Dry electrode sheet and preparation method thereof, and battery
By forming a rectangular array structure of large blind holes and small blind holes on the surface of the dry electrode plate and treating it with naphthalene lithium solution, the problem of poor electrolyte wettability is solved and the ion conductivity and battery life of the lithium-ion battery are improved.
Patent Information
- Application Number
- CN202410980634.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Dry electrodes have poor electrolyte wettability in lithium-ion batteries, resulting in low ionic conductivity and affecting charge and discharge efficiency and battery life.
Laser drilling technology is used to form a rectangular array structure of large blind holes and small blind holes on the surface of the dry electrode pole piece, and the wettability and surface energy of the electrolyte are improved by infiltration treatment with naphthalene lithium solution.
It significantly improves the permeability and uniform distribution of the electrolyte, shortens the ion transmission path, improves the rate performance and cycle life of the battery, and reduces the risk of local overheating and side reactions.
Smart Images

Figure CN118522856B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new energy batteries, and in particular to a dry electrode sheet and a preparation method thereof, and a battery. Background Art
[0002] As the global demand for renewable energy increases, lithium-ion batteries have been widely used as an efficient energy storage device. From consumer electronics to electric vehicles and large-scale energy storage systems, the market demand for lithium-ion batteries continues to grow. Although the traditional wet electrode manufacturing process is mature, it has many limitations, such as environmental pollution, high production costs and process complexity. In order to overcome these problems, dry electrode technology came into being and became an important innovation direction in the field of lithium-ion battery manufacturing.
[0003] At present, a variety of surface treatment technologies are applied in the manufacturing process of dry electrodes, with the aim of improving the conductivity, wettability, adhesion and other properties of dry electrode materials. These treatment technologies mainly include physical and chemical methods. The following are some common surface treatment technologies:
[0004] Plasma treatment introduces polar functional groups or cleans the surface through the interaction between high-energy particles and the material surface, thereby increasing surface energy and improving the adhesion and wettability of the material. It coats a layer of chemical substances on the surface of the electrode material to form a protective layer or functional layer through chemical reactions, thereby improving the stability and performance of the material. It uses the cavitation effect generated by ultrasound in the liquid to clean and modify the material surface.
[0005] The development of dry electrode technology benefits from the application of a variety of surface treatment technologies, which work together to significantly improve the performance and stability of electrode materials. Through continuous optimization and innovation of surface treatment methods, the application prospects of dry electrodes in lithium-ion battery manufacturing will be broader.
[0006] Dry electrode technology uses PTFE (Polytetrafluoro-Ethylene) as a binder. Although PTFE has excellent chemical stability and mechanical properties as a binder in dry electrodes, the extremely low surface energy of PTFE makes PTFE highly hydrophobic, preventing aqueous and organic electrolytes from being evenly distributed and permeated on its surface. Due to the low surface energy of PTFE, it is difficult for the electrolyte to be evenly distributed on the electrode surface, which may lead to insufficient electrolyte in local areas, thus affecting the overall performance of the battery. Poor wettability will hinder the conduction of ions between electrode materials, reduce the ion conductivity of the battery, and further affect the charge and discharge efficiency. Poor electrolyte wettability will also lead to a decrease in the utilization rate of electrode active materials, and the capacity and cycle life of the battery may be negatively affected.
[0007] The surface energy of PTFE can be increased and the wettability of electrolyte can be improved by using methods such as plasma treatment, surface coating, mixed binder, and surface activation treatment. However, each method has its own disadvantages and limitations. For example, plasma treatment requires special equipment and precise control of treatment parameters, which is costly; surface coating increases process complexity and cost. Therefore, a surface treatment method suitable for large-scale production and effective in improving the wettability of dry electrode electrolyte is needed. Summary of the invention
[0008] The technical problem to be solved by the embodiments of the present invention is to provide a dry electrode plate and a preparation method thereof, and a battery, so as to improve the electrolyte wettability of the dry electrode plate.
[0009] In order to solve the above technical problems, an embodiment of the present invention proposes a dry electrode plate, including a dry electrode plate, wherein N×M large blind holes are arranged on the surface of the dry electrode plate, and the large blind holes form a rectangular array of N rows×M columns, and small blind holes are correspondingly arranged between adjacent large blind holes in the M columns of large blind holes, and the small blind holes form a rectangular array of (N-1) rows×M columns, and N and M are both positive integers greater than 2.
[0010] Furthermore, the hole depths of the large blind hole and the small blind hole are both less than or equal to half the thickness of the dry electrode; the aperture of the large blind hole is less than or equal to the hole depth of the large blind hole, and the aperture of the small blind hole is less than or equal to the hole depth of the small blind hole; the aperture of the large blind hole is larger than the aperture of the small blind hole.
[0011] Furthermore, the column spacing between the large blind holes ranges from 90 microns to 110 microns, the row spacing between the large blind holes ranges from 25 microns to 35 microns, the row spacing between the small blind holes ranges from 15 microns to 25 microns, the column spacing between the small blind holes and the large blind holes ranges from 45 microns to 55 microns, the aperture size of the large blind holes ranges from 50 microns to 80 microns, the aperture size of the small blind holes ranges from 35 microns to 55 microns, the hole depth of the large blind holes ranges from 70 microns to 110 microns, and the hole depth of the small blind holes ranges from 45 microns to 85 microns.
[0012] Furthermore, both the large blind hole and the small blind hole are inverted tapered blind holes.
[0013] Furthermore, the dry-process electrode comprises the following components by mass percentage: 80%-98% active material, 1%-10% conductive agent, and 1%-10% binder;
[0014] Among them, the active material is a positive electrode active material or a negative electrode active material, the positive electrode active material includes one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide and lithium cobalt oxide, the negative electrode active material includes one or more of graphite, soft carbon, hard carbon, and mesophase carbon microbeads, the binder material is polytetrafluoroethylene, and the conductive agent includes one or more of conductive carbon black, carbon nanotubes, graphene, carbon fiber, acetylene black and Ketjen black.
[0015] Furthermore, the dry-process electrode is wetted with a naphthalene-lithium solution.
[0016] Accordingly, an embodiment of the present invention further provides a method for preparing a dry electrode sheet, comprising:
[0017] Step 1: dry-mixing the positive electrode active material or the negative electrode active material with the conductive agent and the binder to prepare a dry electrode sheet;
[0018] Step 2: Use laser to punch holes on the surface of the dry electrode to obtain a punched dry electrode;
[0019] Step 3: Use naphthalene lithium solution to wet the punched dry electrode sheet to obtain a dry electrode sheet.
[0020] Furthermore, the naphthalene-lithium solution is prepared by dissolving lithium metal in liquid ammonia and then adding naphthalene.
[0021] Correspondingly, an embodiment of the present invention further provides a battery, comprising the above-mentioned dry electrode plate, or a dry electrode plate prepared by the above-mentioned method for preparing the dry electrode plate.
[0022] The beneficial effects of the present invention are:
[0023] (1) The present invention can significantly increase the surface area of the dry electrode plate by laser drilling, and the two blind holes with different apertures can improve the permeability and uniform distribution of the electrolyte inside the electrode plate, and improve the ion conductivity of the battery. This structure of the present invention can promote the electrolyte to penetrate into the electrode material faster and more evenly, and improve the reaction efficiency; the capillary action of the blind hole helps to improve the wettability of the electrolyte of the dry electrode plate, making it easier for the electrolyte to penetrate into the dry electrode plate, shortening the ion transmission path and improving the ion transmission rate. Holes with different apertures can provide transmission channels of various sizes, making the transmission of ions inside the electrode smoother, reducing resistance, and thus improving the rate performance of the dry electrode cell; laser drilling can create a uniform and orderly pore structure, which helps to evenly distribute the electrolyte and reduce the risk of local electrolyte loss. The multi-porous structure helps to dissipate heat inside the battery. Holes with different apertures can effectively disperse the current density and reduce the current concentration effect, thereby reducing the probability of local overheating and side reactions, reducing the accumulation of heat inside the battery, reducing the battery operating temperature, extending the battery life and improving safety. Punching can relieve the thermal expansion stress generated by the battery during the charging and discharging process, and reduce the mechanical stress and damage of the battery material. Holes with different pore sizes can effectively disperse the current density and reduce the current concentration effect, thereby reducing the probability of local overheating and side reactions and extending the cycle life of the battery.
[0024] (2) The present invention soaks the punched electrode in a naphthalene-lithium solution. The naphthalene-lithium solution is a strong reducing agent that can react with the PTFE on the surface of the dry electrode electrode material to change its chemical properties and surface energy, thereby further improving the wettability of the electrolyte and the electrochemical activity of the electrode. At the same time, the lithium ions in the naphthalene-lithium solution can be embedded in the dry electrode electrode to compensate for the lithium ion loss during the first charge and discharge process, thereby improving the first coulomb efficiency of the dry electrode battery cell. This helps to form a more stable and uniform SEI film, reduce the side reactions between the dry electrode surface and the electrolyte, and thus extend the cycle life of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a structural diagram of a dry electrode plate according to an embodiment of the present invention.
[0026] Figure 2 It is a cross-sectional schematic diagram of a dry electrode plate according to an embodiment of the present invention and a schematic diagram of the specifications of a large blind hole and a small blind hole.
[0027] Figure 3 This is a test diagram of the electrolyte wetting angle of the comparative example of the present invention.
[0028] Figure 4 This is a test diagram of the electrolyte wetting angle of Example 1 of the present invention.
[0029] Figure 5This is a test diagram of the electrolyte wetting angle of Example 2 of the present invention.
[0030] Figure 6 This is a test diagram of the electrolyte wetting angle of Example 3 of the present invention.
[0031] Description of Figure Numbers
[0032] Dry-process electrode 1, large blind via 2, small blind via 3, current collector 4, large blind via row 5, small blind via row 6. DETAILED DESCRIPTION
[0033] It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments may be combined with each other. The present invention is further described in detail below in conjunction with the drawings and specific embodiments.
[0034] In the embodiments of the present invention, if there are directional indications (such as up, down, left, right, front, back, etc.), they are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0035] In addition, in the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.
[0036] Please refer to Figure 1-2 , the dry electrode plate of the embodiment of the present invention includes a dry electrode plate.
[0037] The dry electrode plate uses PTFE as a binder powder to form a film, which can achieve high thickness and high compaction effect, and improve the energy density of the battery. However, due to the strong hydrophobicity of PTFE, the dry electrode plate has the problem of poor electrolyte wettability, which has an adverse effect on the capacity of the battery, so the dry electrode plate needs to be surface treated.
[0038] The surface of the dry-process electrode is provided with N×M large blind holes, and the large blind holes form a rectangular array of N rows×M columns. Small blind holes are correspondingly provided between the adjacent large blind holes of the M columns of large blind holes, and the small blind holes form a rectangular array of (N-1) rows×M columns, where N and M are both positive integers greater than 2. The large number of blind holes on the surface of the dry-process electrode will produce capillary action, greatly improving the wettability of the electrolyte, which can effectively solve the problem of poor wettability of the dry-process electrode electrolyte and improve the rate performance and capacity release of the battery cell. The dry-process electrode after drilling is treated with a naphthalene-lithium solution for infiltration. The strong reducing property of the naphthalene-lithium solution destroys and increases the surface energy of PTFE, further improving the electrolyte wettability of the dry-process electrode, and the lithium ions in the naphthalene-lithium solution will be embedded in the dry-process electrode to compensate for the lithium ion loss after the formation of SEI, thereby improving the first coulombic efficiency of the battery cell.
[0039] The aperture and depth of the large and small blind holes match. The dry-process electrode is prepared by dry mixing the positive / negative active materials with the conductive agent and the binder. In the specific implementation, the dry mixing can be carried out by high-speed homogenization for 5min-30min. The thickness of the dry-process electrode after calendering is 200μm-500μm, and the thickness after compounding with the carbon-coated current collector is 210μm-510μm.
[0040] In terms of mass percentage, the dry electrode includes: 80%-98% active material, 1%-10% binder and 1%-10% conductive agent. The binder material is polytetrafluoroethylene. The conductive agent includes one or a combination of conductive carbon black, carbon nanotubes, graphene, carbon fiber, acetylene black and Ketjen black. The positive electrode active material includes one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide and lithium cobalt oxide. The negative electrode active material includes one or more of graphite, soft carbon, hard carbon, and mesophase carbon microspheres.
[0041] The method for preparing a dry electrode sheet of the present invention comprises steps 1 to 3.
[0042] Step 1: Dry-mix the positive electrode active material or the negative electrode active material with the conductive agent and the binder to prepare a dry electrode sheet.
[0043] Step 2: Use laser to punch holes on the surface of the dry-process electrode to obtain a punched dry-process electrode.
[0044] Mechanical drilling is a common way to treat the surface of the electrode in the industry, but it has low accuracy and consistency, and there may be certain deviations in the hole diameter and position, which affects the consistency and performance of the battery. The present invention uses laser drilling, which can achieve very high hole diameter and hole spacing accuracy, usually at the micron level. This makes the hole distribution of the dry electrode electrode more uniform, which is beneficial to the consistency of the battery performance.
[0045] Step 3: Use naphthalene lithium solution to soak the punched dry electrode piece for 0.5 to 1.5 minutes to obtain a dry electrode piece. The dry electrode piece has the problem of low initial coulombic efficiency. The present invention uses naphthalene lithium solution to soak the dry electrode piece. The strong reducing property of naphthalene lithium solution can increase the surface energy of PTFE, further improve the electrolyte wettability of the dry electrode piece, and pre-lithiation is performed to solve the problem of low initial coulombic efficiency.
[0046] As an embodiment, the naphthalene lithium solution is prepared by dissolving lithium metal in liquid ammonia and then adding naphthalene. First dissolve the lithium: Dissolve the lithium metal in liquid ammonia to form a blue solution. This is due to the color change caused by the dissolution of lithium electrons in ammonia. Then add naphthalene: Add naphthalene to the above solution, and the color of the solution will change from blue to dark green or black, indicating the formation of naphthalene lithium. The main components of the naphthalene lithium solution are naphthalene anions ( ) and lithium cations ( ), the compound they form is generally called naphthalene lithium. The preparation chemical formula of naphthalene lithium solution is: .
[0047] The battery of the present invention comprises a dry electrode plate, and the dry electrode plate is compounded on the surface of the current collector.
[0048] Comparative Example:
[0049] By mass percentage, 94% lithium manganese oxide active material, 4% binder, and 2% conductive agent are used; the binder material is polytetrafluoroethylene, and the conductive agent is conductive carbon black. All materials are dried in a drying oven at 60°C for 12 hours to remove moisture from the materials to prevent moisture from affecting subsequent processes. The mixed powder is processed in a high-speed homogenizer for 15 minutes, and then calendered. After calendering, it is compounded with the current collector, and the thickness after compounding is 250 microns.
[0050] like Figure 1 As shown, the dry electrode plate is laser-drilled, and two groups of lasers are used to simultaneously drill large and small blind holes. Figure 2 As shown, the large blind hole column spacing w2 is 100 microns, the small blind hole and large blind hole column spacing w1 is 50 microns, the large blind hole aperture r1 is 60 microns, the small blind hole aperture r2 is 40 microns, the large blind hole row spacing (i.e., the row spacing between N rows of large blind holes) d1 is 30 microns, the small blind hole row spacing d2 is 20 microns, the large blind hole depth h1 is 80 microns, the small blind hole depth h2 is 60 microns, and the laser setting parameters are shown in Table 1. A high-power MOPA fiber laser is used to perform laser cleaning on the above-mentioned area; after the drilling is completed, a high-pressure airflow is used to clean the dust and impurities on the surface of the electrode to ensure that the hole is clean and free of residue. The electrolyte wetting angle test is performed on the dry electrode after drilling, and the test results are shown in Table 1. Figure 3 .
[0051] Table 1
[0052] Example 1
[0053] By mass percentage, 94% lithium manganese oxide active material, 4% binder, and 2% conductive agent are used; the binder material is polytetrafluoroethylene, and the conductive agent is conductive carbon black. All materials are dried in a drying oven at 60°C for 12 hours to remove moisture from the materials to prevent moisture from affecting subsequent processes. The mixed powder is processed in a high-speed homogenizer for 15 minutes, and the thickness after calendering and compounding is 250 microns.
[0054] like Figure 1 As shown, the dry electrode plate is laser-drilled, and two groups of lasers are used to simultaneously drill large and small blind holes. Figure 2 As shown, the large blind hole column spacing w2 is 100 microns, the small blind hole and large blind hole column spacing w1 is 50 microns, the large blind hole aperture r1 is 60 microns, the small blind hole aperture r2 is 40 microns, the large blind hole row spacing d1 is 30 microns, the small blind hole row spacing d2 is 20 microns, the large blind hole depth h1 is 80 microns, the small blind hole depth h2 is 60 microns, and the laser setting parameters are shown in Table 2. A high-power MOPA fiber laser is used to perform laser cleaning on the above-mentioned area; after the drilling is completed, a high-pressure airflow is used to clean the dust and impurities on the surface of the electrode to ensure that the hole is clean and free of residue. The dry electrode after drilling is treated with a naphthalene lithium solution for 0.5 minutes to obtain a dry electrode electrode, and then the electrolyte infiltration angle test is performed on the dry electrode electrode. The test results are shown in Figure 4 shown.
[0055] Table 2
[0056] Example 2
[0057] By mass percentage, 94% lithium iron phosphate active material, 4% binder, and 2% conductive agent are used; the binder material is polytetrafluoroethylene, and the conductive agent is conductive carbon black. All materials are dried in a drying oven at 60°C for 12 hours to remove moisture from the materials to prevent moisture from affecting subsequent processes. The mixed powder is processed in a high-speed homogenizer for 15 minutes, and the thickness after calendering and compounding is 300 microns.
[0058] like Figure 1 As shown, the dry electrode plate is laser-drilled, and two groups of lasers are used to simultaneously drill large and small blind holes. Figure 2As shown, the column spacing w2 of the large blind holes is 100 microns, the column spacing w1 between the small blind holes and the large blind holes is 50 microns, the aperture r1 of the large blind holes is 70 microns, the aperture r2 of the small blind holes is 50 microns, the row spacing d1 of the large blind holes is 30 microns, the row spacing d2 of the small blind holes is 20 microns, the hole depth h1 of the large blind holes is 100 microns, the hole depth h2 of the small blind holes is 80 microns, and the laser setting parameters are shown in Table 3. A high-power MOPA fiber laser is used to perform laser cleaning on the above-mentioned area; after the drilling is completed, a high-pressure airflow is used to clean the dust and impurities on the surface of the electrode to ensure that the holes are clean and free of residue. The dry electrode piece with the hole cleaned is infiltrated with a naphthalene lithium solution for 1 minute to obtain a dry electrode piece, and then the electrolyte infiltration angle test is performed on the dry electrode piece. The test results are shown in Figure 5 shown.
[0059] Table 3
[0060] Example 3
[0061] According to the percentage by mass, 94% of graphite active material, 4% of adhesive, and 2% of conductive agent are selected; the adhesive material is polytetrafluoroethylene, and the conductive agent is conductive carbon black. All materials are dried in a drying oven at 60°C for 12 hours to remove moisture from the materials to prevent moisture from affecting subsequent processes. The mixed powder is processed in a high-speed homogenizer for 15 minutes, and the thickness after calendering and compounding is 200 microns.
[0062] like Figure 1 As shown, the dry electrode plate is laser-drilled, and two groups of lasers are used to simultaneously drill large and small blind holes. Figure 2 As shown, the large blind hole column spacing w2 is 100 microns, the small blind hole and large blind hole column spacing w1 is 50 microns, the large blind hole aperture r1 is 70 microns, the small blind hole aperture r2 is 50 microns, the large blind hole row spacing d1 is 30 microns, the small blind hole row spacing d2 is 20 microns, the large blind hole depth h1 is 80 microns, the small blind hole depth h2 is 50 microns, and the laser setting parameters are shown in Table 4. A high-power MOPA fiber laser is used to perform laser cleaning on the above-mentioned area; after the drilling is completed, a high-pressure airflow is used to clean the dust and impurities on the surface of the electrode to ensure that the hole is clean and free of residue. The dry electrode piece with the hole cleaned is infiltrated with a naphthalene lithium solution for 1.5 minutes to obtain a dry electrode piece, and then the electrolyte infiltration angle test is performed on the dry electrode piece. The test results are shown in Figure 6 shown.
[0063] Table 4
[0064]
[0065] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A dry electrode plate, comprising a dry electrode plate, It is characterized in that The surface of the dry electrode is provided with N×M large blind holes, the large blind holes form a rectangular array of N rows×M columns, small blind holes are correspondingly provided between adjacent large blind holes in the M columns, the small blind holes form a rectangular array of (N-1) rows×M columns, and N and M are both positive integers greater than 2; The dry-process electrode comprises the following components by mass percentage: 80%-98% active material, 1%-10% conductive agent, and 1%-10% binder; The active material is a positive electrode active material or a negative electrode active material, the positive electrode active material includes one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide and lithium cobalt oxide, the negative electrode active material includes one or more of graphite, soft carbon, hard carbon, and mesophase carbon microspheres, the binder material is polytetrafluoroethylene, and the conductive agent includes one or more of conductive carbon black, carbon nanotubes, graphene, and carbon fibers; The dry-process electrode is wetted with a naphthalene-lithium solution.
2. The dry electrode sheet according to claim 1, It is characterized in that The depths of the large blind holes and the small blind holes are both less than or equal to half the thickness of the dry electrode; the diameter of the large blind hole is less than or equal to the depth of the large blind hole, and the diameter of the small blind hole is less than or equal to the depth of the small blind hole; The aperture of the large blind hole is larger than that of the small blind hole.
3. The dry electrode sheet according to claim 2, It is characterized in that The column spacing between large blind holes ranges from 90 microns to 110 microns, the row spacing between large blind holes ranges from 25 microns to 35 microns, the row spacing between small blind holes ranges from 15 microns to 25 microns, the column spacing between small blind holes and large blind holes ranges from 45 microns to 55 microns, the aperture size of large blind holes ranges from 50 microns to 80 microns, the aperture size of small blind holes ranges from 35 microns to 55 microns, the hole depth of large blind holes ranges from 70 microns to 110 microns, and the hole depth of small blind holes ranges from 45 microns to 85 microns.
4. The dry electrode sheet according to claim 1, It is characterized in that Both the large blind hole and the small blind hole are inverted tapered blind holes.
5. A method for preparing a dry electrode sheet according to any one of claims 1 to 4, It is characterized in that include: Step 1: dry-mixing the positive electrode active material or the negative electrode active material with the conductive agent and the binder to prepare a dry electrode sheet; Step 2: Use laser to punch holes on the surface of the dry electrode to obtain a punched dry electrode; Step 3: Use naphthalene lithium solution to wet the punched dry electrode sheet to obtain a dry electrode sheet.
6. The method for preparing a dry electrode sheet according to claim 5, It is characterized in that The naphthalene-lithium solution is prepared by dissolving lithium metal in liquid ammonia and then adding naphthalene.
7. A battery, It is characterized in that A dry electrode sheet comprising the dry electrode sheet as described in any one of claims 1 to 4, or a dry electrode sheet prepared by the preparation method of the dry electrode sheet as described in any one of claims 5 to 6.
Citation Information
Patent Citations
Electrode material, electrode active membrane and preparation method and application thereof
CN115832260A
Negative plate, battery as well as preparation method and application of negative plate
CN117832384A
Preparation method of multi-stage pre-lithiation composite negative pole piece and lithium ion battery
CN118352480A
Nonaqueous secondary battery
JP2012190625A
Rechargeable lithium ion battery with silicon anode
US20130136973A1