Additive composition, electrolyte and battery
By using additive compositions with specific structures in the electrolyte to form CEI films and SEI films with strong lithium conductivity, the problem of poor performance of the battery at room temperature and high temperature is solved, and the circulation and safety performance of the battery is significantly improved.
Patent Information
- Application Number
- CN202410961803.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-18
AI Technical Summary
During the operation of the battery, existing electrolyte additives are prone to problems such as large impedance, poor circulation performance at room temperature and high temperature, poor rate performance and low safety performance.
Using an additive composition, including a first additive with a specific structure and a trimethylolpropane phosphite as the second additive, the formation of a CEI film and SEI film with strong lithium conductivity and uniform density in the electrolyte solution, improves the Battery room temperature and high temperature cycle performance, rate performance and safety performance.
It significantly improves the battery's normal temperature and high temperature cycle performance, rate performance and safety performance, reduces the battery's impedance and gas production, and extends the battery's service life.
Smart Images

Figure SMS_17 
Figure SMS_18 
Figure SMS_19
Abstract
Description
Technical Field
[0001] The invention relates to an additive composition, in particular to an additive composition, an electrolyte and a battery, belonging to the technical field of secondary batteries. Background Art
[0002] With the rapid development of pure electric vehicles, smart homes, power tools, smart transportation and other markets, consumers' requirements for battery performance are constantly increasing. Secondary batteries are widely used in consumer electronics and energy storage and power batteries due to their advantages such as high specific energy, long cycle life and low self-discharge.
[0003] At present, electrolyte additives are often added to the electrolyte to improve the performance of the battery. However, the current electrolyte additives still have problems in the actual application process, such as making the battery prone to high impedance, poor cycle performance at room temperature and high temperature, gas generation and other problems during operation, thereby deteriorating the battery's cycle performance, rate performance and safety performance.
[0004] Therefore, it is urgent to develop an additive composition that can improve the room temperature and high temperature cycle performance, rate performance and safety performance of the battery. Summary of the invention
[0005] The invention provides an additive composition, which is applied to an electrolyte to improve the normal temperature and high temperature cycle performance, rate performance and safety performance of a battery.
[0006] The present invention provides an electrolyte, which can enable a battery to exhibit excellent room-temperature and high-temperature cycle performance, rate performance and safety performance.
[0007] The present invention provides a battery having excellent normal temperature and high temperature cycle performance, rate performance and safety performance.
[0008] The present invention provides an additive composition, wherein the additive composition comprises a first additive and a second additive; the first additive comprises a compound having a structural formula 1:
[0009] Formula 1,
[0010] wherein n is 0 or 1, A is selected from methylene or O, X is selected from sulfonyl or carbonyl, R1 and R2 are each independently selected from H, , , One of, and R1 and R2 are not selected from H at the same time, and X, R1 and R2 contain at least one sulfur atom;
[0011] The second additive includes trimethylolpropane phosphite.
[0012] The additive composition as described above, wherein the first additive comprises a compound having a structural formula 2:
[0013] Formula 2,
[0014] Among them, X, R1 and R2 contain 1 or 2 sulfur atoms.
[0015] The additive composition as described above, wherein the first additive comprises at least one of compounds having the structural formulae 3 to 6:
[0016] .
[0017] The additive composition as described above, wherein the mass ratio of the first additive to the second additive is (0.25-20):1.
[0018] The additive composition as described above, wherein the additive composition further comprises a third additive, and the third additive comprises vinyl sulfate.
[0019] The additive composition as described above, wherein the mass ratio of the first additive to the third additive is (0.25-20):1.
[0020] The present invention provides an electrolyte, wherein the electrolyte comprises the additive composition as described above.
[0021] The electrolyte as described above, wherein the mass percentage of the first additive in the electrolyte is 0.5-2%;
[0022] And / or, the mass percentage of the second additive in the electrolyte is 0.1%-1%;
[0023] And / or, the electrolyte includes a third additive, and the mass percentage of the third additive in the electrolyte is 0.1%-1%.
[0024] The electrolyte as described above, wherein the electrolyte further includes a negative electrode film-forming additive, and the negative electrode film-forming additive includes at least one of vinylene carbonate, fluoroethylene carbonate, and vinyl ethylene carbonate; the mass percentage of each of the negative electrode film-forming additives in the electrolyte is 0.5-1%.
[0025] The electrolyte as described above, wherein the electrolyte further comprises triphenyl phosphite; the mass percentage of the triphenyl phosphite in the electrolyte is 0.01-0.5%.
[0026] The electrolyte as described above, wherein the electrolyte further comprises an electrolyte salt and an organic solvent, the molar concentration of the electrolyte salt in the electrolyte is 0.8 mol / L - 2 mol / L; the electrolyte salt is a lithium salt or a sodium salt, and the lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, and lithium bis(trifluoromethanesulfonyl)imide; the sodium salt includes at least one of sodium hexafluorophosphate and sodium bis(fluorosulfonyl)imide).
[0027] And / or, the organic solvent includes at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, propyl propionate, and butyl propionate.
[0028] The present invention also provides a battery comprising the electrolyte as described above.
[0029] The battery as described above, wherein the battery comprises a positive electrode plate and a negative electrode plate, and the positive active material in the positive electrode plate is Li a Ni b Co c M1 d M2 e O f R g , where 1 ≤ a ≤ 1.2, 0.6 < b < 1, 0 < c < 1, 0 < d < 1, 0 ≤ e ≤ 0.2, b + c + d + e = 1, 1 ≤ f ≤ 2, 0 ≤ g ≤ 1, f + g = 2; M1 includes Mn and / or Al, M2 includes at least one of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb; R includes at least one of N, F, S, Cl;
[0030] Or, the positive active material in the positive electrode plate is at least one of three-dimensional tunnel type Na 0.44 MnO2, P2 layered type NaMO2, NaFePO4, Na4Fe3(PO4)2P2O7, Na3V2(PO4)3, Na3V2(PO4)2F3, Na2Fe(CN)6, Na2MnFe(CN)6; where M is at least one of Ni, Mn, Fe;
[0031] The negative active material in the negative electrode plate includes at least one of graphite, hard carbon, soft carbon, mesophase carbon microspheres, silicon-based negative electrode materials, and lithium-containing metal composite oxide materials.
[0032] The additive composition provided by the present invention limits the selection of the first additive and the second additive in the electrolyte. The first additive and the second additive work simultaneously, and can generate a CEI film and a SEI film with strong lithium conductivity and uniform and dense on the surface of the positive electrode and the negative electrode. The second additive can improve the ion transmission efficiency of the CEI film, and at the same time reduce the acidity of the electrolyte, thereby improving the room temperature and high temperature cycle performance, rate performance and safety performance of the battery.
[0033] The present invention provides an electrolyte comprising the additive composition, which can improve the normal temperature and high temperature cycle performance, rate performance and safety performance of the battery.
[0034] The battery of the present invention is prepared based on the electrolyte as described above, and the battery has excellent normal temperature and high temperature cycle performance, rate performance and safety performance at high temperature. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] The present invention provides an additive composition, comprising a first additive and a second additive; the first additive comprises a compound having a structural formula 1:
[0037] Formula 1,
[0038] wherein n is 0 or 1, A is selected from methylene or O, X is selected from sulfonyl or carbonyl, R1 and R2 are each independently selected from H, One of the following, and R1 and R2 are not selected from H at the same time, and at least one sulfur atom is contained in X, R1 and R2; the second additive includes trimethylolpropane phosphite.
[0039] In the compound of the present invention having the structure shown in Formula 1, n is 0 or 1, that is, the compound of Formula 1 can be a five-membered ring or a six-membered ring, and R2 in the structural formula of Formula 1 is specifically a substituent of a methylene or methine in the five-membered ring or the six-membered ring, that is, it can replace the hydrogen atom in the methylene or methine. For example, the compound of Formula 1 can be A of the present invention is methylene (the methylene may be substituted by R2) or O, and X is selected from sulfonyl or carbonyl. R1 and R2 of the present invention are each independently selected from H, , , One of Any methylene group in the five-membered ring can be converted into a methine group to become a substituent. For example, the compound of formula 1 can be Etc. In the present invention, R1 and R2 are not selected from H at the same time, that is, when R1 is H, R2 cannot be H, or when R2 is H, R1 cannot be H. In the present invention, X, R1 and R2 contain at least one sulfur atom.
[0040] The oxidation and reduction potentials of the first additive are both before those of the electrolyte solvent, so during the pre-charging process of the battery, it is oxidized at the positive electrode and reduced at the negative electrode before the solvent. Then a CEI film is formed at the positive electrode and a SEI film is formed at the negative electrode. It can reduce the gas production of the battery during the charging and discharging process, and as a low-impedance additive, it can reduce the battery impedance and improve the fast charging cycle performance. However, because the main component of the first additive in the positive electrode film formation is lithium carbonate, and the high content of lithium carbonate will be easily corroded by HF, causing the CEI film to become thicker, thereby causing the battery performance to decrease. Moreover, under high-temperature conditions of high-temperature cycling and high-temperature storage, electrolyte salts (such as lithium hexafluorophosphate) are easily hydrolyzed to generate hydrofluoric acid, thereby destroying the CEI and SEI solid electrolyte membranes, causing the electrolyte to decompose on the surface of the positive and negative electrodes, thereby reducing battery performance and increasing battery gas production. The second additive is trimethylolpropane phosphite. Compared with phosphate additives, its LUMO energy level is lower and more easily oxidized, and while participating in the positive electrode film formation, it will modify the positive electrode surface to make the positive electrode closer to the original positive electrode. On the other hand, the three-dimensional skeleton structure of the second additive can form a cavity channel during the film formation process, improve the porosity of the CEI film, and then improve the ion transmission efficiency and the performance of the battery cell. When the second additive is used in combination with the first additive, on the one hand, the phosphorus and sulfur-containing CEI film formed is more compact and has better performance. At the same time, the second additive can use its characteristics of electron-deficient compounds to preferentially react with water and hydrogen fluoride in the electrolyte, reduce the acidity of the electrolyte, and prevent HF from corroding the lithium carbonate component in the CEI film, thereby reducing the risk of increased impedance and reducing gas generation, thereby improving the room temperature and high temperature cycle performance, rate performance and safety performance of the battery.
[0041] In one embodiment, the first additive includes a compound having the structural formula 2:
[0042] Formula 2,
[0043] Among them, X, R1 and R2 contain 1 or 2 sulfur atoms.
[0044] When the first additive includes a compound having the structural formula 2, the first additive can further synergize with the second additive to improve the stability and lithium conductivity of the SEI film and the CEI film to a greater extent, thereby reducing the impedance of the battery, while avoiding the contact between the electrolyte and the positive and negative electrodes to a greater extent, inhibiting the gas production problem of the battery, and thereby making the battery's room temperature and high temperature cycle performance, rate performance and safety performance better.
[0045] In one embodiment, the first additive includes at least one of compounds having the structural formulae 3 to 6:
[0046] .
[0047] When the above-mentioned compound is selected as the first additive, the above-mentioned compound can better synergize with the second additive to generate SEI film and CEI film with higher lithium conductivity and better stability, thereby reducing the impedance of the battery and reducing the gas production problem of the battery, and can make the second additive perform better, thereby making the battery exhibit better room temperature and high temperature cycle performance, rate performance and safety performance.
[0048] In a specific embodiment, the mass ratio of the first additive to the second additive is (0.25-20):1, for example, the mass ratio of the first additive to the second additive is 0.25:1, 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1 or 20:1, etc. When the mass ratio of the first additive to the second additive is within the above range, the first additive and the second additive further act synergistically, so that the performance of the SEI membrane and the CEI membrane is better, and the porosity of the CEI membrane can be improved to a greater extent, the electrochemical impedance can be reduced, and the transmission rate of lithium ions can be accelerated. At the same time, the acidity of the electrolyte can be further reduced, and the positive electrode can be effectively inhibited from being corroded by HF and the electrolyte solvent can be prevented from decomposing, thereby reducing the generation of gas, thereby improving the normal temperature and high temperature cycle performance, rate performance and safety performance of the battery.
[0049] In a specific embodiment, the additive composition further includes a third additive, and the third additive includes vinyl sulfate. When vinyl sulfate is selected as the third additive, the third additive can be used in combination with the first additive and the second additive. The third additive will react with the electrolyte during the formation process to generate a substance similar to the first additive. At the same time, the third additive has a lower LUMO energy level than the first additive, so it will be reduced at the negative electrode before the first additive. The compound formed after the third additive is opened will promote the reduction of the first additive at the negative electrode, accelerate the film formation of the first additive, and reduce the content of lithium carbonate in the SEI film. At the same time, the lithium carbonate will be reduced by Li2SO4 and its perlithiation products (lithium oxide and amorphous Li x S and Li x O) is sandwiched in the middle, limiting the decomposition of HF in the electrolyte and the thickening of the SEI film, thereby avoiding the damage of the SEI film, making the constructed SEI film more conductive and denser, thereby improving the room temperature and high temperature cycle performance, rate performance and safety performance of the battery, and the third additive can work together with the first additive and the second additive to construct a denser and more uniform CEI film, thereby further improving the room temperature and high temperature cycle performance, rate performance and safety performance of the battery.
[0050] In a specific embodiment, the mass ratio of the first additive to the third additive is (0.25-20): 1, for example, the mass ratio of the first additive to the third additive is 0.25: 1, 0.5: 1, 1: 1, 2: 1, 3: 1, 4: 1, 5: 1, 6: 1, 7: 1, 8: 1, 9: 1, 10: 1, 11: 1, 12: 1, 13: 1, 14: 1, 15: 1, 16: 1, 17: 1, 18: 1, 19: 1 or 20: 1, etc. When the mass ratio of the first additive to the third additive is within the above range, the first additive, the second additive and the third additive further synergize, the stability and lithium conductivity of the SEI film and the CEI film are better, and the third additive can promote the film formation speed of the first additive on the negative electrode surface to a greater extent, and can further reduce the content of lithium carbonate in the SEI film, thereby further improving the stability of the SEI film, and thus making the battery present higher room temperature and high temperature cycle performance, rate performance and safety performance.
[0051] The present invention provides an electrolyte, which comprises the above-mentioned additive composition and can enable a battery to exhibit excellent normal temperature and high temperature cycle performance, rate performance and safety performance.
[0052] In a specific embodiment, the mass percentage of the first additive in the electrolyte is 0.5-2%, for example, the mass percentage of the first additive in the electrolyte is 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9% or 2%, etc. When the mass percentage of the first additive is within the above range, the first additive, the second additive and the third additive further synergize, and the lithium conductivity and stability of the SEI film and CEI film of the battery are higher, so that the impedance of the battery is lower, and the gas production problem of the battery can be reduced, thereby improving the normal temperature and high temperature cycle performance, rate performance and safety performance of the battery.
[0053] In a specific embodiment, the mass percentage of the second additive in the electrolyte is 0.1%-1%, for example, the mass percentage of the second additive in the electrolyte is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%, etc. When the mass percentage of the second additive is within the above range, the first additive, the second additive and the third additive further synergize to generate a SEI membrane and a CEI membrane with higher stability and lithium conductivity, and can further improve the porosity of the CEI membrane, improve the ion transmission efficiency of the CEI membrane, and further improve the room temperature and high temperature cycle performance and rate performance of the battery, and at the same time can reduce the acidity of the electrolyte to a greater extent, thereby suppressing the gas production problem of the battery to a greater extent and improving the safety performance of the battery.
[0054] In a specific embodiment, the electrolyte includes a third additive, and the mass percentage of the third additive in the electrolyte is 0.1%-1%, for example, the mass percentage of the third additive in the electrolyte is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%, etc. When the mass percentage of the third additive is within the above range, the first additive, the second additive and the third additive further synergize to make the stability and lithium conductivity of the SEI film and the CEI film better, and the third additive can further promote the film formation speed of the first additive, and at the same time, the stability of the SEI film is further improved, so that the normal temperature and high temperature cycle performance, rate performance and safety performance of the battery are better.
[0055] In a specific embodiment, the electrolyte further includes a negative electrode film-forming additive, and the negative electrode film-forming additive includes at least one of vinylene carbonate, fluoroethylene carbonate, and vinyl ethylene carbonate; the mass percentage of each negative electrode film-forming additive in the electrolyte is 0.5-1%, that is, the mass percentage of each additive in the negative electrode film-forming additive in the electrolyte is 0.5-1%, for example, the mass percentage of vinylene carbonate in the electrolyte is 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%, etc. When the above compounds are selected as negative electrode film-forming additives and their mass percentage is controlled within the above range, the addition of negative electrode film-forming additives can participate in the construction of SEI film, improve the uniformity of SEI film formation, thereby further protecting the negative electrode, and can reduce the gas production problem caused by the contact reaction between the electrolyte and the negative electrode, thereby further improving the normal temperature and high temperature cycle performance and safety performance of the battery.
[0056] In a specific embodiment, the electrolyte further comprises triphenyl phosphite, and its mass percentage in the electrolyte is 0.01-0.5%, for example, 0.01%, 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45% or 0.5%. When the mass percentage of triphenyl phosphite is within the above range, the storage stability of the electrolyte can be improved, which helps the electrolyte to maintain stable properties during storage and transportation, and reduce deterioration caused by changes in the external environment.
[0057] In a specific embodiment, the electrolyte further includes a lithium salt, and the lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate and lithium bis(trifluoromethanesulfonyl)imide; the molar concentration of the lithium salt in the electrolyte is 0.8mol / L-2mol / L, for example, the molar concentration of the lithium salt in the electrolyte is 0.8mol / L, 0.9mol / L, 1mol / L, 1.1mol / L, 1.2mol / L, 1.3mol / L, 1.4mol / L, 1.5mol / L, 1.6mol / L, 1.7mol / L, 1.8mol / L, 1.9mol / L or 2mol / L. When the lithium salt is selected from the above compounds and its molar concentration is controlled, the lithium salt can be fully dissolved in the solvent and release lithium ions, so that the lithium ions and the solvent form a solvation structure, which is conducive to the rapid migration of lithium ions. Preferably, the lithium salt can be lithium bis(fluorosulfonyl)imide. Lithium bis(fluorosulfonyl)imide helps reduce the generation of hydrogen fluoride in the electrolyte.
[0058] In a specific embodiment, the electrolyte further includes a sodium salt, and the sodium salt includes at least one of sodium hexafluorophosphate and sodium bis(fluorosulfonyl)imide. The molar concentration of the sodium salt in the electrolyte is 0.8mol / L-2mol / L, for example, the molar concentration of the sodium salt in the electrolyte is 0.8mol / L, 0.9mol / L, 1mol / L, 1.1mol / L, 1.2mol / L, 1.3mol / L, 1.4mol / L, 1.5mol / L, 1.6mol / L, 1.7mol / L, 1.8mol / L, 1.9mol / L or 2mol / L. When the sodium salt is selected from the above compounds and its molar concentration is controlled, the sodium salt can be fully dissolved in the solvent and release sodium ions, so that the sodium ions and the solvent form a solvation structure, which is conducive to the rapid migration of sodium ions.
[0059] In a specific embodiment, the electrolyte further includes an organic solvent, and the organic solvent includes at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, propyl propionate and butyl propionate. When the above organic solvent is selected, the above organic solvent is used as an important carrier for ion transmission, and the electrolyte salt, the first additive, the second additive, the third additive, the negative electrode film-forming additive and the stabilizing additive can be fully dissolved to obtain an electrolyte with high stability and high conductivity. At the same time, the viscosity of the electrolyte is appropriate, so that the electrolyte salt, the first additive, the second additive, the third additive and the negative electrode film-forming additive can better play their role, so that the battery exhibits higher normal temperature, high temperature cycle performance and safety performance.
[0060] The present invention also provides a battery comprising the electrolyte as described above. Based on the electrolyte provided by the present invention, the battery provided by the present invention exhibits excellent normal temperature and high temperature cycle performance and safety performance.
[0061] In a specific embodiment, the battery of the present invention includes a positive electrode plate, the positive electrode plate includes a positive electrode current collector and a positive electrode active material layer disposed on the surface of the positive electrode current collector, the positive electrode active material layer includes a positive electrode active material, a conductive agent and a binder, wherein the positive electrode current collector is generally an aluminum foil. As an example, when the battery is a lithium ion battery, the positive electrode active material is Li a Ni b Co c M1 d M2 e O f R g, where 1 ≤ a ≤ 1.2, 0.6 < b < 1, 0 < c < 1, 0 < d < 1, 0 ≤ e ≤ 0.2, b + c + d + e = 1, 1 ≤ f ≤ 2, 0 ≤ g ≤ 1, f + g = 2; M1 includes Mn and / or Al, M2 includes at least one of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, and R includes at least one of N, F, S, Cl. When the above positive electrode active material is selected, the gram capacity of the positive electrode active material can be improved, thereby reducing the cost of the positive electrode active material in the battery.
[0062] As another example, when the battery is a sodium-ion battery, the positive electrode active material includes, but is not limited to, three-dimensional tunnel-type Na 0.44 MnO2, P2-layered NaMO2, NaFePO4, Na4Fe3(PO4)2P2O7, Na3V2(PO4)3, Na3V2(PO4)2F3, Na2Fe(CN)6, Na2MnFe(CN)6; where M is at least one of Ni, Mn, Fe.
[0063] In a specific embodiment, in addition to the electrolyte and the positive electrode sheet provided by the present invention, a negative electrode sheet and a separator are further included. Specifically:
[0064] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer provided on the surface of the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, a conductive agent, and a binder. Among them, the negative electrode current collector is generally a copper foil, and the negative electrode active material is selected from one or more of graphite, hard carbon, soft carbon, mesophase carbon microspheres, silicon-based negative electrode materials, and lithium-containing metal composite oxide materials.
[0065] The selection of the conductive agent and the binder in the positive electrode active material layer and the negative electrode active material layer can be conventional materials in the art.
[0066] The separator is a separator well-known in the art that can be used in the battery and is stable for the electrolyte used, and can include one or more of polyolefin, aromatic polyamide, polytetrafluoroethylene, and polyethersulfone, and can be specifically set according to needs.
[0067] Hereinafter, the present invention will be further described in detail through specific examples.
[0068] Example 1
[0069] The electrolyte provided in this embodiment includes: the lithium salt includes lithium hexafluorophosphate, the molar concentration of lithium hexafluorophosphate is 1 mol / L, the organic solvent includes ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate, the mass ratio of ethylene carbonate and ethyl methyl carbonate is 3:5:2, the first additive is a compound with the structural formula 3, the mass percentage of the first additive is 0.5%, the second additive is trimethylolpropane phosphite, the mass percentage of the second additive is 0.5%, and the organic solvent is used to make up for less than 100%.
[0070] The preparation method of the electrolyte of this embodiment includes: preparing the electrolyte in a glove box, the glove box is filled with argon gas with a purity of 99.999%, the moisture in the glove box is controlled at ≤0.1ppm, the temperature is controlled at room temperature, ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate are fully mixed, lithium salt is mixed into the mixed solvent, after mixing evenly, a first additive and a second additive are added and fully mixed, and finally an electrolyte is obtained.
[0071] The electrolyte formulas provided in Examples 2-50 and Comparative Examples 1-3 are substantially the same as that in Example 1, and the specific parameters are shown in Table 1.
[0072] Table 1
[0073]
[0074]
[0075]
[0076]
[0077]
[0078]
[0079] Test example
[0080] The electrolytes of the embodiment and the comparative example are matched with the positive electrode sheet, the negative electrode sheet and the separator to prepare a lithium ion battery. Specifically, the positive electrode active material NCM811, the binder polyvinylidene fluoride (PVDF), the conductive agent carbon black and the conductive agent carbon nanotube are mixed uniformly according to the weight ratio of NCM:SP:CNT:PVDF=97.3:1:0.5:1.2, N-methylpyrrolidone (NMP) is added, and the mixture is stirred under the action of a vacuum stirrer until the mixed system becomes a positive electrode slurry with uniform fluidity; the positive electrode slurry is uniformly coated on the positive electrode current collector aluminum foil, and the coating amount is 35g / m 2After drying at 85°C, cold pressing is performed, trimming, cutting, and slitting are performed. After slitting, drying is performed at 85°C under vacuum conditions for 4 hours, and the tabs are welded to obtain the positive electrode sheet. The total thickness of the positive electrode sheet is 113μm, and the compaction density of the positive active material layer is 3.4mg / cm 3 .
[0081] The negative electrode active material graphite, the conductive agent carbon black, the thickener sodium carboxymethyl cellulose (CMC-Na), and the binder styrene-butadiene rubber were mixed in a weight ratio of 95:1.5:1:2.5, and deionized water was added to obtain the negative electrode slurry under the action of a vacuum mixer; the negative electrode slurry was evenly coated on the negative electrode current collector copper foil, and the coating amount was 20g / m 2 After drying at 85°C, cold pressing is performed, trimming, cutting, and slitting are performed, and after slitting, drying is performed at 85°C under vacuum conditions for 4 hours, and the tabs are welded to obtain the negative electrode sheet. The total thickness of the negative electrode sheet is 164μm, and the compaction density of the negative electrode active material layer is 1.5mg / cm 3 .
[0082] The prepared positive electrode sheet, negative electrode sheet and separator are stacked in order. The separator is a polyethylene separator with a thickness of 8μm. The separator is placed between the positive electrode sheet and the negative electrode sheet. After winding, the battery cell is placed in an aluminum plastic film package and dried to make a lithium-ion battery with a thickness of 4.7mm, a width of 55mm, and a length of 60mm. It is vacuum-baked at 75°C for 10 hours and the above-prepared electrolyte is injected. After standing for 24 hours, the battery is placed in an environment of 45°C, a pressure of 3kg is applied, and it is charged to 4.0V at 0.1C (160mA), and then it is left to stand for 2 days (to fully activate the battery) to obtain a lithium-ion battery.
[0083] The following battery performance tests were performed on lithium batteries including the electrolytes of the embodiments and comparative examples, and the test methods were as follows:
[0084] At an ambient temperature of 25°C, the lithium-ion battery was left to stand for 4 hours, and then the lithium battery was subjected to 600 charge and discharge cycle tests at a current of 0.5C. The test voltage window was 2.75-4.25V, and the discharge capacity of the first cycle was recorded as C1, and the discharge capacity of the 600th cycle was recorded as C2. 600 , record the capacity retention rate η1=C after 600 cycles at 25℃ 600 / C1*100%, see Table 2.
[0085] At an ambient temperature of 45°C, the lithium-ion battery was left to stand for 4 hours, and then the lithium battery was subjected to 600 charge and discharge cycle tests at a current of 0.5C. The test voltage window was 2.75-4.25V, and the discharge capacity of the first cycle was recorded as C2, and the discharge capacity of the 600th cycle was recorded as C 600, record the capacity retention rate η2=C after 600 cycles at 45℃ 600 / C2*100%, see Table 2.
[0086] The thickness of the battery was weighed and recorded as m1. After standing for 24 hours, the battery was placed in a 45°C environment, a pressure of 3kg was applied, and it was charged to 4.0V at 0.1C (160mA). After standing for 2 days (to fully activate the battery), the thickness of the battery was weighed and recorded as m2. The gas production was recorded as ∆V=(m1-m2) / ρ, where ρ is the density of liquid water. See Table 2.
[0087] After the battery was stored at 60℃ for 30 days, it was discharged at 1C constant current to a cut-off voltage of 2.5V, left to stand for 5min, and then charged at 1C constant current and constant voltage to an upper limit voltage of 4.25V, with a cut-off current of 0.05C. It was then discharged at 1C constant current for 30min. The battery adjusted to 50% SOC was left to stand for 5min at 25℃, and then discharged at 2C constant current for 30s. The discharge current during 2C discharge is I 2C Record the initial voltage V0 and the voltage V1 after 30s of discharge. The discharge DC internal resistance calculation formula at 50% SOC is as follows: DCR (mΩ) = (V0-V1) / I 2C *100%.
[0088] The battery was placed in a 25°C environment, discharged at a constant current of 1C to a cut-off voltage of 2.5V, left to stand for 5 minutes, and charged at a constant current and voltage of 1.6C to an upper limit voltage of 4.25V, with a cut-off current of 0.05C. Then, it was charged and discharged at a constant current of 1.6C / 1C for 600 cycles, and the discharge capacity of the first cycle was recorded as C3, and the discharge capacity of the 600th cycle was recorded as C4, η3=C4 / C3*100%, as shown in Table 2.
[0089] Table 2
[0090]
[0091]
[0092] As can be seen from Table 2, the compound having the structural formula 1 and trimethylolpropane phosphite act synergistically, can participate in the construction of SEI film and CEI film, and generate CEI film and SEI film with strong lithium conductivity and uniform and dense, thereby improving the normal temperature and high temperature cycle performance, rate performance and safety performance of the battery. In addition, the addition of vinyl sulfate to the electrolyte can further synergize the compound having the structural formula 1, trimethylolpropane phosphite and vinyl sulfate, so that the lithium conductivity and stability of the CEI film and SEI film are higher, thereby making the normal temperature and high temperature cycle performance, rate performance and safety performance of the battery better. In addition, the addition of negative electrode film-forming additives and stability additives can further improve the lithium conductivity and stability of the SEI film, thereby further improving the normal temperature and high temperature cycle performance, rate performance and safety performance of the battery.
[0093] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An additive composition for battery electrolyte, characterized in that: The additive composition includes a first additive and a second additive; the first additive includes a compound having a structural formula 1: Formula 1, wherein n is 0 or 1, A is selected from methylene or O, X is selected from sulfonyl or carbonyl, R1 and R2 are each independently selected from H, , , One of, and R1 and R2 are not selected from H at the same time, and X, R1 and R2 contain at least one sulfur atom; The second additive includes trimethylolpropane phosphite.
2. The additive composition according to claim 1, characterized in that The first additive includes a compound having a structural formula 2: Formula 2, Among them, X, R1 and R2 contain 1 or 2 sulfur atoms.
3. The additive composition according to claim 2, characterized in that The first additive includes at least one of compounds having structural formulae 3 to 6: 、 、 、 。 4. The additive composition according to claim 3, characterized in that The mass ratio of the first additive to the second additive is (0.25-20):
1.
5. The additive composition according to claim 4, characterized in that The additive composition also includes a third additive including vinyl sulfate.
6. The additive composition according to claim 5, characterized in that The mass ratio of the first additive to the third additive is (0.25-20):
1.
7. An electrolyte, characterized in that: The electrolyte comprises the additive composition according to any one of claims 1 to 6.
8. The electrolyte according to claim 7, characterized in that The mass percentage of the first additive in the electrolyte is 0.5-2%; And / or, the mass percentage of the second additive in the electrolyte is 0.1%-1%; And / or, the electrolyte includes a third additive, and the mass percentage of the third additive in the electrolyte is 0.1%-1%.
9. The electrolyte according to claim 8, characterized in that The electrolyte also includes a negative electrode film-forming additive, which includes at least one of vinylene carbonate, fluoroethylene carbonate, and vinyl ethylene carbonate; the mass percentage of each of the negative electrode film-forming additives in the electrolyte is 0.5-1%.
10. The electrolyte according to claim 9, characterized in that The electrolyte also includes triphenyl phosphite; the mass percentage of the triphenyl phosphite in the electrolyte is 0.01-0.5%.
11. The electrolyte according to claim 10, characterized in that The electrolyte further comprises an electrolyte salt and an organic solvent, wherein the molar concentration of the electrolyte salt in the electrolyte is 0.8 mol / L-2 mol / L; the electrolyte salt comprises a lithium salt or a sodium salt, wherein the lithium salt comprises at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate and lithium bis(trifluoromethanesulfonyl)imide, and the sodium salt comprises at least one of sodium hexafluorophosphate and sodium bis(fluorosulfonyl)imide; And / or, the organic solvent includes at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, propyl propionate and butyl propionate.
12. A battery, characterized in that: The battery comprises the electrolyte according to any one of claims 7 to 11.
13. The battery according to claim 12, characterized in that The battery includes a positive electrode plate and a negative electrode plate, and the positive active material in the positive electrode plate is Li a Ni b Co c M1 d M2 e O f R g , where 1 ≤ a ≤ 1.2, 0.6 < b < 1, 0 < c < 1, 0 < d < 1, 0 ≤ e ≤ 0.2, b + c + d + e = 1, 1 ≤ f ≤ 2, 0 ≤ g ≤ 1, f + g = 2; M1 includes Mn and / or Al, M2 includes at least one of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, etc., and R includes at least one of N, F, S, Cl, etc.; Or, the positive electrode active material in the positive electrode plate is a three-dimensional tunnel-type Na 0.44 At least one of MnO2, P2 layered NaMO2, NaFePO4, Na4Fe3(PO4)2P2O7, Na3V2(PO4)3, Na3V2(PO4)2F3, Na2Fe(CN)6, Na2MnFe(CN)6; wherein M is at least one of Ni, Mn, and Fe; The negative electrode active material in the negative electrode plate includes at least one of graphite, hard carbon, soft carbon, mesophase carbon microspheres, silicon-based negative electrode materials and lithium-containing metal composite oxide materials.