Tabs, batteries and power devices
By arranging multiple layers of foil on the battery tabs and performing specific welding treatments, the problem of poor foil welding quality is solved, welding quality and production efficiency are improved, and costs are reduced.
Patent Information
- Application Number
- CN202410970867.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The foil welding quality of existing battery tabs is poor, resulting in poor laser welding results and a high welding defect rate, which increases production costs.
By setting N layers of foil on the tabs, M welding marks are formed along the length of the tabs, and a 90° peeling force test is performed to control the area ratio of the welding marks within different intervals to ensure welding quality, including controlling the spacing of the welding marks. , overlapping areas and arc transition connections to ensure the stability and quality of welding.
It effectively improves the yield rate of tab welding, ensures the subsequent laser welding effect between the tab and pole, reduces production costs, and improves welding quality.
Smart Images

Figure CN118523049B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a tab, a battery and a power device. Background Art
[0002] The battery tabs are usually made of multiple layers of foil, which are then connected together by ultrasonic welding. The tabs are then welded to the battery poles by laser welding.
[0003] In the actual production process, the ultrasonic welding effect is poor and there will be gaps between the foils, which will affect the subsequent laser welding effect between the poles, resulting in explosion points in the laser welding, poor welding quality, and a high defective rate of the pole ear welding, resulting in battery scrapping and high production costs. Summary of the invention
[0004] In view of this, the present invention provides a tab, a battery and a power device to solve the problem of poor welding quality between the foil materials of the tab itself.
[0005] In a first aspect, the present invention provides a tab, the tab is located on an electrode assembly, the tab comprises N layers of foil material stacked, 20≤N≤200, the N layers of foil material are connected as a whole by welding, and M weld marks are formed along the length direction of the tab, M≥2; a 90° peeling force test is performed on the i-th layer of foil material of the tab, 1≤i≤N, and the total area of the M weld marks is S1, in units of mm 2 The remaining total area of M weld marks after the 90° peel force test is S2, in mm 2 , the test results must meet the following conditions at the same time:
[0006] In the range of 1≤i≤5, the result of 90° peeling force test for each foil layer is: 80%≤S2 / S1≤100%;
[0007] In the range of 6≤i≤N-5, the result of 90° peeling force test for any layer of foil is: 10%≤S2 / S1≤100%;
[0008] In the range of N-4≤i≤N, the result of 90° peeling force test for each layer of foil is: 80%≤S2 / S1≤100%.
[0009] Beneficial effect: The number of foil layers of the pole ear provided by the present invention is controlled within three intervals, 1≤i≤5 for the first five layers, N-4≤i≤N for the last five layers, and 6≤i≤N-5 for several intermediate layers. In different intervals, the ratio of the remaining total area S2 of the M weld marks after the 90° peeling force test to the total area S1 of the M weld marks is controlled within the above range, which can effectively improve the yield of the pole ear welding, ensure the subsequent laser welding effect between the pole ear and the pole, improve the welding quality, and reduce the production cost.
[0010] In an optional embodiment, the length of the pole ear is L, the unit is mm, the total length of the M weld marks is K, the unit is mm, the pole ear includes a first edge and a second edge located at both ends of the length direction thereof, the minimum distance between the weld mark close to the first edge and the first edge is B, the unit is mm, the minimum distance between the weld mark close to the second edge and the second edge is C, the unit is mm, the M weld marks are arranged at intervals, the spacing between adjacent weld marks is A, the unit is mm, satisfying: 4mm≤A≤30mm, wherein A= (LKB -C) / (M-1).
[0011] In an optional implementation, the minimum distance B between the weld mark close to the first edge and the first edge is in the range of: B ≥ 1.5 mm.
[0012] In an optional implementation, the minimum distance C between the weld mark close to the second edge and the second edge is in the range of: C ≥ 1.5 mm.
[0013] In an optional implementation, the length of each weld mark is D, expressed in mm, and then K=M×D.
[0014] In an optional implementation, there is an overlapping area between adjacent weld marks, and the length of the overlapping area is P, in mm, satisfying: 2mm≤P≤20mm.
[0015] In an optional embodiment, the total length of the M weld marks is K, in mm, the length of each weld mark is D, in mm, and the length of each overlapping area is P, then K=M×D-(M-1)×P.
[0016] In an optional embodiment, two adjacent edges of the weld mark are connected by an arc transition with a radius of R, 0.01 mm≤R≤10 mm.
[0017] In a second aspect, the present invention further provides a battery, comprising a shell, an electrode assembly and a pole ear of any one of the above technical solutions, the shell is provided with a cover assembly, and the shell and / or the cover assembly are provided with a pole; the electrode assembly is sealed in the shell by the cover assembly; one end of the pole ear is conductively connected to the electrode assembly, and the other end of the pole ear is conductively connected to the pole.
[0018] Beneficial effect: Because the battery includes a tab, it has the same effect as the tab, which will not be described in detail here.
[0019] In a third aspect, the present invention further provides a power device, comprising the battery in the above technical solution.
[0020] Beneficial effect: Since the power device includes a battery, it has the same effect as the battery and will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 A schematic diagram of the cross-sectional structure of a tab according to an embodiment of the present invention;
[0023] Figure 2 A schematic diagram of a structure in which welding and printing are arranged in an interval manner;
[0024] Figure 3 A schematic diagram of a structure in which welding and printing are arranged in an overlapping manner;
[0025] Figure 4 It is a schematic diagram of the structure of the remaining weld mark after the 90° peeling force test;
[0026] Figure 5 This is a schematic diagram of various parameters when the welding print is set in interval mode;
[0027] Figure 6 This is a schematic diagram of various parameters when the welding print is set in overlapping mode;
[0028] Figure 7 This is a schematic diagram of the welding structure.
[0029] Description of reference numerals:
[0030] 1. Tab; 2. Electrode assembly; 3. Foil; 4. Welding mark. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0032] Combine the following Figures 1 to 7 , describing an embodiment of the present invention.
[0033] According to an embodiment of the present invention, on the one hand, a tab 1 is provided, the tab 1 is located on an electrode assembly 2, the tab 1 comprises N layers of foil 3 stacked, 20≤N≤200, the N layers of foil 3 are connected as a whole by welding, and M weld marks 4 are formed along the length direction of the tab 1, M≥2; a 90° peeling force test is performed on the i-th layer of foil 3 of the tab 1, 1≤i≤N, and the total area of the M weld marks 4 is S1, in units of mm 2 The remaining total area of M weld marks 4 after the 90° peeling force test is S2, in mm 2 , the test results must meet the following conditions at the same time:
[0034] In the range of 1≤i≤5, the result of the 90° peeling force test for each layer of foil 3 is: 80%≤S2 / S1≤100%;
[0035] In the range of 6≤i≤N-5, the result of 90° peeling force test of any layer of foil 3 is: 10%≤S2 / S1≤100%;
[0036] In the range of N-4≤i≤N, the result of the 90° peeling force test of each layer of foil 3 is: 80%≤S2 / S1≤100%.
[0037] Specifically, the electrode assembly 2 includes a positive electrode sheet, a negative electrode sheet, and a separator between the positive electrode sheet and the negative electrode sheet.
[0038] exist Figure 1 , along the X direction are the 1st foil layer, the 2nd foil layer, the 3rd foil layer, the 4th foil layer, the 5th foil layer, the 6th foil layer ... the N-5th foil layer, the N-4th foil layer, the N-3rd foil layer, the N-2nd foil layer, the N-1st foil layer and the Nth foil layer.
[0039] Specifically, within the range of 1≤i≤5, each layer of foil 3 must be subjected to a 90° peel force test, and the value of S2 / S1 after the 90° peel force test of each layer of foil 3 must be within the range of 80% to 100%.
[0040] Similarly, within the range of N-4≤i≤N, each layer of foil 3 must be subjected to a 90° peel force test, and the value of S2 / S1 after the 90° peel force test of each layer of foil 3 must be within the range of 80% to 100%.
[0041] In the range of 6≤i≤N-5, S2 / S1 of any layer of foil 3 after 90° peeling force test should be in the range of 10% to 100%. Within this range, the test can be performed once or multiple times.
[0042] In the pole tab 1 provided in the embodiment of the present invention, the number of layers of the foil 3 is controlled within three intervals, 1≤i≤5 is the first five layers, N-4≤i≤N is the last five layers, and 6≤i≤N-5 is a number of intermediate layers. In different intervals, the ratio of the remaining total area S2 of the M weld marks 4 after the 90° peeling force test to the total area S1 of the M weld marks 4 is controlled within the above range, which can effectively improve the welding yield of the pole tab 1, ensure the subsequent laser welding effect between the pole tab 1 and the pole, improve the welding quality, and reduce the production cost.
[0043] In some embodiments, the length of the pole ear 1 is L, the unit is mm, the total length of the M weld marks 4 is K, the unit is mm, the pole ear 1 includes a first edge and a second edge located at both ends of its length direction, the minimum distance between the weld mark close to the first edge and the first edge is B, the unit is mm, the minimum distance between the weld mark close to the second edge and the second edge is C, the unit is mm, the M weld marks 4 are arranged at intervals, the spacing between adjacent weld marks 4 is A, the unit is mm, and it satisfies: 4mm≤A≤30mm, where A= (LKB -C) / (M-1).
[0044] By controlling the spacing A between adjacent weld marks 4 within the range of 4 mm to 30 mm, it can be ensured that the foil 3 will not crack after welding, and at the same time the length of the pole ear 1 can be controlled within a reasonable range, thereby controlling the weight of the pole piece, which is beneficial to the process welding.
[0045] It should be noted that the total length K of the M weld marks 4 refers to the sum of the lengths of the M weld marks 4 themselves, and does not include the gaps between adjacent weld marks 4. In some embodiments, the weld marks 4 are of equal length, and the length is D, in mm, then K=M×D. When the weld marks 4 are of unequal lengths, K is the sum of the lengths of the M weld marks 4.
[0046] In some embodiments, the minimum distance B between the weld mark close to the first edge of the tab 1 and the first edge of the tab 1 is in the range of B≥1.5 mm.
[0047] Since the shape of the pole lug 1 is not limited, B is the minimum distance between the weld mark 4 closest to the first edge of the pole lug 1 and the first edge of the pole lug 1 along the length direction of the pole lug 1. Since there are errors in the lamination process of the pole sheets, the edges of each layer of the pole lug 1 will not be on the same vertical plane, which is called the staggered layer of the pole lug. The weld mark 4 falling on the staggered layer of the pole lug 1 will reduce the life of the welding head, and in severe cases, the pole lug 1 will be torn. Therefore, by setting the minimum distance B between the first weld mark 4 and the first edge of the pole lug 1, and controlling B within a range of at least 1.5 mm, it can be ensured that the weld mark 4 avoids the staggered layer of the pole lug and improves the welding life.
[0048] In some embodiments, the minimum distance C between the weld mark close to the second edge and the second edge of the tab 1 is in the range of: C ≥ 1.5 mm.
[0049] Similarly, since the shape of the pole lug 1 is not limited, C is the minimum distance between the weld mark 4 closest to the second edge of the pole lug 1 and the second edge of the pole lug 1 along the length direction of the pole lug 1. Similarly, by setting C and controlling C within a range of at least 1.5 mm, it is possible to ensure that the weld mark 4 avoids the staggered layer of the pole lug and improve the welding life. For the two weld marks 4 located at both ends of the length direction of the pole lug 1, the minimum distance B between the first weld mark 4 and the first edge of the pole lug 1 and the minimum distance C between the last weld mark 4 and the second edge can be equal or different, depending on the specific situation.
[0050] In some embodiments, there is an overlapping area between adjacent weld marks 4, and the length of the overlapping area is P, in mm, satisfying: 2mm≤P≤20mm.
[0051] By controlling the length P of the overlapping area within the range of 2 mm ≤ P ≤ 20 mm, it can be ensured that the foil 3 in the overlapping area will not crack after welding, while ensuring a sufficient available laser welding area, which is beneficial to improving the current carrying capacity of the weld mark 4 .
[0052] In some embodiments, the total length of the M weld marks 4 is K, in mm, the length of each weld mark 4 is D, in mm, and the length of each overlapping area is P, then K=M×D- (M-1) ×P.
[0053] The M weld marks 4 are divided into two embodiments of equal length and unequal length. When there is an overlapping area between two adjacent weld marks 4 and the lengths of the overlapping areas are equal, the total length of the M weld marks 4 can be calculated using K=M×D- (M-1) ×P.
[0054] During the design process, the total length L of the tab 1 is first determined, and then the length D of the weld mark 4 and the number of weld marks 4 are determined as M. For multiple weld marks 4, it is finally determined whether the weld marks 4 are overlapped or spaced.
[0055] In some embodiments, when the total length L of the tab 1 is less than 100 mm, a scheme of overlapping arrangement between adjacent weld marks 4 is selected. When the total length L of the tab 1 is greater than or equal to 100 mm, according to actual conditions, a scheme of overlapping arrangement between weld marks 4 or a scheme of spacing arrangement between adjacent weld marks 4 can be selected.
[0056] In some embodiments, two adjacent edges of the weld mark 4 are connected by an arc transition with a radius of R, where 0.01 mm ≤ R ≤ 10 mm.
[0057] This arrangement allows the two adjacent sides of the weld mark 4 to transition smoothly, thereby preventing the edges of the weld mark 4 from tearing during ultrasonic welding.
[0058] Two sets of implementation cases are provided below, and the same loading speed is used to perform 90° peel force tests on the three sections where i is located. The test results are shown in Tables 1 and 2.
[0059] Table 1:
[0060]
[0061] Table 2:
[0062]
[0063] From Table 1 we can see that:
[0064] For implementation case 1, in the range of 1≤i≤5, S2 / S1 is less than 80%, in the range of 6≤i≤55, S2 / S1 is less than 10%, in the range of 56≤i≤60, S2 / S1≤80%, and after ultrasonic welding, the middle layer tab 1 is detached during the transfer process.
[0065] For implementation cases 2 and 3, within the range of 1≤i≤5, S2 / S1 is less than 80%, within the range of 6≤i≤55, S2 / S1 is less than 10%, within the range of 56≤i≤60, S2 / S1≤80%, and explosion spots appear in the laser welding between the pole ear 1 and the pole base, with a high defect rate.
[0066] From Table 2 we can see that:
[0067] For implementation case eleven, in the range of 1≤i≤5, S2 / S1 is less than 80%, in the range of 6≤i≤95, S2 / S1 is less than 10%, in the range of 96≤i≤100, S2 / S1≤80%, and after ultrasonic welding, the middle layer tab 1 is detached during the transfer process.
[0068] For Implementation Case 12 and Implementation Case 13, within the range of 1≤i≤5, S2 / S1 is less than 80%, within the range of 6≤i≤95, S2 / S1 is less than 10%, within the range of 96≤i≤100, S2 / S1≤80%, and explosion spots appear in the laser welding between the pole ear 1 and the pole base, and the defective rate is high.
[0069] For the remaining implementation cases in Table 1 and Table 2, the limited range of the 90° peeling force test was met, no abnormality occurred in the laser welding between the tab and the pole base, and the yield rate exceeded 99%.
[0070] The third implementation case is provided below, and different weld print 4 spacings A are tested. The test results are shown in Table 3.
[0071] Table 3:
[0072]
[0073] From Table 3 we can see that:
[0074] For Implementation Case 21, the spacing A between adjacent weld marks 4 is 2 mm, which is lower than the lower limit of A of 4 mm. The distance between two adjacent weld marks 4 is relatively close, and the foil 3 in the blank area between the weld marks 4 cracks after welding.
[0075] For implementation case 30, the spacing A between adjacent weld marks 4 is 32 mm, which is higher than the upper limit of A by 30 mm. No cracking occurs after welding. However, the distance between adjacent weld marks 4 is too large, and the foil 3 bulges between adjacent weld marks 4, which may easily cause damage to the tab 1. Therefore, it is not recommended for use.
[0076] For Implementation Case 24, C=1mm, which is less than the lower limit of C of 1.5mm, and the edge of the right ear is damaged.
[0077] For Implementation Case 25, B=1mm, which is less than the lower limit of B of 1.5mm, and the edge of the left ear is damaged.
[0078] In the other implementation cases, 4mm≤A≤30mm, B≥1.5mm, C≥1.5mm are satisfied, and no cracking or ear damage occurs after welding.
[0079] The fourth implementation case is provided below, and different weld overlap area lengths P are tested. The test results are shown in Table 4.
[0080] Table 4:
[0081]
[0082] From Table 4 we can see that:
[0083] For implementation case thirty-four, the length P of the overlapping area between adjacent weld marks 4 is 1 mm, which is lower than the lower limit of P of 2 mm. The length of the overlapping area of two adjacent weld marks 4 is small, and the foil 3 in the overlapping area cracks after welding.
[0084] For Implementation Case 43, the length P of the overlapping area between adjacent weld marks 4 is 24 mm, which is higher than the upper limit of P of 20 mm. No cracking occurs after welding. However, the length of the overlapping area between adjacent weld marks 4 is too large, and the usable laser welding area is reduced, which is not conducive to improving the current carrying capacity of the weld mark 4. It is not recommended for use.
[0085] For the remaining implementation cases, the length P of the overlapping area between adjacent weld marks 4 is in the range of 2 mm to 20 mm, and no cracking occurs after welding.
[0086] According to an embodiment of the present invention, in a second aspect, a battery is further provided, comprising a shell, an electrode assembly 2 and a pole lug 1 according to any one of the above embodiments, the shell being provided with a cover assembly, and the shell and / or the cover assembly being provided with a pole; the electrode assembly 2 is sealed in the shell by the cover assembly; one end of the pole lug 1 is conductively connected to the electrode assembly 2, and the other end of the pole lug 1 is conductively connected to the pole.
[0087] Because the battery includes the pole lug 1, it has the same effect as the pole lug 1 and is not described in detail here.
[0088] According to an embodiment of the present invention, in a third aspect, a power device is also provided, comprising the battery in the above embodiment.
[0089] Since the power device includes a battery and has the same effect as the battery, it will not be described in detail here.
[0090] Although the embodiments of the present invention have been described in conjunction with the accompanying drawings, those skilled in the art may make various modifications and variations without departing from the spirit and scope of the present invention, and such modifications and variations are all within the scope defined by the appended claims.
Claims
1. A tab, characterized in that: The tab is located on the electrode assembly, and the tab includes N layers of foil materials stacked together, 20≤N≤200, the N layers of foil materials are connected as a whole by welding, and M weld marks are formed along the length direction of the tab, M≥2; The 90° peeling force test is performed on the i-th foil of the tab, 1≤i≤N, and the total area of the M weld marks is S1, in mm 2 The remaining total area of the M weld marks after the 90° peeling force test is S2, in mm 2 , the test results must meet the following conditions at the same time: In the range of 1≤i≤5, the result of the 90° peeling force test of each layer of the foil is: 80%≤S2 / S1≤100%; In the range of 6≤i≤N-5, the result of 90° peeling force test of any layer of the foil is: 10%≤S2 / S1≤100%; In the range of N-4≤i≤N, the result of the 90° peeling force test on each layer of the foil is: 80%≤S2 / S1≤100%.
2. The tab according to claim 1, characterized in that: The length of the pole ear is L, in mm, the total length of the M weld marks is K, in mm, the pole ear includes a first edge and a second edge located at both ends of the length direction thereof, the minimum distance between the weld mark close to the first edge and the first edge is B, in mm, the minimum distance between the weld mark close to the second edge and the second edge is C, in mm, the M weld marks are arranged at intervals, the spacing between adjacent weld marks is A, in mm, satisfying: 4mm≤A≤30mm, wherein A=(LKB -C) / (M-1).
3. The tab according to claim 2, characterized in that: The range of the minimum distance B between the weld mark close to the first edge and the first edge is: B≥1.5mm.
4. The electrode tab according to claim 2 or 3, characterized in that: The range of the minimum distance C between the weld mark close to the second edge and the second edge is: C≥1.5mm.
5. The electrode tab according to claim 2 or 3, characterized in that: The length of each weld mark is D, in mm, then K=M×D.
6. The tab according to claim 1, characterized in that: There is an overlapping area between adjacent weld marks, and the length of the overlapping area is P, in mm, satisfying: 2mm≤P≤20mm.
7. The tab according to claim 6, characterized in that: The total length of the M weld marks is K, in mm, the length of each weld mark is D, in mm, and the length of each overlapping area is P, then K=M×D- (M-1) ×P.
8. The electrode tab according to any one of claims 1 to 3, characterized in that: Two adjacent edges of the weld mark are connected by an arc transition with a radius of R, 0.01mm≤R≤10mm.
9. A battery, characterized in that: include: A shell, wherein the shell is provided with a cover plate assembly, and the shell and / or the cover plate assembly is provided with a pole; an electrode assembly, wherein the electrode assembly is sealed in the housing by the cover plate assembly; The electrode tab according to any one of claims 1 to 8, wherein one end of the electrode tab is conductively connected to the electrode assembly, and the other end of the electrode tab is conductively connected to the electrode post.
10. A power device, characterized in that: A battery comprising the battery of claim 9.