A three-dimensional lithium-free negative electrode current collector, preparation method thereof and lithium metal battery

The three-dimensional lithium-free negative electrode current collector was prepared through electrochemical polarization to form a stable and uniform lithium-philic layer SEI film, which solved the problem of poor lithium dendrites generation and circulation performance, and significantly improved the circulation and safety performance of lithium metal batteries.

CN118547351BActive Publication Date: 2024-11-01WUHAN INSTITUTE OF MARINE ELECTRIC PROPULSION (THE 712TH RESEARCH INSTITUTE OF CHINA STATE SHIPBUILDING CORP LTD)
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411029746.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-01
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The lithium negative electrode current collector in existing lithium metal batteries is prone to produce lithium dendrites, and the circulation performance is poor. The three-dimensional metal current collector has problems such as poor lithium wetting and excessive electron flux, which leads to excessive polarization of the battery and deterioration of the cycle performance. .

Method used

The three-dimensional lithium-free negative electrode current collector is prepared by electrochemical polarization. By regulating the polarization voltage range, polarization current density and electrolyte components, a lithium-philic layer solid electrolyte dielectric film (SEI) with adjustable thickness is formed to uniformly Cover the current collector, inhibit the formation of lithium dendrites and improve circulation efficiency.

Benefits of technology

Effectively reduce the hysteresis voltage of lithium deposition, uniform lithium deposition, inhibit the generation of lithium dendrites, improve the circulation and safety performance of lithium metal batteries, and improve the energy density and cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118547351B_ABST
    Figure CN118547351B_ABST
Patent Text Reader

Abstract

The present invention discloses a three-dimensional lithium-free negative electrode current collector, a preparation method thereof and a lithium metal battery. The preparation method of the three-dimensional lithium-free negative electrode current collector comprises the following steps: a first lithium salt, a first organic solvent and a film-forming additive are prepared into a first electrolyte; the first electrolyte is used as an electrolyte, and a three-dimensional lithium-free negative electrode current collector is prepared by electrochemical polarization. The present invention adopts an electrochemical polarization method to modify a lithium-philic layer SEI with adjustable thickness on the three-dimensional current collector. The SEI film prepared by this method completely and evenly covers the three-dimensional current collector, and the thickness and components are controllable, and the method is simple. The three-dimensional lithium-free negative electrode current collector prepared by the present invention can effectively reduce the lithium deposition hysteresis voltage, uniform the lithium deposition process, inhibit the formation of lithium dendrites, and improve the cycle efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium metal batteries, and in particular relates to a three-dimensional lithium-free negative electrode current collector, a preparation method thereof and a lithium metal battery. Background Art

[0002] With the demand for long-lasting battery life in electronic products and electric vehicles, it is urgent to develop secondary battery systems with higher energy density. Lithium metal has an extremely high theoretical specific capacity (3860 mAh g -1 ), ultra-low electrode potential (-3.04 vs. SHE), and is considered to be the most promising high-energy-density lithium battery anode. However, in the development of lithium metal batteries, the positive electrode matched with excessive lithium metal anode will not only lead to a decrease in the specific energy of the entire battery, but also cause safety problems due to the continuous generation of lithium dendrites.

[0003] Negative electrode-free lithium battery is an effective way to solve the problem of excessive negative electrode lithium in the battery, in which the positive electrode provides the lithium source and the negative electrode is copper foil or other non-lithium-based current collector. However, the two-dimensional copper foil current collector inevitably has a tip effect, which causes uneven deposition of lithium and generates fluffy "dead lithium", causing the solid electrolyte interphase (SEI) on the surface of the deposited lithium to continuously generate / break, consuming the limited lithium source of the positive electrode, resulting in battery capacity decay and reduced cycle life. Stable three-dimensional metal current collectors with high specific surface area can effectively reduce local current density and provide a strong conductive network and pores for the deposited Li, thus avoiding the generation of "dead lithium" to a great extent.

[0004] However, three-dimensional metal current collectors also have disadvantages such as poor wettability with lithium and excessive electron flux at skeleton nodes, which leads to local deposition of lithium, excessive battery polarization, and deterioration of cycle performance. Summary of the invention

[0005] The purpose of the present invention is to overcome the above technical deficiencies, propose a three-dimensional lithium-free negative electrode current collector, a preparation method thereof and a lithium metal battery, and solve the technical problems in the prior art that the lithium-free negative electrode current collector is prone to produce lithium dendrites and has poor cycle performance.

[0006] In a first aspect, the present invention provides a method for preparing a three-dimensional lithium-free negative electrode current collector, comprising the following steps:

[0007] The first lithium salt, the first organic solvent and the film-forming additive are prepared into a first electrolyte;

[0008] The first electrolyte is used as the electrolyte, and a three-dimensional lithium-free negative electrode current collector is prepared by electrochemical polarization.

[0009] In a second aspect, the present invention provides a three-dimensional lithium-free negative electrode current collector, which is obtained by the preparation method of the three-dimensional lithium-free negative electrode current collector provided by the first aspect of the present invention.

[0010] In a third aspect, the present invention provides a lithium metal battery, which includes the three-dimensional lithium-free negative electrode current collector provided in the second aspect of the present invention.

[0011] Compared with the prior art, the beneficial effects of the present invention include:

[0012] The present invention uses electrochemical polarization to modify a lithium-philic layer SEI with adjustable thickness on a three-dimensional current collector. The SEI film prepared by this method completely and evenly covers the three-dimensional current collector, and the thickness and composition are controllable, and the method is simple. The three-dimensional lithium-free negative electrode current collector prepared by the present invention can effectively reduce the lithium deposition hysteresis voltage, uniform lithium deposition process, inhibit the generation of lithium dendrites, and improve the cycle efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a SEM image of the lithium deposition state on the three-dimensional negative electrode of a half-cell assembled from the three-dimensional lithium-free negative electrode current collector obtained in Example 2 at the 50th week of charge and discharge cycle;

[0014] Figure 2 This is a SEM image of the lithium deposition state on the three-dimensional negative electrode of the half-cell assembled from the three-dimensional lithium-free negative electrode current collector obtained in Example 5 at the 50th week of charge and discharge cycle;

[0015] Figure 3 This is a SEM image of the lithium deposition state on the three-dimensional negative electrode of a half-cell assembled from the three-dimensional lithium-free negative electrode current collector obtained in Comparative Example 1 at the 50th week of charge and discharge cycle;

[0016] Figure 4 It is a cycle performance curve diagram of a full battery assembled from the three-dimensional lithium-free negative electrode current collectors obtained in Example 2 and Comparative Example 1. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0018] In a first aspect, the present invention provides a method for preparing a three-dimensional lithium-free negative electrode current collector, comprising the following steps:

[0019] S1, preparing a first electrolyte by mixing a first lithium salt, a first organic solvent and a film-forming additive;

[0020] S2. Using the first electrolyte as the electrolyte, a three-dimensional lithium-free negative electrode current collector is prepared by electrochemical polarization.

[0021] This method uses electrochemical polarization to adjust the polarization voltage range, polarization current density and electrolyte composition to adjustably prepare a three-dimensional lithium-free negative electrode current collector with stable interface and uniform lithium deposition, solving the capacity attenuation and safety problems in the long-cycle cycle of lithium batteries, and is easy to operate on a large scale. The rich pore structure of the three-dimensional lithium-free negative electrode current collector can evenly accommodate a large amount of lithium, greatly improving the cycle performance and safety performance of lithium metal batteries while increasing the battery energy density.

[0022] In this embodiment, in step S1, the first lithium salt is at least one of lithium perchlorate, lithium tetrafluoroborate, lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium bis(fluoromethanesulfonyl)imide.

[0023] In this embodiment, in step S1, in the first electrolyte, the concentration of the first lithium salt is 0.2~1.2 mol / L, including but not limited to 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.1 mol / L, 1.2 mol / L, etc.

[0024] In this embodiment, in step S1, the first organic solvent is at least one of ethylene carbonate, dimethyl carbonate, vinylene carbonate, propylene carbonate, butylene carbonate, ethylene glycol dimethyl ether, 1,3-dioxolane, and diethylene glycol dimethyl ether.

[0025] In this embodiment, in step S1, the film-forming additive is at least one of lithium difluorooxalatoborate, lithium nitrate, fluoroethylene carbonate, and trifluoromethylethylene carbonate.

[0026] In this embodiment, in step S1, the mass fraction of the film-forming additive in the first electrolyte is 0.02%~0.1%, including but not limited to 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, and 0.1%.

[0027] In this embodiment, step S1 specifically includes: dissolving a first lithium salt in a first organic solvent, and then adding a film-forming additive and mixing them evenly to obtain a first electrolyte.

[0028] The mixture is dissolved and mixed evenly by stirring for 10 to 20 minutes.

[0029] In this embodiment, in step S2, during the electrochemical polarization process, a three-electrode system is used, the working electrode is a three-dimensional current collector, and the counter electrode and the reference electrode are both metallic lithium.

[0030] In some specific embodiments of the present invention, the working electrode is a three-dimensional mesh copper metal or a three-dimensional mesh nickel metal.

[0031] In some more specific embodiments of the present invention, the working electrode is a copper foam with a thickness of 0.2-0.75 mm.

[0032] In some more specific embodiments of the present invention, the three-dimensional mesh copper metal and the three-dimensional mesh nickel metal need to be washed alternately with 0.01-0.1 mol / L hydrochloric acid, acetone, and deionized water before use, and then vacuum dried at 50-60° C. for 2-6 hours.

[0033] In this embodiment, the electrochemical polarization adopts a constant current-constant potential polarization process. The present invention uses constant current polarization to reduce the components in the electrolyte in sequence, and the order of reduction is determined by the reduction potential of the components relative to lithium, and the components with higher reduction potential are reduced first; however, even under very small polarization current conditions, concentration polarization will exist, and concentration polarization may cause the actual polarization cutoff voltage to be slightly higher than the set cutoff voltage, thereby causing some electrolyte components to react incompletely, so a constant potential polarization process is subsequently added to eliminate concentration polarization and make the electrolyte components react more completely.

[0034] In some specific embodiments of the present invention, the polarization voltage range is from the open circuit voltage to 1.7V~0.6V, including but not limited to 1.7V, 1.5V, 1.3V, 1.1V, 0.9V, 0.7V, 0.6V, etc., and the current density is 0.005~0.1mA / cm 2 , including but not limited to 0.005mA / cm 2 , 0.01mA / cm 2 , 0.03mA / cm 2 , 0.05mA / cm 2 , 0.08mA / cm 2 , 0.1mA / cm 2 etc.; the constant potential polarization time is 1 to 30 min, including but not limited to 1 min, 5 min, 8 min, 10 min, 15 min, 20 min, 25 min, 30 min, etc.

[0035] In this implementation, step S2 specifically includes:

[0036] S21, assembling a working electrode, a counter electrode and a reference electrode into a three-electrode device, and then adding a first electrolyte;

[0037] S22. Place the three-electrode device on a charge and discharge cabinet and let it stand. By letting it stand, the present invention can, on the one hand, wet the electrodes, and on the other hand, eliminate concentration polarization caused by different local concentrations, thereby avoiding the problem of uneven film formation caused by uneven local polarization during the polarization process.

[0038] S23. Performing electrochemical polarization treatment on the working electrode in the three-electrode device to obtain a three-dimensional lithium-free negative electrode current collector.

[0039] Among them, the standing time is 10~30min, including but not limited to 10min, 15min, 20min, 25min, 30min, etc.

[0040] In this embodiment, the operation processes of steps S1 to S2 are all performed in a glove box filled with inert gas and having oxygen and water content less than 0.1 ppm.

[0041] In a second aspect, the present invention provides a three-dimensional lithium-free negative electrode current collector, which is obtained by the preparation method of the three-dimensional lithium-free negative electrode current collector provided by the first aspect of the present invention.

[0042] In a third aspect, the present invention provides a lithium metal battery, which includes the three-dimensional lithium-free negative electrode current collector provided in the second aspect of the present invention.

[0043] The three-dimensional lithium-free negative electrode current collector of the present invention is used as the negative electrode of a lithium metal battery. The rich pore structure can evenly accommodate a large amount of lithium, thereby greatly improving the cycle performance and safety performance of the lithium metal battery while increasing the battery energy density.

[0044] In this embodiment, the lithium metal battery comprises: a negative electrode, a positive electrode, a separator and a second electrolyte, wherein the negative electrode is a three-dimensional lithium-free negative electrode current collector or a three-dimensional lithium-free negative electrode current collector after pre-lithiation.

[0045] The present invention does not limit the types of the positive electrode, the separator and the second electrolyte, and those skilled in the art can make their selections according to actual conditions.

[0046] In some specific embodiments of the present invention, the material used for the positive electrode is one of lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, lithium nickel cobalt manganese oxide, sulfur or lithium metal.

[0047] In some specific embodiments of the present invention, the second electrolyte includes a second lithium salt and a second organic solvent. The second lithium salt is at least one of lithium perchlorate, lithium hexafluorophosphate, lithium bistrifluoromethanesulfonyl imide, and lithium bisfluoromethanesulfonyl imide; the second organic solvent is at least one of ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethylene glycol dimethyl ether, and 1,3 dioxolane. The second organic solvent is more specifically: ethylene carbonate and diethyl carbonate in a volume ratio of 1: (1~3), or dimethyl carbonate and ethylene carbonate in a volume ratio of 1: (3~4), or ethylene glycol dimethyl ether and 1,3 dioxolane in a volume ratio of 1: (0.3~3). In the second electrolyte, the concentration of the second lithium salt is 0.5~3 mol / L, including but not limited to 0.5mol / L, 1mol / L, 1.5mol / L, 2mol / L, 2.5mol / L, 3mol / L, etc.

[0048] In some specific embodiments of the present invention, the separator is one of a polypropylene (PP) separator, a polyethylene (PE) separator, and a polypropylene / polyethylene (PP / PE) separator.

[0049] Example 1

[0050] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the organic solvent is ethylene glycol dimethyl ether. The lithium salt is dissolved in the organic solvent and stirred for 10 minutes to obtain a uniformly mixed 0.5 mol / L electrolyte A. The film-forming additive is fluoroethylene carbonate, which is added to the electrolyte A described above and stirred for 10 minutes to obtain a uniform electrolyte B, wherein the mass fraction of the film-forming additive in electrolyte B is 0.05%. The foam copper (working electrode), metal lithium (counter electrode), and metal lithium (reference electrode) are assembled into a dried three-electrode device. Among them, the thickness of the foam copper is 0.3 mm, and the preliminary treatment is alternately washed with 0.05 mol / L hydrochloric acid, acetone, and deionized water, and vacuum dried at 50°C for 4 hours. Electrolyte B is added dropwise to the three-electrode device and the three-electrode device is assembled. The above-mentioned operation processes are all carried out in a glove box filled with inert gas with an oxygen and water content of less than 0.1 ppm. The three-electrode device is placed on the charge and discharge cabinet and left to stand for 20 minutes. From the open circuit voltage to 0.03mA / cm 2 The current density was polarized to 1.3 V and then switched to constant voltage for 8 min to obtain a three-dimensional lithium-free negative electrode current collector.

[0051] Example 2

[0052] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the organic solvent is ethylene glycol dimethyl ether. The lithium salt is dissolved in the organic solvent and stirred for 10 minutes to obtain a uniformly mixed 0.5 mol / L electrolyte A. The film-forming additive is fluoroethylene carbonate, which is added to the electrolyte A described above and stirred for 10 minutes to obtain a uniform electrolyte B, wherein the mass fraction of the film-forming additive in electrolyte B is 0.05%. The foam copper (working electrode), metal lithium (counter electrode), and metal lithium (reference electrode) are assembled into a dried three-electrode device. Among them, the thickness of the foam copper is 0.3 mm, and the preliminary treatment is alternately washed with 0.05 mol / L hydrochloric acid, acetone, and deionized water, and vacuum dried at 50°C for 4 hours. Electrolyte B is added dropwise to the three-electrode device and the three-electrode device is assembled. The above-mentioned operation processes are all carried out in a glove box filled with inert gas with an oxygen and water content of less than 0.1 ppm. The three-electrode device is placed on the charge and discharge cabinet and left to stand for 20 minutes. From the open circuit voltage to 0.03mA / cm 2 The current density was polarized to 1.0 V and then switched to constant voltage for 8 min to obtain a three-dimensional lithium-free negative electrode current collector.

[0053] Example 3

[0054] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the organic solvent is ethylene glycol dimethyl ether. The lithium salt is dissolved in the organic solvent and stirred for 10 minutes to obtain a uniformly mixed 0.5 mol / L electrolyte A. The film-forming additive is fluoroethylene carbonate, which is added to the electrolyte A described above and stirred for 10 minutes to obtain a uniform electrolyte B, wherein the mass fraction of the film-forming additive in electrolyte B is 0.05%. The foam copper (working electrode), metal lithium (counter electrode), and metal lithium (reference electrode) are assembled into a dried three-electrode device. Among them, the thickness of the foam copper is 0.3 mm, and the preliminary treatment is alternately washed with 0.05 mol / L hydrochloric acid, acetone, and deionized water, and vacuum dried at 50°C for 4 hours. Electrolyte B is added dropwise to the three-electrode device and the three-electrode device is assembled. The above-mentioned operation processes are all carried out in a glove box filled with inert gas with an oxygen and water content of less than 0.1 ppm. The three-electrode device is placed on the charge and discharge cabinet and left to stand for 20 minutes. From the open circuit voltage to 0.01mA / cm 2 The current density was polarized to 1.0 V and then switched to constant voltage for 8 min to obtain a three-dimensional lithium-free negative electrode current collector.

[0055] Example 4

[0056] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the organic solvent is ethylene glycol dimethyl ether. The lithium salt is dissolved in the organic solvent and stirred for 10 minutes to obtain a uniformly mixed 0.5 mol / L electrolyte A. The film-forming additive is fluoroethylene carbonate, which is added to the electrolyte A described above and stirred for 10 minutes to obtain a uniform electrolyte B, wherein the mass fraction of the film-forming additive in electrolyte B is 0.05%. The foam copper (working electrode), metal lithium (counter electrode), and metal lithium (reference electrode) are assembled into a dried three-electrode device. Among them, the thickness of the foam copper is 0.3 mm, and the preliminary treatment is alternately washed with 0.05 mol / L hydrochloric acid, acetone, and deionized water, and vacuum dried at 50°C for 4 hours. Electrolyte B is added dropwise to the three-electrode device and the three-electrode device is assembled. The above-mentioned operation processes are all carried out in a glove box filled with inert gas with an oxygen and water content of less than 0.1 ppm. The three-electrode device is placed on the charge and discharge cabinet and left to stand for 20 minutes. From the open circuit voltage at 0.05 mA / cm 2 The current density was polarized to 1.0 V and then switched to constant voltage for 8 min to obtain a three-dimensional lithium-free negative electrode current collector.

[0057] Example 5

[0058] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the organic solvent is ethylene glycol dimethyl ether. The lithium salt is dissolved in the organic solvent and stirred for 10 minutes to obtain a uniformly mixed 0.5 mol / L electrolyte A. The film-forming additive is lithium difluorooxalate borate, which is added to the electrolyte A described above and stirred for 10 minutes to obtain a uniform electrolyte B, wherein the mass fraction of the film-forming additive in electrolyte B is 0.05%. The foamed copper (working electrode), metal lithium (counter electrode), and metal lithium (reference electrode) are assembled into a dried three-electrode device. Among them, the thickness of the foamed copper is 0.3 mm, and the preliminary treatment is alternately washed with 0.05 mol / L hydrochloric acid, acetone, and deionized water, and vacuum dried at 50°C for 4 hours. Electrolyte B is added dropwise to the three-electrode device and the three-electrode device is assembled. The above-mentioned operation processes are all carried out in a glove box filled with inert gas with an oxygen and water content of less than 0.1 ppm. The three-electrode device is placed on the charge and discharge cabinet and left to stand for 20 minutes. From the open circuit voltage to 0.03mA / cm 2 The current density was polarized to 1.0 V and then switched to constant voltage for 8 min to obtain a three-dimensional lithium-free negative electrode current collector.

[0059] Comparative Example 1

[0060] A 0.3 mm thick copper foam was selected and washed alternately with 0.05 mol / L hydrochloric acid, acetone, and deionized water, and dried under vacuum at 50° C. for 4 h to obtain an untreated three-dimensional lithium-free negative electrode current collector.

[0061] Comparative Example 2

[0062] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the organic solvent is ethylene glycol dimethyl ether. The lithium salt is dissolved in the organic solvent and stirred for 10 minutes to obtain a uniformly mixed 0.5 mol / L electrolyte A. The film-forming additive is fluoroethylene carbonate, which is added to the electrolyte A described above and stirred for 10 minutes to obtain a uniform electrolyte B, wherein the mass fraction of the film-forming additive in the electrolyte B is 0.01%. The foam copper (working electrode), metal lithium (counter electrode), and metal lithium (reference electrode) are assembled into a dried three-electrode device. Among them, the thickness of the foam copper is 0.3 mm, and the preliminary treatment is alternately washed with 0.05 mol / L hydrochloric acid, acetone, and deionized water, and vacuum dried at 50°C for 4 hours. Electrolyte B is added dropwise to the three-electrode device and the three-electrode device is assembled. The above-mentioned operation processes are all carried out in a glove box filled with inert gas with an oxygen and water content of less than 0.1 ppm. The three-electrode device is placed on the charge and discharge cabinet and left to stand for 20 minutes. From the open circuit voltage to 0.03mA / cm 2 The current density was polarized to 1.0 V and then switched to constant voltage for 8 min to obtain a three-dimensional lithium-free negative electrode current collector.

[0063] Comparative Example 3

[0064] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the organic solvent is ethylene glycol dimethyl ether. The lithium salt is dissolved in the organic solvent and stirred for 10 minutes to obtain a uniformly mixed 0.5 mol / L electrolyte A. The film-forming additive is fluoroethylene carbonate, which is added to the electrolyte A described above and stirred for 10 minutes to obtain a uniform electrolyte B, wherein the mass fraction of the film-forming additive in electrolyte B is 0.25%. The foam copper (working electrode), metal lithium (counter electrode), and metal lithium (reference electrode) are assembled into a dried three-electrode device. Among them, the thickness of the foam copper is 0.3 mm, and the preliminary treatment is alternately washed with 0.05 mol / L hydrochloric acid, acetone, and deionized water, and vacuum dried at 50°C for 4 hours. Electrolyte B is added dropwise to the three-electrode device and the three-electrode device is assembled. The above-mentioned operation processes are all carried out in a glove box filled with inert gas with an oxygen and water content of less than 0.1 ppm. The three-electrode device is placed on the charge and discharge cabinet and left to stand for 20 minutes. From the open circuit voltage to 0.03mA / cm 2 The current density was polarized to 1.0 V and then switched to constant voltage for 8 min to obtain a three-dimensional lithium-free negative electrode current collector.

[0065] Comparative Example 4

[0066] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the organic solvent is ethylene glycol dimethyl ether. The lithium salt is dissolved in the organic solvent and stirred for 10 minutes to obtain a uniformly mixed 0.5 mol / L electrolyte A. The film-forming additive is fluoroethylene carbonate, which is added to the electrolyte A described above and stirred for 10 minutes to obtain a uniform electrolyte B, wherein the mass fraction of the film-forming additive in electrolyte B is 0.05%. The foam copper (working electrode), metal lithium (counter electrode), and metal lithium (reference electrode) are assembled into a dried three-electrode device. Among them, the thickness of the foam copper is 0.3 mm, and the preliminary treatment is alternately washed with 0.05 mol / L hydrochloric acid, acetone, and deionized water, and vacuum dried at 50°C for 4 hours. Electrolyte B is added dropwise to the three-electrode device and the three-electrode device is assembled. The above-mentioned operation processes are all carried out in a glove box filled with inert gas with an oxygen and water content of less than 0.1 ppm. The three-electrode device is placed on the charge and discharge cabinet and left to stand for 20 minutes. From the open circuit voltage to 0.03mA / cm 2 The current density was polarized to 1.9 V and then switched to constant voltage for 8 min to obtain a three-dimensional lithium-free negative electrode current collector.

[0067] Comparative Example 5

[0068] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the organic solvent is ethylene glycol dimethyl ether. The lithium salt is dissolved in the organic solvent and stirred for 10 minutes to obtain a uniformly mixed 0.5 mol / L electrolyte A. The film-forming additive is fluoroethylene carbonate, which is added to the electrolyte A described above and stirred for 10 minutes to obtain a uniform electrolyte B, wherein the mass fraction of the film-forming additive in electrolyte B is 0.05%. The foam copper (working electrode), metal lithium (counter electrode), and metal lithium (reference electrode) are assembled into a dried three-electrode device. Among them, the thickness of the foam copper is 0.3 mm, and the preliminary treatment is alternately washed with 0.05 mol / L hydrochloric acid, acetone, and deionized water, and vacuum dried at 50°C for 4 hours. Electrolyte B is added dropwise to the three-electrode device and the three-electrode device is assembled. The above-mentioned operation processes are all carried out in a glove box filled with inert gas with an oxygen and water content of less than 0.1 ppm. The three-electrode device is placed on the charge and discharge cabinet and left to stand for 20 minutes. From the open circuit voltage to 0.03mA / cm 2 The current density was polarized to 0.3 V and then switched to constant voltage for 8 min to obtain a three-dimensional lithium-free negative electrode current collector.

[0069] Comparative Example 6

[0070] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the organic solvent is ethylene glycol dimethyl ether. The lithium salt is dissolved in the organic solvent and stirred for 10 minutes to obtain a uniformly mixed 0.5 mol / L electrolyte A. The film-forming additive is fluoroethylene carbonate, which is added to the electrolyte A described above and stirred for 10 minutes to obtain a uniform electrolyte B, wherein the mass fraction of the film-forming additive in electrolyte B is 0.05%. The foam copper (working electrode), metal lithium (counter electrode), and metal lithium (reference electrode) are assembled into a dried three-electrode device. Among them, the thickness of the foam copper is 0.3 mm, and the preliminary treatment is alternately washed with 0.05 mol / L hydrochloric acid, acetone, and deionized water, and vacuum dried at 50°C for 4 hours. Electrolyte B is added dropwise to the three-electrode device and the three-electrode device is assembled. The above-mentioned operation processes are all carried out in a glove box filled with inert gas with an oxygen and water content of less than 0.1 ppm. The three-electrode device is placed on the charge and discharge cabinet and left to stand for 20 minutes. From the open circuit voltage to 0.003mA / cm 2 The current density was polarized to 1.0 V and then switched to constant voltage for 8 min to obtain a three-dimensional lithium-free negative electrode current collector.

[0071] Comparative Example 7

[0072] The lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the organic solvent is ethylene glycol dimethyl ether. The lithium salt is dissolved in the organic solvent and stirred for 10 minutes to obtain a uniformly mixed 0.5 mol / L electrolyte A. The film-forming additive is fluoroethylene carbonate, which is added to the electrolyte A described above and stirred for 10 minutes to obtain a uniform electrolyte B, wherein the mass fraction of the film-forming additive in electrolyte B is 0.05%. The foam copper (working electrode), metal lithium (counter electrode), and metal lithium (reference electrode) are assembled into a dried three-electrode device. Among them, the thickness of the foam copper is 0.3 mm, and the preliminary treatment is alternately washed with 0.05 mol / L hydrochloric acid, acetone, and deionized water, and vacuum dried at 50°C for 4 hours. Electrolyte B is added dropwise to the three-electrode device and the three-electrode device is assembled. The above-mentioned operation processes are all carried out in a glove box filled with inert gas with an oxygen and water content of less than 0.1 ppm. The three-electrode device is placed on the charge and discharge cabinet and left to stand for 20 minutes. From the open circuit voltage at 0.15 mA / cm 2 The current density was polarized to 1.0 V and then switched to constant voltage for 8 min to obtain a three-dimensional lithium-free negative electrode current collector.

[0073] Test Example 1

[0074] The three-dimensional lithium-free negative electrode current collectors prepared in Examples 1 to 5 and Comparative Examples 1 to 7 were assembled into a pair of batteries to test the polarization and hysteresis voltage within 50 cycles of lithium deposition / oxidation. 2The current density pre-deposition capacity is 2 mAh / cm 2 The same two electrodes after pre-lithiation were assembled into a pair of batteries. The lithium salt in the electrolyte was lithium bis(trifluoromethanesulfonyl)imide, and the solvent was ethylene glycol dimethyl ether and 1,3-dioxolane in a volume ratio of 1:1. The lithium salt concentration was 1 mol / L, and the battery separator was PP / PE. The current density of the battery cycle was 1 mA / cm 2 , the capacity of deposited / oxidized lithium is 1 mAh / cm 2 , the relevant test data results are shown in Table 1 below.

[0075] Table 1

[0076]

[0077] Test Example 2

[0078] The three-dimensional lithium-free negative electrode current collectors prepared in Example 2, Example 5 and Comparative Example 1 were assembled with lithium metal into a half-cell, and the lithium deposition state of the three-dimensional lithium-free negative electrode current collector at the 50th cycle was tested. The lithium salt in the circulating electrolyte was lithium bis(trifluoromethanesulfonyl)imide, and the solvent was ethylene glycol dimethyl ether and 1,3-dioxolane in a volume ratio of 1:1, where the lithium salt concentration was 1 mol / L, and the battery separator was PP / PE separator. The current density of the half-cell cycle was 1 mA / cm 2 , the lithium oxidation cut-off voltage on the working electrode is 0.8V. Related test data such as Figure 1 , Figure 2 and Figure 3 .

[0079] Test Example 3

[0080] The three-dimensional lithium-free negative electrode current collector prepared in Example 2 and Comparative Example 1 was assembled into a full battery to test the cycle performance. A lithium iron phosphate positive electrode was selected and a 0.5 mA / cm 2 The current density pre-deposition capacity is 2 mAh / cm 2 The lithium salt in the circulating electrolyte is lithium hexafluorophosphate, the solvent is ethylene carbonate and diethyl carbonate in a volume ratio of 1:1, the lithium salt concentration is 1 mol / L, the battery separator is PP / PE separator, and the cycle voltage range is 4.2V~2.75V. Related test data are as follows Figure 4 .

[0081] In the results of Test Example 1, the hysteresis voltage of Examples 1 to 5 in the first 50 cycles is much smaller than that of Comparative Example 1, indicating that the surface of the three-dimensional lithium-free negative electrode current collector prepared by the technical solution of the present invention does have a lithium affinity, and compared with the blank (Comparative Example 1), the hysteresis voltage during the cycle is reduced. Among them, by comparing Examples 1 to 2, it can be concluded that when the polarization cut-off voltage is 1.0V, a more stable artificial SEI film can be prepared on the three-dimensional lithium-free negative electrode current collector. The main reason is that when the polarization cut-off voltage is 1.3V, only the fluoroethylene carbonate component in the electrolyte is reduced, and when the cut-off voltage is 1.0V, the fluoroethylene carbonate in the electrolyte begins to be reduced first, and then another component in the electrolyte, lithium bistrifluoromethanesulfonyl imide, begins to be reduced. The reduction products of the two electrolyte components accumulate to form a multilayer regular SEI film containing rich lithium fluoride, lithium sulfide, lithium carbonate, lithium nitride and carbon fluoride, which is conducive to the uniform deposition behavior of lithium metal. Comparing Examples 2 to 4, it can be seen that the polarization current density affects the polarization behavior of the battery during the cycle, and the current density affects the thickness and density of the prepared artificial SEI film. Figure 1 and Figure 2 It can be seen that when the film-forming additive components are different, the performance of the prepared SEI film is also different. Figure 3 It can be seen that when the film-forming additive components are different, no dendrites are generated on the negative electrode surface during the battery cycle, and the interface stability is good, but the lithium deposition state is different, which is also related to the components of the SEI film. In Example 5, the reduction product of the electrolyte component lithium difluorooxalatoborate contains boron-containing oligomers, etc., and an SEI film with different components from Examples 1 to 4 is prepared.

[0082] In the results of Test Example 1, Example 2 is compared with Comparative Examples 2~3 and Comparative Examples 5~7. When the mass proportion of the additive is too low (Comparative Example 2) and the polarization current density is too large (Comparative Example 7), the SEI film on the surface of the three-dimensional lithium-free negative electrode current collector prepared is locally uneven. As the battery cycle proceeds, the SEI film continues to rupture / rebuild, resulting in a deterioration in the polarization degree of the battery. When the mass proportion of the additive is too high (Comparative Example 3), the polarization cut-off voltage is too low (Comparative Example 5), and the polarization current is too small (Comparative Example 6), the SEI film on the surface of the three-dimensional lithium-free negative electrode current collector prepared is too thick, which is not conducive to lithium ion transmission. When the cycle is 20 weeks, the voltage hysteresis is large. As the cycle proceeds, the battery polarization still tends to increase. Comparing Example 2 and Comparative Example 4, when the polarization cut-off voltage is 1.9V, the electrolyte B component does not begin to be reduced, and an effective SEI film is not obtained at this time, so the performance of the assembled battery is equivalent to that of Comparative Example 1.

[0083] It can be seen from the results of Test Example 3 that Example 2 shows better cycle performance than Comparative Example 1. Figure 1, indicating that the SEI film on the surface of the three-dimensional lithium-free negative electrode current collector prepared in Example 2 is conducive to the uniform deposition of lithium and has good stability, thereby ensuring the battery cycle stability.

[0084] In summary, the three-dimensional lithium-free negative electrode current collector of the present invention can induce uniform deposition of lithium metal, exhibits lower polarization during the cycle process, and has good interface stability, which greatly inhibits the formation of lithium dendrites. On the basis of improving the overall battery energy density, it improves the battery's cycle performance and safety performance.

[0085] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a three-dimensional lithium-free negative electrode current collector, It is characterized in that The following steps are involved: The first electrolyte is prepared by mixing a first lithium salt, a first organic solvent and a film-forming additive; The first electrolyte is used as the electrolyte, and a three-dimensional lithium-free negative electrode current collector is prepared by electrochemical polarization; wherein, The film-forming additive is at least one of lithium difluorooxalatoborate, lithium nitrate, fluoroethylene carbonate, and trifluoromethylethylene carbonate; the mass fraction of the film-forming additive is 0.02% to 0.1%; The electrochemical polarization adopts a constant current-constant potential polarization process; the polarization voltage range is from open circuit voltage to 0.6V~1.7V, and the current density is 0.005~0.1mA / cm 2 The constant potential polarization time is 1~30min.

2. The method for preparing the three-dimensional lithium-free negative electrode current collector according to claim 1, It is characterized in that The first lithium salt is at least one of lithium perchlorate, lithium tetrafluoroborate, lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium bis(fluoromethanesulfonyl)imide; the first organic solvent is at least one of ethylene carbonate, dimethyl carbonate, vinylene carbonate, propylene carbonate, butylene carbonate, ethylene glycol dimethyl ether, 1,3-dioxolane, and diethylene glycol dimethyl ether.

3. The method for preparing the three-dimensional lithium-free negative electrode current collector according to claim 1, It is characterized in that In the first electrolyte, the concentration of the first lithium salt is 0.2-1.2 mol / L.

4. The method for preparing the three-dimensional lithium-free negative electrode current collector according to claim 1, It is characterized in that During the electrochemical polarization process, a three-electrode system is used, the working electrode is a three-dimensional current collector, and the counter electrode and the reference electrode are both metallic lithium.

5. The method for preparing the three-dimensional lithium-free negative electrode current collector according to claim 4, It is characterized in that The working electrode is a three-dimensional mesh copper metal or a three-dimensional mesh nickel metal.

6. The method for preparing the three-dimensional lithium-free negative electrode current collector according to claim 1, It is characterized in that The polarization voltage range is from open circuit voltage to 1.0V~1.3V, and the current density is 0.01~0.05mA / cm 2 The constant potential polarization time is 8 minutes.

7. A three-dimensional lithium-free negative electrode current collector, It is characterized in that The three-dimensional lithium-free negative electrode current collector is obtained by the preparation method of the three-dimensional lithium-free negative electrode current collector according to any one of claims 1 to 6.

8. A lithium metal battery, It is characterized in that The lithium metal battery comprises the three-dimensional lithium-free negative electrode current collector according to claim 7.

9. The lithium metal battery according to claim 8, It is characterized in that include: A negative electrode, a positive electrode, a separator and a second electrolyte; wherein, The negative electrode is a three-dimensional lithium-free negative electrode current collector or a pre-lithiated three-dimensional lithium-free negative electrode current collector; The material used for the positive electrode is one of lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, lithium nickel cobalt manganese oxide or lithium metal; The second electrolyte includes a second lithium salt and a second organic solvent; the second lithium salt is at least one of lithium perchlorate, lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium bis(fluoromethanesulfonyl)imide; the second organic solvent is at least one of ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethylene glycol dimethyl ether, and 1,3-dioxolane; in the second electrolyte, the concentration of the second lithium salt is 0.5-3 mol / L; The diaphragm is one of a polypropylene diaphragm, a polyethylene diaphragm, and a polypropylene / polyethylene diaphragm.

Citation Information

Patent Citations

  • Lithium metal anode, fabrication method thereof, and lithium secondary battery comprising same anode

    CN110291666A

  • Metal lithium surface treatment process

    CN110350143A

  • Preparation method of negative electrode of ionic membrane coated metal lithium sheet capable of completely inhibiting lithium dendrites

    CN114068881A

  • Ultralow-temperature graphite-based lithium ion battery and preparation method of electrolyte of ultralow-temperature graphite-based lithium ion battery

    CN114552000A

  • Lithium metal negative electrode material as well as preparation method and application thereof

    CN116130632A