhance the anti-temperature difference effect of the ethylene carbonate and fluoroethylene carbonate in the electrolyte of the present application on the high-nickel ternary positive electrode interface film formation under the support of the composite current collector. The above synergistic effect enables the secondary battery to withstand the impact of high and low temperature conversion. The added 1,3,6-hexane trinitrile and lithium salicylate can further enhance the synergistic effect between the positive electrode including the composite current collector and the high-nickel ternary and the electrolyte including ethylene carbonate and fluoroethylene carbonate, and further improve the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests.

[0022] The nickel cobalt manganese oxide compound includes nickel cobalt manganese oxide and nickel cobalt manganese oxide derivatives, such as coating materials or derivatives doped with other metal elements. For example, the nickel cobalt manganese oxide compound can be LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.88 Co 0.1 Mn0.02 O2. Nickel cobalt manganese oxide derivatives can be Li 0.8 Ni 0.8982 Co 0.0589 Mn 0.0409 Zr 0.002 O2.

[0023] In some optional embodiments, X can be 82%, 85%, 87%, 90%, 92%, 95%, or any value within the range formed by any two of the above values. The value of Y1 / Y2 can be 1, 2, 5, 7, 9, 12, 15, 17, 19, 22, 25, 30, 35, or any value within the range formed by any two of the above values.

[0024] In some embodiments, 5%≤Y1≤40%, which can further improve the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests.

[0025] In some optional embodiments, Y1 can be 5%, 7%, 10%, 15%, 20%, 22%, 25%, 30%, 32%, 35%, 37%, 40% or any value within the range formed by any two of the above values.

[0026] In some embodiments, 10%≤Y1≤20%, which is more conducive to improving the capacity retention and lithium ion acceptance of the secondary battery after high and low temperature impact tests.

[0027] In some embodiments, 0.3%≤Y2≤7%, which can further improve the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests.

[0028] In some optional embodiments, Y2 can be 0.3%, 0.5%, 1%, 3%, 4%, 5%, 7% or any value within the range formed by any two of the above values.

[0029] In some optional embodiments, Y3 can be 0.1%, 0.2%, 0.5%, 0.7%, 1%, 1.2%, 1.5%, 2%, 2.2%, 2.5%, 3%, 3.2%, 3.5%, 4%, or any value within the range formed by any two of the above values. The ratio of Y2 / Y3 can be 1, 1.5, 1.7, 2, 2.5, 3, 4, 5, 5.5, 6, 10, 20, 30, 40, 50, 60, or any value within the range formed by any two of the above values.

[0030] In some embodiments, the electrolyte further includes butylene sulfite. It is beneficial to further improve the capacity retention rate and lithium ion acceptance of the secondary battery after the high and low temperature impact test. Based on the mass of the electrolyte, the mass percentage of butylene sulfite is 0.1% to 0.5%, which is beneficial to improve the capacity retention rate and lithium ion acceptance of the secondary battery after the high and low temperature impact test. In some embodiments, the mass percentage of butylene sulfite can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5% or any value within the range composed of any two of the above values.

[0031] In some embodiments, the addition of lithium salicylate to the electrolyte is beneficial to further improve the capacity retention rate and lithium ion acceptance of the secondary battery after the high and low temperature impact test. Based on the mass of the electrolyte, the mass percentage of lithium salicylate is 0.2% to 0.5%, which is beneficial to improve the capacity retention rate and lithium ion acceptance of the secondary battery after the high and low temperature impact test. In some embodiments, the mass percentage of lithium salicylate can be 0.2%, 0.25%, 0.3%, 0.4%, 0.45%, 0.5% or any value within the range of any two of the above values.

[0032] Electrolyte

[0033] According to some embodiments of the present application, the electrolyte includes the above-described ethylene carbonate, fluoroethylene carbonate, 1,3,6-hexanetrinitrile, butylene sulfite and lithium salicylate.

[0034] In some embodiments, the electrolyte further includes an organic solvent, and the organic solvent includes, but is not limited to, propylene carbonate (PC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate, or ethyl propionate.

[0035] In some embodiments, the organic solvent further comprises an ether solvent, and in some optional embodiments comprises at least one of 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME).

[0036] In some embodiments, the electrolyte may further include a lithium salt, the lithium salt including at least one of an organic lithium salt or an inorganic lithium salt. In some embodiments, the lithium salt includes, but is not limited to: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium trifluoromethanesulfonyl imide LiN(CF3SO2)2 (LiTFSI), lithium bis(fluorosulfonyl)imide Li(N(SO2F)2) (LiFSI), lithium bis(oxalatoborate) LiB(C2O4)2 (LiBOB) or lithium di(oxalatoborate) LiBF2(C2O4) (LiDFOB). In some embodiments, the additive includes at least one of adiponitrile.

[0037] Positive electrode

[0038] In some embodiments, the composite current collector includes a polymer support layer and a metal conductive layer disposed on at least one surface of the polymer support layer. The polymer support layer has good structural strength, which can improve the structural strength of the composite current collector, thereby further improving the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests.

[0039] In some embodiments, the polymer support layer includes polyethylene terephthalate and / or polypropylene. The above polymer materials as the polymer support layer have good thermal stability and mechanical properties.

[0040] The metal conductive layer may include at least one of aluminum or an aluminum alloy.

[0041] In some embodiments, the thickness of the polymer support layer is T, 3μm≤T≤12μm. Within the above range, it is beneficial to make the polymer support layer have good structural strength, support the metal conductive layer, improve the structural stability of the composite current collector, and further improve the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests. In some optional embodiments, T can be 3μm, 5μm, 7μm, 10μm, 12μm or any value within the range of any two of the above values.

[0042] The positive electrode material layer also includes a binder to bond the positive electrode active material particles to facilitate the formation of a film layer, and at the same time, it can also improve the bonding force between the positive electrode material layer and the positive electrode current collector. In some embodiments, the binder may include but is not limited to polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylic (ester) styrene butadiene rubber, epoxy resin or nylon, etc. At least one of the above.

[0043] The cathode material layer may also include a conductive material, including but not limited to carbon-based materials, metal-based materials, conductive polymers, or any combination thereof. In some embodiments, carbon-based materials may include but are not limited to natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, metal-based materials may include but are not limited to metal powder or metal fiber, in some optional embodiments copper, nickel, aluminum or silver. In some embodiments, the conductive polymer may be a polyphenylene derivative.

[0044] Negative electrode

[0045] In some embodiments, the negative electrode material layer includes graphite and a silicon material. The graphite includes artificial graphite and / or natural graphite.

[0046] The silicon material includes at least one of (a composite of a silicon-based substance and a carbon-based substance) or a silicon oxide (SiOx, 0 < x ≤ 2). The silicon-based substance can be silicon particles, silicon alloy particles, etc.

[0047] Since graphite has a certain flexibility, its combination with the silicon-carbon composite material can alleviate the overall volume expansion of the negative electrode material layer. At the same time, both graphite and the silicon-carbon composite material as the negative electrode active material can make full use of the advantages of both the silicon-carbon composite material and graphite to achieve better electrochemical performance.

[0048] In this application, the mass ratio of graphite in the negative electrode material layer is 35 wt.% to 95 wt.%. When the mass ratio of graphite in the negative electrode material layer is within the above range, the cycle performance of the negative electrode material layer can be further improved, thereby improving the cycle performance of the secondary battery.

[0049] The negative electrode current collector can be at least one of copper foil, nickel foil, stainless steel foil, titanium foil, or a carbon-based current collector, etc., and can also be a composite current collector disclosed in any prior art, and in some alternative embodiments, but not limited to, the current collector formed by combining the foregoing conductive foil and a polymer substrate.

[0050] The negative electrode material layer further contains a binder for binding the negative electrode active material particles to facilitate the formation of a film layer, and at the same time can also improve the bonding force between the negative electrode material layer and the negative electrode current collector. In some embodiments, the binder can include but is not limited to polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, a polymer containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene 1,1-difluoroethylene, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, or nylon, etc.

[0051] The negative electrode material layer may further include a conductive material, and the conductive material includes but is not limited to a carbon-based material, a metal-based material, a conductive polymer, or any combination thereof. In some embodiments, the carbon-based material can include but is not limited to natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, the metal-based material can include but is not limited to metal powder or metal fiber, and in some alternative embodiments, copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer can be a polyphenylene derivative.

[0052] The negative electrode material layer may further include a dispersant, the dispersant including at least one of sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, carboxymethyl cellulose, lithium hydroxypropyl carboxymethyl cellulose, sodium hydroxypropyl carboxymethyl cellulose, hydroxypropyl carboxymethyl cellulose, lithium hydroxyethyl carboxymethyl cellulose, sodium hydroxyethyl carboxymethyl cellulose or hydroxyethyl carboxymethyl cellulose.

[0053] Isolation film

[0054] The material and shape of the separator used in the secondary battery of the present application are not particularly limited, and can be any technology disclosed in the prior art. In some embodiments, the separator includes a polymer or inorganic substance formed of a material that is stable to the electrolyte of the present application.

[0055] In some optional embodiments, the isolation film may include a substrate layer and a surface treatment layer. The substrate layer is a non-woven fabric, a film or a composite film having a porous structure, and the material of the substrate layer is selected from at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Specifically, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film can be selected.

[0056] A surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. The inorganic layer includes inorganic particles and a binder, and the inorganic particles are selected from at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The binder is selected from at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyethylene alkoxy, polymethyl methacrylate, polytetrafluoroethylene and polyhexafluoropropylene. The polymer layer contains a polymer, and the material of the polymer is selected from at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyethylene alkoxy, polyvinylidene fluoride and poly (vinylidene fluoride-hexafluoropropylene).

[0057] The secondary battery is applied to electronic devices to power the loads in the electronic devices, which may include but are not limited to laptop computers, pen-input computers, mobile computers, electronic book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD televisions, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries, and lithium-ion capacitors.

[0058] The present application is described below by specific examples and comparative examples. Those skilled in the art should understand that the preparation methods described in the present application are only examples, and any other suitable preparation methods are within the scope of the present application.

[0059] Example 1

[0060] 1. Preparation of positive electrode

[0061] LiNi 0.88 Co 0.1 Mn 0.02 O2, Super-P and polyvinylidene fluoride were mixed with N-methylpyrrolidone (NMP) in a mass ratio of 96:2:2 and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry was coated on a 12 μm composite aluminum foil (commercially available, a composite current collector made of polyethylene terephthalate (PET) as a base material and deposited with a metal aluminum layer on both sides of the foil using an advanced vacuum coating process), dried, cold pressed, and then cut and welded to obtain a positive electrode sheet.

[0062] 2. Preparation of negative electrode

[0063] Artificial graphite and SiO2 (mass ratio 90:10), styrene-butadiene rubber, sodium hydroxyethyl carboxymethyl cellulose are mixed with deionized water in a mass ratio of 96.5%:1.5%:2%, and then triazine compound is added and stirred evenly to obtain slurry. The slurry is coated on a 9μm copper foil. Drying, cold pressing, cutting and welding of the tabs are performed to obtain the negative electrode.

[0064] 3. Preparation of Electrolyte

[0065] In a dry argon environment, propylene carbonate (PC), diethyl carbonate (DMC) and ethyl propionate (EP) (weight ratio 2:2:3) were mixed, and LiPF6 was added, wherein the concentration of LiPF6 was 12.5%, to obtain a basic electrolyte. Ethylene carbonate (EC) and fluoroethylene carbonate (FEC) and other optional substances were added to the basic electrolyte according to the contents shown in Table 1 to obtain electrolytes of different embodiments and comparative examples.

[0066] 4. Preparation of isolation membrane

[0067] A 7-micron polyethylene porous polymer film was used as the separator.

[0068] 5. Preparation of secondary batteries

[0069] The obtained positive electrode, separator and negative electrode are wound in order and placed in an outer packaging foil, leaving a liquid injection port. The electrolyte is poured from the liquid injection port, packaged, and then subjected to formation, capacity and other processes to obtain a secondary battery.

[0070] Example 2 to Example 21

[0071] The difference between Example 2 to Example 21 and Example 1 is that, except for adjusting the electrolyte related parameters according to Table 1, the rest are the same as Example 1.

[0072] Example 22 to Example 27

[0073] The difference between Example 22 to Example 27 and Example 15 is that, except for adjusting the relevant parameters of the composite current collector according to Table 1, the rest are the same as Example 1.

[0074] Comparative Examples 1 to 5

[0075] Comparative Example 1 is the same as Example 1 except that a conventional positive electrode current collector with a thickness of 10 μm is used. Comparative Examples 2 to 5 are the same as Example 1 except that the preparation parameters of the electrolyte are adjusted according to Table 1.

[0076] Test Method

[0077] 1. Capacity retention rate after high and low temperature impact test

[0078] Take 3 lithium-ion batteries from each group, charge and discharge the 3 lithium-ion batteries respectively through the following steps, and calculate the discharge capacity retention rate of the secondary batteries.

[0079] First, in an environment of 25°C, the first charge and discharge were performed. First, a constant current charge was performed at 0.5C, and constant voltage charge was performed after charging to 4.3V. Then, a constant current discharge was performed at a current of 1C, and the discharge was performed to 2.8V. The discharge capacity of the first cycle was recorded. Then, the lithium-ion battery was placed in an environment of -20°C for 100 charge and discharge cycles. After the low-temperature cycle was completed, the lithium-ion battery was transferred to an environment of 45°C within one hour for 200 charge and discharge cycles, and the discharge capacity of the 200th cycle at 45°C was recorded.

[0080] Capacity retention rate=(discharge capacity at the 200th cycle / discharge capacity at the first cycle)×100%.

[0081] Evaluation was performed according to the following criteria: A higher capacity retention rate indicates that the performance of the secondary battery after the high and low temperature impact test is better.

[0082] A: Capacity retention rate is greater than 85%;

[0083] B: Capacity retention rate is greater than or equal to 80% and less than 85%;

[0084] C: Capacity retention rate is greater than or equal to 75% and less than 80%;

[0085] D: Capacity retention rate is less than 75%.

[0086] 2. Lithium ion acceptance after high and low temperature impact test

[0087] After the secondary battery was allowed to stand at 35°C for 24 hours, it was charged at a constant current of 1.0C for 1 hour at 35°C to measure the high-temperature charge capacity (C0). Then, at 35°C, the discharge was stopped at a constant current of 0.1C until it reached 3V. Next, at -15°C, the battery was charged at a constant current of 1.0C for 1 hour to measure the low-temperature charge capacity (C1). Then, the ratio of C1 to C0 (C1 / C0) was calculated and evaluated using the following benchmarks. The larger the value of C1 / C0, the better the lithium ion acceptance of the secondary battery at low temperatures.

[0088] A: C1 / C0 is 0.65 or more;

[0089] B: C1 / C0 is greater than 0.55 and less than 0.65;

[0090] C: C1 / C0 is greater than 0.5 and less than 0.55;

[0091] D: C1 / C0 is less than 0.5.

[0092] Table 1

[0093]

[0094]

[0095] In the above table, “ / ” means no relevant parameter.

[0096] Compared with the comparative example, in the embodiment, when the composite current collector and the high-nickel ternary positive electrode material work together and cooperate with the ethylene carbonate and fluoroethylene carbonate present in a specific proportion in the electrolyte, the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests can be improved.

[0097] In particular, when a certain content of 1,3,6-hexanetricarbonitrile exists in the electrolyte, the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests can be further improved.

[0098] In particular, when butylene sulfite and / or lithium salicylate exist in the electrolyte, the capacity retention rate and lithium ion acceptance of the secondary battery after the high and low temperature impact test can be further improved.

[0099] In particular, when the polymer support layer of the composite current collector meets the range defined in the present application, the capacity retention rate and lithium ion acceptance of the secondary battery after high and low temperature impact tests can be further improved.

[0100] Although illustrative embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the principles and scope of the present application.

Claims

1. A secondary battery, It is characterized in that The invention comprises a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the positive electrode sheet comprises a composite current collector and a positive electrode material layer disposed on at least one surface of the composite current collector, wherein the positive electrode material layer comprises a nickel cobalt manganese oxide compound, and based on the total molar amount of metal elements other than lithium, the molar percentage of nickel element in the nickel cobalt manganese oxide compound is X, and X>80%; The electrolyte comprises ethylene carbonate, fluoroethylene carbonate, 1,3,6-hexane trinitrile, butylene sulfite and lithium salicylate. Based on the mass of the electrolyte, the mass percentage of the ethylene carbonate is Y1, the mass percentage of the fluoroethylene carbonate is Y2, 1≤Y1 / Y2≤35, 5%≤Y1≤40%, 0.3%≤Y2≤7%; based on the mass of the electrolyte, the mass percentage of the 1,3,6-hexane trinitrile is Y3, 0.1%≤Y3≤4%, 1≤Y2 / Y3≤60; The electrolyte also includes a basic electrolyte, and the basic electrolyte includes LiPF 6 , propylene carbonate, diethyl carbonate and ethyl propionate, the weight ratio of the propylene carbonate, the diethyl carbonate and the ethyl propionate is 2:2:3, in the basic electrolyte, the LiPF 6 The mass concentration is 12.5%.

2. The secondary battery according to claim 1, It is characterized in that The composite current collector includes a polymer support layer and a metal conductive layer disposed on at least one surface of the polymer support layer.

3. The secondary battery according to claim 2, It is characterized in that The polymer support layer includes polyethylene terephthalate and / or polypropylene.

4. The secondary battery according to claim 2 or 3, It is characterized in that The thickness of the polymer support layer is T, 3 μm≤T≤12 μm.

5. The secondary battery according to any one of claims 1 to 3, It is characterized in that The negative electrode plate includes a negative electrode material layer, the negative electrode material layer includes graphite and silicon material, and the graphite includes artificial graphite and / or natural graphite.

6. An electronic device, It is characterized in that The invention comprises the secondary battery according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Composite current collector, electrode plate and electrochemical device

    CN110943227A

  • Non-aqueous electrolyte solution for lithium secondary battery and lithium secondary battery comprising same

    CN114641884A

  • Water-based lithium ion battery and preparation method thereof

    CN115882074A