Lithium ion battery separator and lithium ion battery

Through the combined technology of modified polypropylene, cellulose and lithium chloride, the problem of flammability and low wettability of lithium-ion battery separators has been solved, high-performance separator preparation has been achieved, and the flame retardant, conductive and mechanical properties of the battery have been improved. .

CN118507987BActive Publication Date: 2024-10-25江西巨电新能源科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410657103.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-25
Publication Date
2024-10-25
Estimated Expiration
2044-05-25

AI Technical Summary

Technical Problem

Existing lithium-ion battery separators have low wettability to electrolytes, poor absorption effects, and are flammable, which affects battery performance.

Method used

It uses a combination of modified polypropylene, modified cellulose and lithium chloride, and uses sodium periodate oxidation, DOPO reaction, sulfoxide chloride substitution reaction and dibenzoyl peroxide free radical grafting technology to form a flame retardant Porous membrane with high performance and high ion conductivity.

Benefits of technology

The flame retardant performance, ion conductivity performance, electrolyte wettability and mechanical properties of the lithium-ion battery separator are improved, and the overall performance of the battery is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 8TQT2GZTGUGACT4KMUIKK9NWSTSIYL03PONMEF9I
    Figure 8TQT2GZTGUGACT4KMUIKK9NWSTSIYL03PONMEF9I
  • Figure IGSKTAEVHW16HGTV9LEW2CBPJWBEZZBG4CBFWMJV
    Figure IGSKTAEVHW16HGTV9LEW2CBPJWBEZZBG4CBFWMJV
  • Figure JI3UUJ8TKF8GVWB51GOVSYFP3SEIUMDRTUYB7RAF
    Figure JI3UUJ8TKF8GVWB51GOVSYFP3SEIUMDRTUYB7RAF
Patent Text Reader

Abstract

The invention discloses a lithium ion battery separator and a lithium ion battery, and relates to the technical field of lithium batteries. When preparing the lithium ion battery separator, the present invention oxidizes cellulose with sodium periodate and then reacts with DOPO to obtain pre-modified cellulose; then reacts the pre-modified cellulose with thionyl chloride to obtain modified cellulose; reacts octamethylcyclotetrasiloxane, 3-dimethylaminopropyl (dimethoxy)methylsilane and vinyl pentamethyldisiloxane to obtain functionalized polysiloxane; reacts polypropylene with functionalized polysiloxane to obtain modified polypropylene; and mixes the modified polypropylene, modified cellulose and lithium chloride and then applies them on a glass plate to prepare the lithium ion battery separator. The lithium ion battery separator prepared by the present invention has excellent flame retardancy, ion conductivity, electrolyte wettability and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, in particular to a lithium ion battery separator and a lithium ion battery. Background Art

[0002] The diaphragm is known as the third "electrode material" in the battery. It is a microporous membrane processed and formed from a non-good electronic conductor material. When participating in the assembly of a lithium-ion battery, it is sandwiched between the positive and negative electrodes and is completely immersed in the electrolyte. The diaphragm can prevent negatively charged electrons from freely passing through the inside of the battery, but allows positively charged lithium ions to pass freely. As one of the three main components in a lithium-ion battery, the performance of the lithium battery diaphragm will directly affect the performance of the lithium-ion battery. To date, polyethylene and polypropylene are still the most important commercial diaphragms on the market, but they have low wettability to electrolytes, poor absorption effects, and are extremely flammable. Therefore, the present invention prepares a lithium-ion battery diaphragm with excellent flame retardant properties and electrolyte absorption. Summary of the invention

[0003] The object of the present invention is to provide a lithium ion battery separator and a lithium ion battery to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0005] A lithium ion battery separator is obtained by mixing modified polypropylene, modified cellulose and lithium chloride and then applying the mixture on a glass plate.

[0006] As an optimization, the modified polypropylene is obtained by reacting polypropylene and functionalized polysiloxane.

[0007] As an optimization, the polypropylene model is BH3520, which comes from Shanghai Chaoqi Plastic Chemical Co., Ltd.

[0008] As an optimization, the functionalized polysiloxane is obtained by reacting octamethylcyclotetrasiloxane, 3-dimethylaminopropyl (dimethoxy)methylsilane and vinylpentamethyldisiloxane.

[0009] As an optimization, the modified cellulose is obtained by oxidizing cellulose with sodium periodate and then reacting with DOPO and thionyl chloride in sequence.

[0010] As an optimization, the cellulose comes from Nanjing Tongying Biotechnology Co., Ltd.

[0011] As an optimization, a lithium-ion battery separator comprises the following preparation steps:

[0012] (1) Mix cellulose and deionized water in a mass ratio of 1:(49-51), add 30-40% hydrochloric acid solution to adjust the pH to 2-4, ultrasonically disperse for 10-20 min, add 1-3 times the molar amount of sodium periodate of cellulose, stir at 30-40 °C and 200-300 rpm for 2-4 h in a dark environment, cool naturally to room temperature, add 1-2 times the mass of cellulose of ethylene glycol, continue stirring for 1-3 h, filter, and rinse with deionized water and anhydrous ethanol. Wash alternately 3 to 5 times, dry at 65 to 75°C for 10 to 12 hours to obtain aldehyded cellulose; mix aldehyded cellulose, DOPO, deionized water and acetonitrile in a mass ratio of 1:(2 to 4):(0.7 to 0.9):(48 to 50), stir at 85 to 95°C and 100 to 200 rpm for 5 to 7 hours, cool naturally to room temperature and filter, wash with acetonitrile and tetrahydrofuran for 3 to 5 times respectively, and dry at 50 to 60°C for 11 to 13 hours to obtain pre-modified cellulose;

[0013] (2) Pre-modified cellulose and N,N-dimethylformamide were mixed in a mass ratio of 1:(18-20), stirred at 250-350 r / min and heated to 85-95°C, 3-4 times the mass of pre-modified cellulose of thionyl chloride was added at a uniform rate within 30-40 min, and stirring was continued for 2-3 h. Deionized water of 40-50 times the mass of pre-modified cellulose was added, and stirred at 400-500 r / min until the mass of precipitated solids remained unchanged, then filtered, washed with 2-4% ammonia water and deionized water for 3-5 times respectively, and dried at 50-70°C for 11-13 h to obtain modified cellulose;

[0014] (3) Octamethylcyclotetrasiloxane, 3-dimethylaminopropyl (dimethoxy)methylsilane and tetramethylammonium hydroxide silicon alkoxide are mixed in a mass ratio of 1:(1.1-1.3):(0.01-0.03), nitrogen is passed through for 10-20 min, and the mixture is stirred at 80-90°C and 100-200 rpm for 2-3 h. Vinylpentamethyldisiloxane (0.2-0.4 times the mass of octamethylcyclotetrasiloxane) is added, the mixture is heated to 95-105°C and stirred for 7-9 h. The mixture is heated to 130-140°C at a rate of 10-20°C / min and stirred for 40-50 min. The mixture is distilled at 0.1-0.3 MPa for 1-2 h to obtain a functionalized polysiloxane.

[0015] (4) Polypropylene, functionalized polysiloxane, dibenzoyl peroxide and deionized water are mixed in a mass ratio of 1:(0.2-0.3):(0.01-0.03):(8-10), stirred at 100-200 rpm for 55-65 min under a nitrogen atmosphere, heated to 85-95°C and continued to stir for 4-6 h, naturally cooled to room temperature and filtered, added with deionized water 199-201 times the mass of polypropylene, boiled for 25-35 min, naturally cooled to room temperature and filtered, repeated boiling and filtering 3-5 times, extracted with acetone in a Soxhlet extractor for 35-37 h, filtered, and dried at 60-70°C for 17-19 h to obtain modified polypropylene;

[0016] (5) Modified polypropylene, modified cellulose, lithium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:(0.2-0.4):(0.07-0.09):(6-8), and the mixture was ultrasonically treated at 20-30°C for 30-40 min and allowed to stand for 1-2 h. A wet film with a thickness of 145-155 μm was applied to a glass plate using a four-sided applicator. The film was allowed to stand at 60-70°C for 3-5 h. The coated glass plate was immersed in deionized water for 25-35 min to obtain a porous membrane. The porous membrane was then immersed in deionized water for 47-49 h, with the deionized water replaced every 11-13 h. The membrane was dried at 75-85°C for 23-25 ​​h to obtain a lithium-ion battery separator.

[0017] As an optimization, the reaction equation of the pre-modified cellulose in step (1) is:

[0018] ;

[0019] Where R is .

[0020] As an optimization, the reaction equation for modifying the cellulose in step (2) is:

[0021] ;

[0022] Where R is .

[0023] As an optimization, the reaction equation of the functionalized polysiloxane in step (3) is:

[0024] .

[0025] As an optimization, the reaction equation of the modified polypropylene in step (4) is:

[0026] .

[0027] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0028] When preparing a lithium-ion battery separator, the present invention comprises the following steps: oxidizing cellulose with sodium periodate and reacting the cellulose with DOPO to obtain pre-modified cellulose; reacting the pre-modified cellulose with thionyl chloride to obtain modified cellulose; reacting octamethylcyclotetrasiloxane, 3-dimethylaminopropyl (dimethoxy)methylsilane and vinylpentamethyldisiloxane to obtain functionalized polysiloxane; reacting polypropylene with the functionalized polysiloxane to obtain modified polypropylene; and uniformly mixing the modified polypropylene, the modified cellulose and lithium chloride and applying the mixture on a glass plate to prepare the lithium-ion battery separator.

[0029] Firstly, cellulose is oxidized with sodium periodate and then reacted with DOPO to obtain pre-modified cellulose; then the pre-modified cellulose is reacted with thionyl chloride to obtain modified cellulose; cellulose is oxidized with sodium periodate to form aldehyde groups, and then the aldehyde groups are used to undergo a phosphorus-hydrogen addition reaction and grafted with a flame retardant DOPO, thereby improving the flame retardant properties of lithium-ion battery separators; chlorine atoms are introduced into the pre-modified cellulose through a substitution reaction with thionyl chloride, thereby facilitating a subsequent quaternary ammonium reaction, forming an ionic structure and a cross-linked network, thereby improving the ion conductivity and mechanical properties of the lithium-ion battery separators.

[0030] Secondly, octamethylcyclotetrasiloxane, 3-dimethylaminopropyl (dimethoxy)methylsilane and vinyl pentamethyldisiloxane are reacted to obtain functionalized polysiloxane; polypropylene and functionalized polysiloxane are reacted to obtain modified polypropylene; modified polypropylene, modified cellulose and lithium chloride are mixed and then applied on a glass plate to prepare a lithium-ion battery separator; firstly, a functionalized polysiloxane with a single-end double bond having a dimethyl tertiary amine structure is synthesized; then, the free radicals generated by dibenzoyl peroxide are used to remove the methine hydrogen on the polypropylene to form a macromolecular free radical of polypropylene, which is grafted with the functionalized polysiloxane. Flexible, low-surface-energy long silicon-oxygen chains are introduced into the polypropylene main body to improve the mechanical properties and electrolyte wettability of the lithium-ion battery separator. At the same time, the dimethyl tertiary amine structure on the side chain can react with the chlorine on the modified cellulose to form a quaternary ammonium structure, which promotes the migration of lithium ions and the formation of a cross-linked network, further improving the ion conductivity and mechanical properties of the lithium-ion battery separator. Lithium chloride is used as a porogen and is washed off with water after film formation to form a rich pore structure, which improves the conduction of lithium ions and the penetration of electrolytes, further enhancing the electrolyte wettability and ion conductivity of the lithium-ion battery separator. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0032] A lithium ion battery separator, comprising the following preparation steps:

[0033] (1) Cellulose and deionized water were mixed in a mass ratio of 1:49, and a 30% hydrochloric acid solution was added to adjust the pH to 2. The mixture was ultrasonically dispersed for 10 min, and sodium periodate (1 times the molar amount of cellulose) was added. The mixture was stirred at 30°C and 200 rpm for 4 h in a dark environment. The mixture was naturally cooled to room temperature. Ethylene glycol (1 times the mass of cellulose) was added, and the mixture was stirred for 3 h. The mixture was filtered and washed with deionized water and anhydrous ethanol alternately for 3 times. The mixture was dried at 65°C for 12 h to obtain aldehyded cellulose. Aldehydated cellulose, DOPO, deionized water and acetonitrile were mixed in a mass ratio of 1:2:0.7:48, and stirred at 85°C and 100 rpm for 7 h. The mixture was naturally cooled to room temperature and filtered. The mixture was washed with acetonitrile and tetrahydrofuran for 3 times respectively. The mixture was dried at 50°C for 13 h to obtain pre-modified cellulose.

[0034] (2) Pre-modified cellulose and N,N-dimethylformamide were mixed at a mass ratio of 1:18, heated to 85°C at 250 r / min with stirring, and thionyl chloride in an amount 3 times the mass of the pre-modified cellulose was added at a uniform rate within 30 min. The stirring was continued for 3 h, and deionized water in an amount 40 times the mass of the pre-modified cellulose was added. The mixture was stirred at 400 r / min until the mass of the precipitated solid did not change. The mixture was filtered and washed with 2% ammonia water and deionized water for 3 times respectively. The mixture was dried at 50°C for 13 h to obtain modified cellulose.

[0035] (3) Octamethylcyclotetrasiloxane, 3-dimethylaminopropyl (dimethoxy)methylsilane and tetramethylammonium hydroxide siliconate were mixed in a mass ratio of 1:1.1:0.01, nitrogen was passed for 10 min, and the mixture was stirred at 80°C and 100 rpm for 3 h. Vinylpentamethyldisiloxane (0.2 times the mass of octamethylcyclotetrasiloxane) was added, the temperature was raised to 95°C and stirring was continued for 9 h. The temperature was raised to 140°C at 10°C / min and stirring was continued for 40 min. The mixture was distilled at 0.1 MPa for 2 h to obtain functionalized polysiloxane.

[0036] (4) Polypropylene, functionalized polysiloxane, dibenzoyl peroxide and deionized water were mixed in a mass ratio of 1:0.2:0.01:8, stirred at 100 rpm for 65 min under a nitrogen atmosphere, heated to 85 °C and continued to stir for 6 h, naturally cooled to room temperature and filtered, added deionized water 199 times the mass of polypropylene, boiled for 25 min, naturally cooled to room temperature and filtered, repeated boiling and filtering 3 times, extracted with acetone in a Soxhlet extractor for 35 h, filtered, and dried at 60 °C for 19 h to obtain modified polypropylene;

[0037] (5) Modified polypropylene, modified cellulose, lithium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:0.2:0.07:6, and the mixture was ultrasonically treated at 20°C for 40 min and allowed to stand for 2 h. A wet film with a thickness of 145 μm was applied on a glass plate using a four-sided applicator. The film was allowed to stand at 60°C for 5 h, and the coated glass plate was immersed in deionized water for 25 min to obtain a porous membrane. The porous membrane was then immersed in deionized water for 47 h, with the deionized water replaced every 13 h. The membrane was dried at 75°C for 25 h to obtain a lithium-ion battery separator.

[0038] A lithium ion battery separator, comprising the following preparation steps:

[0039] (1) Cellulose and deionized water were mixed in a mass ratio of 1:50, and a 35% hydrochloric acid solution was added to adjust the pH to 3. The mixture was ultrasonically dispersed for 15 minutes, and sodium periodate twice the molar amount of cellulose was added. The mixture was stirred at 35°C and 250 rpm for 3 hours in a dark environment. The mixture was naturally cooled to room temperature. Ethylene glycol 1.5 times the mass of cellulose was added. The mixture was stirred for 2 hours and filtered. The mixture was washed with deionized water and anhydrous ethanol alternately for 4 times and dried at 70°C for 11 hours to obtain aldehyded cellulose. Aldehydated cellulose, DOPO, deionized water and acetonitrile were mixed in a mass ratio of 1:3:0.8:49, stirred at 90°C and 150 rpm for 6 hours, naturally cooled to room temperature and filtered. The mixture was washed with acetonitrile and tetrahydrofuran for 4 times respectively and dried at 55°C for 12 hours to obtain pre-modified cellulose.

[0040] (2) Pre-modified cellulose and N,N-dimethylformamide were mixed at a mass ratio of 1:19, heated to 90°C with stirring at 300 r / min, and 3.5 times the mass of pre-modified cellulose of thionyl chloride was added at a uniform rate within 35 min. The stirring was continued for 2.5 h, and deionized water was added in an amount of 45 times the mass of the pre-modified cellulose. The mixture was stirred at 450 r / min until the mass of the precipitated solid remained unchanged, and then filtered. The mixture was washed four times with 3% ammonia water and deionized water, respectively, and dried at 60°C for 12 h to obtain modified cellulose.

[0041] (3) Octamethylcyclotetrasiloxane, 3-dimethylaminopropyl (dimethoxy)methylsilane and tetramethylammonium hydroxide siliconate were mixed in a mass ratio of 1:1.2:0.02, nitrogen was passed for 15 minutes, and the mixture was stirred at 85°C and 150 rpm for 2.5 hours. Vinylpentamethyldisiloxane (0.3 times the mass of octamethylcyclotetrasiloxane) was added, the temperature was raised to 100°C and stirring was continued for 8 hours. The temperature was raised to 135°C at 15°C / min and stirring was continued for 45 minutes. The mixture was distilled at 0.2 MPa for 1.5 hours to obtain functionalized polysiloxane.

[0042] (4) Polypropylene, functionalized polysiloxane, dibenzoyl peroxide and deionized water were mixed in a mass ratio of 1:0.25:0.02:9, stirred at 150 rpm for 60 min under a nitrogen atmosphere, heated to 90 °C and continued to stir for 5 h, naturally cooled to room temperature and filtered, added deionized water 200 times the mass of polypropylene, boiled for 30 min, naturally cooled to room temperature and filtered, repeated boiling and filtering 4 times, extracted with acetone in a Soxhlet extractor for 36 h, filtered, and dried at 65 °C for 18 h to obtain modified polypropylene;

[0043] (5) Modified polypropylene, modified cellulose, lithium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:0.3:0.08:7, and the mixture was ultrasonically treated at 25°C for 35 min and allowed to stand for 1.5 h. A wet film with a thickness of 150 μm was applied on a glass plate using a four-sided applicator. The film was allowed to stand at 65°C for 4 h, and the coated glass plate was immersed in deionized water for 30 min to obtain a porous membrane. The porous membrane was then immersed in deionized water for 48 h, with the deionized water replaced every 12 h. The membrane was dried at 80°C for 24 h to obtain a lithium-ion battery separator.

[0044] A lithium ion battery separator, comprising the following preparation steps:

[0045] (1) Cellulose and deionized water were mixed in a mass ratio of 1:51, a 40% hydrochloric acid solution was added to adjust the pH to 4, ultrasonic dispersion was performed for 20 min, sodium periodate was added in an amount 3 times the molar amount of cellulose, the mixture was stirred at 40°C and 300 rpm for 2 h in a dark environment, the mixture was naturally cooled to room temperature, ethylene glycol was added in an amount 2 times the mass of cellulose, the mixture was stirred for 1 h, filtered, washed with deionized water and anhydrous ethanol alternately for 5 times, dried at 75°C for 10 h, and aldehyde-modified cellulose was obtained; aldehyde-modified cellulose, DOPO, deionized water and acetonitrile were mixed in a mass ratio of 1:4:0.9:50, stirred at 95°C and 200 rpm for 5 h, filtered after naturally cooling to room temperature, washed with acetonitrile and tetrahydrofuran for 5 times respectively, and dried at 60°C for 11 h, and pre-modified cellulose was obtained;

[0046] (2) Pre-modified cellulose and N,N-dimethylformamide were mixed at a mass ratio of 1:20, heated to 95°C at 350 r / min with stirring, and thionyl chloride in an amount 4 times the mass of the pre-modified cellulose was added at a uniform rate within 40 min. The stirring was continued for 2 h, and deionized water in an amount 50 times the mass of the pre-modified cellulose was added. The mixture was stirred at 500 r / min until the mass of the precipitated solid did not change, and then filtered. The mixture was washed 5 times with 4% ammonia water and deionized water, respectively, and dried at 70°C for 11 h to obtain modified cellulose.

[0047] (3) Octamethylcyclotetrasiloxane, 3-dimethylaminopropyl (dimethoxy)methylsilane and tetramethylammonium hydroxide siliconate were mixed in a mass ratio of 1:1.3:0.03, nitrogen was passed through for 20 min, and the mixture was stirred at 90 °C and 200 rpm for 2 h. Vinylpentamethyldisiloxane (0.4 times the mass of octamethylcyclotetrasiloxane) was added, the temperature was raised to 105 °C and stirring was continued for 7 h. The temperature was raised to 130 °C at 20 °C / min and stirring was continued for 50 min. The mixture was distilled at 0.3 MPa for 1 h to obtain functionalized polysiloxane.

[0048] (4) Polypropylene, functionalized polysiloxane, dibenzoyl peroxide and deionized water were mixed in a mass ratio of 1:0.3:0.03:10, stirred at 200 rpm for 55 min under a nitrogen atmosphere, heated to 95 °C and continued to stir for 4 h, naturally cooled to room temperature and filtered, added with deionized water 201 times the mass of polypropylene, boiled for 35 min, naturally cooled to room temperature and filtered, repeated boiling and filtering 5 times, extracted with acetone in a Soxhlet extractor for 37 h, filtered, and dried at 70 °C for 17 h to obtain modified polypropylene;

[0049] (5) Modified polypropylene, modified cellulose, lithium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:0.4:0.09:8, and the mixture was ultrasonically treated at 30°C for 30 min and allowed to stand for 1 h. A wet film with a thickness of 155 μm was applied on a glass plate using a four-sided applicator. The film was allowed to stand at 70°C for 3 h, and the coated glass plate was immersed in deionized water for 35 min to obtain a porous membrane. The porous membrane was then immersed in deionized water for 49 h, with the deionized water replaced every 11 h. The membrane was dried at 85°C for 23 h to obtain a lithium-ion battery separator.

[0050] Comparative Example 1

[0051] A lithium ion battery separator, comprising the following preparation steps:

[0052] (1) Cellulose and N,N-dimethylformamide were mixed in a mass ratio of 1:19, heated to 90°C with stirring at 300 r / min, and 3.5 times the mass of thionyl chloride of the cellulose was added at a uniform rate within 35 min. The stirring was continued for 2.5 h, and deionized water of 45 times the mass of the cellulose was added. The mixture was stirred at 450 r / min until the mass of the precipitated solid remained unchanged, then filtered, washed with 3% ammonia water and deionized water for 4 times respectively, and dried at 60°C for 12 h to obtain modified cellulose.

[0053] (2) Octamethylcyclotetrasiloxane, 3-dimethylaminopropyl (dimethoxy)methylsilane and tetramethylammonium hydroxide siliconate were mixed in a mass ratio of 1:1.2:0.02, nitrogen was passed for 15 minutes, and the mixture was stirred at 85°C and 150 rpm for 2.5 hours. Vinylpentamethyldisiloxane (0.3 times the mass of octamethylcyclotetrasiloxane) was added, the temperature was raised to 100°C and stirring was continued for 8 hours. The temperature was raised to 135°C at 15°C / min and stirring was continued for 45 minutes. The mixture was distilled at 0.2 MPa for 1.5 hours to obtain functionalized polysiloxane.

[0054] (3) Polypropylene, functionalized polysiloxane, dibenzoyl peroxide and deionized water were mixed in a mass ratio of 1:0.25:0.02:9, stirred at 150 rpm for 60 min under a nitrogen atmosphere, heated to 90 °C and continued to stir for 5 h, naturally cooled to room temperature and filtered, added deionized water 200 times the mass of polypropylene, boiled for 30 min, naturally cooled to room temperature and filtered, repeated boiling and filtering 4 times, extracted with acetone in a Soxhlet extractor for 36 h, filtered, and dried at 65 °C for 18 h to obtain modified polypropylene;

[0055] (4) Modified polypropylene, modified cellulose, lithium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:0.3:0.08:7, and the mixture was ultrasonically treated at 25°C for 35 min and allowed to stand for 1.5 h. A wet film with a thickness of 150 μm was applied on a glass plate using a four-sided applicator. The film was allowed to stand at 65°C for 4 h, and the coated glass plate was immersed in deionized water for 30 min to obtain a porous membrane. The porous membrane was then immersed in deionized water for 48 h, with the deionized water replaced every 12 h. The membrane was dried at 80°C for 24 h to obtain a lithium-ion battery separator.

[0056] Comparative Example 2

[0057] A lithium ion battery separator, comprising the following preparation steps:

[0058] (1) Cellulose and deionized water were mixed in a mass ratio of 1:50, and a 35% hydrochloric acid solution was added to adjust the pH to 3. The mixture was ultrasonically dispersed for 15 min, and sodium periodate was added in an amount twice the molar amount of cellulose. The mixture was stirred at 35°C and 250 rpm for 3 h in a dark environment. The mixture was naturally cooled to room temperature. Ethylene glycol was added in an amount of 1.5 times the mass of cellulose. The mixture was stirred for 2 h and filtered. The mixture was washed with deionized water and anhydrous ethanol alternately for 4 times and dried at 70°C for 11 h to obtain aldehyded cellulose. Aldehydated cellulose, DOPO, deionized water and acetonitrile were mixed in a mass ratio of 1:3:0.8:49, stirred at 90°C and 150 rpm for 6 h, naturally cooled to room temperature and filtered. The mixture was washed with acetonitrile and tetrahydrofuran for 4 times respectively and dried at 55°C for 12 h to obtain modified cellulose.

[0059] (2) Octamethylcyclotetrasiloxane, 3-dimethylaminopropyl (dimethoxy)methylsilane and tetramethylammonium hydroxide siliconate were mixed in a mass ratio of 1:1.2:0.02, nitrogen was passed for 15 minutes, and the mixture was stirred at 85°C and 150 rpm for 2.5 hours. Vinylpentamethyldisiloxane (0.3 times the mass of octamethylcyclotetrasiloxane) was added, the temperature was raised to 100°C and stirring was continued for 8 hours. The temperature was raised to 135°C at 15°C / min and stirring was continued for 45 minutes. The mixture was distilled at 0.2 MPa for 1.5 hours to obtain functionalized polysiloxane.

[0060] (3) Polypropylene, functionalized polysiloxane, dibenzoyl peroxide and deionized water were mixed in a mass ratio of 1:0.25:0.02:9, stirred at 150 rpm for 60 min under a nitrogen atmosphere, heated to 90 °C and continued to stir for 5 h, naturally cooled to room temperature and filtered, added deionized water 200 times the mass of polypropylene, boiled for 30 min, naturally cooled to room temperature and filtered, repeated boiling and filtering 4 times, extracted with acetone in a Soxhlet extractor for 36 h, filtered, and dried at 65 °C for 18 h to obtain modified polypropylene;

[0061] (4) Modified polypropylene, modified cellulose, lithium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:0.3:0.08:7, and the mixture was ultrasonically treated at 25°C for 35 min and allowed to stand for 1.5 h. A wet film with a thickness of 150 μm was applied on a glass plate using a four-sided applicator. The film was allowed to stand at 65°C for 4 h, and the coated glass plate was immersed in deionized water for 30 min to obtain a porous membrane. The porous membrane was then immersed in deionized water for 48 h, with the deionized water replaced every 12 h. The membrane was dried at 80°C for 24 h to obtain a lithium-ion battery separator.

[0062] Comparative Example 3

[0063] A lithium ion battery separator, comprising the following preparation steps:

[0064] (1) Cellulose and deionized water were mixed in a mass ratio of 1:50, and a 35% hydrochloric acid solution was added to adjust the pH to 3. The mixture was ultrasonically dispersed for 15 minutes, and sodium periodate twice the molar amount of cellulose was added. The mixture was stirred at 35°C and 250 rpm for 3 hours in a dark environment. The mixture was naturally cooled to room temperature. Ethylene glycol 1.5 times the mass of cellulose was added. The mixture was stirred for 2 hours and filtered. The mixture was washed with deionized water and anhydrous ethanol alternately for 4 times and dried at 70°C for 11 hours to obtain aldehyded cellulose. Aldehydated cellulose, DOPO, deionized water and acetonitrile were mixed in a mass ratio of 1:3:0.8:49, stirred at 90°C and 150 rpm for 6 hours, naturally cooled to room temperature and filtered. The mixture was washed with acetonitrile and tetrahydrofuran for 4 times respectively and dried at 55°C for 12 hours to obtain pre-modified cellulose.

[0065] (2) Pre-modified cellulose and N,N-dimethylformamide were mixed at a mass ratio of 1:19, heated to 90°C with stirring at 300 r / min, and 3.5 times the mass of pre-modified cellulose of thionyl chloride was added at a uniform rate within 35 min. The stirring was continued for 2.5 h, and deionized water was added in an amount of 45 times the mass of the pre-modified cellulose. The mixture was stirred at 450 r / min until the mass of the precipitated solid remained unchanged, and then filtered. The mixture was washed four times with 3% ammonia water and deionized water, respectively, and dried at 60°C for 12 h to obtain modified cellulose.

[0066] (3) Polypropylene, modified cellulose, lithium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:0.3:0.08:7, and the mixture was ultrasonically treated at 25°C for 35 min and then allowed to stand for 1.5 h. A wet film with a thickness of 150 μm was applied on a glass plate using a four-sided applicator. The film was allowed to stand at 65°C for 4 h, and the coated glass plate was immersed in deionized water for 30 min to obtain a porous membrane. The porous membrane was then immersed in deionized water for 48 h, with the deionized water replaced every 12 h. The membrane was dried at 80°C for 24 h to obtain a lithium-ion battery separator.

[0067] Comparative Example 4

[0068] A lithium ion battery separator, comprising the following preparation steps:

[0069] (1) Cellulose and deionized water were mixed in a mass ratio of 1:50, and a 35% hydrochloric acid solution was added to adjust the pH to 3. The mixture was ultrasonically dispersed for 15 minutes, and sodium periodate twice the molar amount of cellulose was added. The mixture was stirred at 35°C and 250 rpm for 3 hours in a dark environment. The mixture was naturally cooled to room temperature. Ethylene glycol 1.5 times the mass of cellulose was added. The mixture was stirred for 2 hours and filtered. The mixture was washed with deionized water and anhydrous ethanol alternately for 4 times and dried at 70°C for 11 hours to obtain aldehyded cellulose. Aldehydated cellulose, DOPO, deionized water and acetonitrile were mixed in a mass ratio of 1:3:0.8:49, stirred at 90°C and 150 rpm for 6 hours, naturally cooled to room temperature and filtered. The mixture was washed with acetonitrile and tetrahydrofuran for 4 times respectively and dried at 55°C for 12 hours to obtain pre-modified cellulose.

[0070] (2) Pre-modified cellulose and N,N-dimethylformamide were mixed at a mass ratio of 1:19, heated to 90°C with stirring at 300 r / min, and 3.5 times the mass of pre-modified cellulose of thionyl chloride was added at a uniform rate within 35 min. The stirring was continued for 2.5 h, and deionized water was added in an amount of 45 times the mass of the pre-modified cellulose. The mixture was stirred at 450 r / min until the mass of the precipitated solid remained unchanged, and then filtered. The mixture was washed four times with 3% ammonia water and deionized water, respectively, and dried at 60°C for 12 h to obtain modified cellulose.

[0071] (3) Octamethylcyclotetrasiloxane, 3-dimethylaminopropyl (dimethoxy)methylsilane and tetramethylammonium hydroxide siliconate were mixed in a mass ratio of 1:1.2:0.02, nitrogen was passed for 15 minutes, and the mixture was stirred at 85°C and 150 rpm for 2.5 hours. Vinylpentamethyldisiloxane (0.3 times the mass of octamethylcyclotetrasiloxane) was added, the temperature was raised to 100°C and stirring was continued for 8 hours. The temperature was raised to 135°C at 15°C / min and stirring was continued for 45 minutes. The mixture was distilled at 0.2 MPa for 1.5 hours to obtain functionalized polysiloxane.

[0072] (4) Polypropylene, functionalized polysiloxane, dibenzoyl peroxide and deionized water were mixed in a mass ratio of 1:0.25:0.02:9, stirred at 150 rpm for 60 min under a nitrogen atmosphere, heated to 90 °C and continued to stir for 5 h, naturally cooled to room temperature and filtered, added deionized water 200 times the mass of polypropylene, boiled for 30 min, naturally cooled to room temperature and filtered, repeated boiling and filtering 4 times, extracted with acetone in a Soxhlet extractor for 36 h, filtered, and dried at 65 °C for 18 h to obtain modified polypropylene;

[0073] (5) Modified polypropylene, modified cellulose and N-methylpyrrolidone were mixed in a mass ratio of 1:0.3:7, and the mixture was ultrasonically treated at 25°C for 35 min and allowed to stand for 1.5 h. A wet film with a thickness of 150 μm was applied on a glass plate using a four-sided applicator. The mixture was allowed to stand at 65°C for 4 h, and then immersed in deionized water for 48 h. The deionized water was replaced every 12 h, and the mixture was dried at 80°C for 24 h to obtain a lithium-ion battery separator.

[0074] Test Case

[0075] 1. Flame retardant performance test

[0076] Test method: The lithium-ion battery separators obtained in each embodiment and the comparative example were cut into a size of 50 mm*150 mm, and the limiting oxygen index was measured according to GB / T2406.

[0077] 2. Ionic conductivity test

[0078] Test method: The lithium-ion battery separator obtained in each embodiment and the comparative example were cut into membrane disc samples with a diameter of 20 mm, and two stainless steel discs with a diameter of 15.8 mm were used as electrode sheets. A simple simulated battery was assembled in the order of stainless steel disc / diaphragm soaked in electrolyte for 12 hours / stainless steel disc. The AC impedance R was measured at 25°C. b Calculate the ionic conductivity σ = thickness / R b ·area.

[0079] 3. Electrolyte wettability test

[0080] Test method: Take the lithium-ion battery separator obtained in each embodiment and the comparative example and weigh the same mass W1, immerse the separator in the electrolyte for 30 minutes and then take it out, wipe off the excess electrolyte on the surface with filter paper, weigh the mass W2 again, calculate the liquid absorption rate = W2-W1 / W1*100%, and judge the wettability.

[0081] 4. Mechanical properties test

[0082] Test method: The lithium-ion battery separators obtained in each embodiment and the comparative example were cut into strips of 15 mm*100 mm, and the tensile strength of the separators was tested on a universal testing machine at a tensile rate of 20 mm / min.

[0083] Table 1 below shows the analysis results of the flame retardancy, ion conductivity, electrolyte wettability and mechanical properties of the lithium ion battery separators of Examples 1 to 3 of the present invention and Comparative Examples 1 to 3.

[0084] Table 1

[0085] Limiting oxygen index% Ionic conductivity mS / cm2 Liquid absorption rate% Tensile strength MPa Example 1 31.9 0.92 324 172 Example 2 32.3 0.97 328 176 Example 3 32.1 0.94 319 175 Comparative Example 1 16.2 0.90 312 169 Comparative Example 2 30.7 0.34 287 72 Comparative Example 3 28.9 0.28 141 67 Comparative Example 4 30.9 0.02 137 176

[0086] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be found that the lithium ion battery separator prepared by the present invention has good flame retardancy, ion conductivity, electrolyte wettability and mechanical properties.

[0087] By comparison, the limiting oxygen index of Examples 1, 2, and 3 is higher than that of Comparative Example 1, indicating that the flame retardant properties of the lithium-ion battery separator are improved by oxidizing cellulose with sodium periodate to form aldehyde groups, then utilizing the aldehyde groups to undergo a phosphorus-hydrogen addition reaction, and grafting the flame retardant DOPO.

[0088] By comparison, the ionic conductivity and tensile strength of Examples 1, 2, and 3 are higher than those of Comparative Example 2, indicating that the substitution reaction of thionyl chloride is used to introduce chlorine atoms into the pre-modified cellulose, which facilitates the subsequent quaternary ammonium reaction, forms an ionic structure, and forms a cross-linked network, thereby improving the ionic conductivity and mechanical properties of the lithium-ion battery separator.

[0089] By comparison, the ionic conductivity, liquid absorption rate and tensile strength of Examples 1, 2 and 3 are higher than those of Comparative Example 3, indicating that the free radicals generated by dibenzoyl peroxide remove the dimethyl hydrogen on the polypropylene to form a macromolecular free radical of polypropylene, which is grafted with functionalized polysiloxane, and flexible, low surface energy silicon oxygen long chains are introduced into the polypropylene body, thereby improving the mechanical properties and electrolyte wettability of the lithium ion battery separator; at the same time, the dimethyl tertiary amine structure on the side chain can react with the chlorine on the modified cellulose to form a quaternary ammonium structure, which promotes the migration of lithium ions and the formation of a cross-linked network, thereby further improving the ion conductivity and mechanical properties of the lithium ion battery separator.

[0090] By comparison, Examples 1, 2, and 3 have higher ionic conductivity and liquid absorption rate than Comparative Example 4, indicating that lithium chloride is used as a porogen and washed away with water after film formation to form a rich pore structure, thereby improving the conduction of lithium ions and the penetration of electrolyte, and enhancing the electrolyte wettability and ion conductivity of the lithium ion battery separator.

[0091] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A lithium ion battery separator, characterized in that: The method comprises the following preparation steps: (1) Mix cellulose and deionized water in a mass ratio of 1:(49-51), add 30-40% hydrochloric acid solution to adjust the pH to 2-4, ultrasonically disperse for 10-20 min, add 1-3 times the molar amount of sodium periodate of cellulose, stir at 30-40 °C and 200-300 rpm for 2-4 h in a dark environment, cool naturally to room temperature, add 1-2 times the mass of cellulose of ethylene glycol, continue stirring for 1-3 h, filter, and rinse with deionized water and anhydrous ethanol. Wash alternately 3 to 5 times, dry at 65 to 75°C for 10 to 12 hours to obtain aldehyded cellulose; mix aldehyded cellulose, DOPO, deionized water and acetonitrile in a mass ratio of 1:(2 to 4):(0.7 to 0.9):(48 to 50), stir at 85 to 95°C and 100 to 200 rpm for 5 to 7 hours, cool naturally to room temperature and filter, wash with acetonitrile and tetrahydrofuran for 3 to 5 times respectively, and dry at 50 to 60°C for 11 to 13 hours to obtain pre-modified cellulose; (2) Pre-modified cellulose and N,N-dimethylformamide were mixed in a mass ratio of 1:(18-20), stirred at 250-350 r / min and heated to 85-95°C, 3-4 times the mass of pre-modified cellulose of thionyl chloride was added at a uniform rate within 30-40 min, and stirring was continued for 2-3 h. Deionized water of 40-50 times the mass of pre-modified cellulose was added, and stirred at 400-500 r / min until the mass of precipitated solids remained unchanged, then filtered, washed with 2-4% ammonia water and deionized water for 3-5 times respectively, and dried at 50-70°C for 11-13 h to obtain modified cellulose; (3) Octamethylcyclotetrasiloxane, 3-dimethylaminopropyl (dimethoxy)methylsilane and tetramethylammonium hydroxide silicon alkoxide are mixed in a mass ratio of 1:(1.1-1.3):(0.01-0.03), nitrogen is passed through for 10-20 min, and the mixture is stirred at 80-90°C and 100-200 rpm for 2-3 h. Vinylpentamethyldisiloxane (0.2-0.4 times the mass of octamethylcyclotetrasiloxane) is added, the mixture is heated to 95-105°C and stirred for 7-9 h. The mixture is heated to 130-140°C at a rate of 10-20°C / min and stirred for 40-50 min. The mixture is distilled at 0.1-0.3 MPa for 1-2 h to obtain a functionalized polysiloxane. (4) Polypropylene, functionalized polysiloxane, dibenzoyl peroxide and deionized water are mixed in a mass ratio of 1:(0.2-0.3):(0.01-0.03):(8-10), stirred at 100-200 rpm for 55-65 min under a nitrogen atmosphere, heated to 85-95°C and continued to stir for 4-6 h, naturally cooled to room temperature and filtered, added with deionized water 199-201 times the mass of polypropylene, boiled for 25-35 min, naturally cooled to room temperature and filtered, repeated boiling and filtering 3-5 times, extracted with acetone in a Soxhlet extractor for 35-37 h, filtered, and dried at 60-70°C for 17-19 h to obtain modified polypropylene; (5) Modified polypropylene, modified cellulose, lithium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:(0.2-0.4):(0.07-0.09):(6-8), and the mixture was ultrasonically treated at 20-30°C for 30-40 min and allowed to stand for 1-2 h. A wet film with a thickness of 145-155 μm was applied to a glass plate using a four-sided applicator. The film was allowed to stand at 60-70°C for 3-5 h. The coated glass plate was immersed in deionized water for 25-35 min to obtain a porous membrane. The porous membrane was then immersed in deionized water for 47-49 h, with the deionized water replaced every 11-13 h. The membrane was dried at 75-85°C for 23-25 ​​h to obtain a lithium-ion battery separator.

2. A lithium ion battery separator according to claim 1, characterized in that: The reaction equation of the pre-modified cellulose in step (1) is: ; Where R is .

3. A lithium ion battery separator according to claim 1, characterized in that: The reaction equation for the modified cellulose in step (2) is: ; Where R is .

4. A lithium ion battery separator according to claim 1, characterized in that: The reaction equation of the functionalized polysiloxane in step (3) is: 。 5. A lithium ion battery separator according to claim 1, characterized in that: The reaction equation of the modified polypropylene in step (4) is: 。 6. A lithium ion battery, characterized in that: The battery separator of the lithium ion battery is the lithium ion battery separator according to any one of claims 1 to 5.