Friction stir welding method
By optimizing the welding path of the stirring head, the problem of welding defects in multi-joint interface welding was solved, and the welding connection effect, microstructure and mechanical properties of the weld were improved.
Patent Information
- Application Number
- CN202411049820.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-01
AI Technical Summary
In the process of friction stir welding with multiple joints, welding defects such as weak joints, cracks and hook-shaped defects are prone to occur, which affect the welding connection effect and product performance.
By optimizing the welding path of the stirring head, shifting it towards or away from the forward side of the butt joint interface to be welded, the material flow trend is changed, the stirring effect and stirring area are increased, and welding defects are reduced.
It effectively reduces welding defects, improves the connection effect between multiple splicing interfaces, and ensures the microstructure and mechanical properties of the weld.
Smart Images

Figure CN118595589B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of friction stir welding, in particular to a friction stir welding method. Background Art
[0002] With the continuous improvement and development of stir friction welding technology and its processes, and the characteristics of stir friction welding technology such as low forming temperature, small welding deformation and green environmental protection, stir friction welding has been widely used in aerospace, rail transportation, communication electronics and other fields.
[0003] In the context of various applications, the form of joints has also changed in a variety of ways, from single interface to double interface, triple interface or even more interfaces. The characteristic of friction stir welding technology is that a stirring head is used to stir and rub the material during the welding process, so that the welded material reaches a thermoplastic state.
[0004] Under the action of the stirring head, the material will migrate around the stirring needle of the stirring head. Therefore, during the welding process, the connection interface between the materials will also migrate under the rotation of the stirring head. However, there will often be a certain gap in the connection interface, and this gap will also migrate under the action of the stirring head.
[0005] In some application scenarios, due to the special structural design, the material is easy to form, and the O-state material is usually used as the base material for welding. After welding, the O-state material needs to reach a certain strength, and the post-weld material usually needs to be heat treated to strengthen it, such as T4 or T6 heat treatment. However, there is a difference in the thermal expansion coefficient of the material at the migration position and the thermal expansion coefficient of the surrounding material. The weak connection and crack defects caused by interface migration during welding will be larger in size before and after heat treatment due to the large tensile stress, which will reduce the performance of the product.
[0006] In the friction stir welding process of a single butt joint interface, the generation of a migration interface can be avoided by optimizing the welding process parameters. However, in the friction stir welding process of multiple joint interfaces, due to the complexity of the interface, the interface fluidity is limited, which easily leads to defective connections and poor welding connection effects. Summary of the invention
[0007] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, one object of the present invention is to provide a friction stir welding method for friction stir welding of multiple joint interfaces, which can reduce the generation of welding defects and improve the welding connection effect.
[0008] According to the friction stir welding method of an embodiment of the present invention, it is used for welding multiple connected splicing interfaces, at least one of the splicing interfaces is a butt interface to be welded, wherein the splicing interface located on one side of the butt interface to be welded is a secondary welding interface, and the friction stir welding method includes: controlling the welding path of the stirring head to offset toward the secondary welding interface to weld the secondary welding interface; or, the splicing interfaces located on both sides of the butt interface to be welded are secondary welding interfaces, and the friction stir welding method includes: controlling the welding path of the stirring head to offset relative to the butt interface to be welded at least toward the forward side of the butt interface to be welded, so as to weld the portion of the secondary welding interface located on the forward side.
[0009] According to the friction stir welding method of the embodiment of the present invention, by optimizing the welding path of the stirring head, the welding path of the stirring head is offset to the secondary welding interface or the forward side of the butt interface to be welded, thereby changing the flow trend of the material at the connection between the secondary welding interface and the butt interface to be welded, and increasing the stirring effect and stirring area of the stirring head on the material at the junction of the butt interface to be welded and the secondary welding interface, thereby facilitating reducing the occurrence of welding defects, improving the connection effect between multiple splicing interfaces, and further ensuring the microstructure and mechanical properties of the formed weld.
[0010] In some embodiments, the splicing interfaces located on both sides of the butt interface to be welded and coplanar are secondary welding interfaces, and the stir friction welding method includes: controlling the stirring head to offset toward the forward side and the backward side of the butt interface to be welded relative to the butt interface to be welded so as to weld the portion of the secondary welding interface located on the forward side and the portion of the secondary welding interface located on the backward side.
[0011] In some embodiments, the plurality of splicing interfaces include a plurality of butt interfaces, at least one of the butt interfaces is a butt interface to be welded, and at least one of the butt interfaces is connected to the butt interface to be welded and is a secondary welding interface; or, the plurality of splicing interfaces include butt interfaces and lap interfaces, at least one of the butt interfaces is an interface to be welded, and the secondary welding interface includes a lap interface, wherein the lap interface extends along a horizontal plane, and the butt interface extends along a vertical plane.
[0012] In some embodiments, the portion of the welding path of the stirring head that deviates from the butt interface to be welded forms a deviated path, and the deviated path includes an arc path, an annular path, or a connected combination of multiple ones of the arc path, the annular path and the straight path.
[0013] In some embodiments, the welding path of the stirring head includes a stable welding path and a deviation path, wherein the welding path of the stirring head is formed as a stable welding path along the portion of the butt interface to be welded, and the welding path of the stirring head deviates from the butt interface to be welded to form a deviation path, wherein the deviation path is an annular path, the annular path is located on one side of the stable welding path, and the starting end and the end of the annular path are respectively connected to the stable welding path; or, the deviation path includes an annular path and two arc paths, one end of the two arc paths is respectively connected to the starting end and the end of the annular path, and the other ends of the two arc paths are both connected to the stable welding path, the two arc paths and part of the annular path are located on one side of the stable welding path, and another part of the annular path is located on the other side of the stable welding path.
[0014] In some embodiments, the speed when moving along the butt interface to be welded is a first speed, and the speed when the stirring head moves away from the butt interface to be welded is a second speed, and the second speed is less than the first speed.
[0015] In some embodiments, the ratio of the second speed to the first speed is α, 0.2<α<1.
[0016] In some embodiments, the rotation speed of the stirring head when it moves along the butt interface to be welded is a first rotation speed, and the rotation speed of the stirring head when it moves away from the butt interface to be welded is a second rotation speed, and the second rotation speed is greater than the first rotation speed.
[0017] In some embodiments, the ratio of the second rotation speed to the first rotation speed is β, 1<β<3.
[0018] In some embodiments, the portion of the welding path of the stirring head that deviates from the butt interface to be welded forms a deviation path, and the deviation path is an annular path. The maximum distance that the deviation path deviates from the butt interface to be welded is 1 to 2 times the root diameter of the stirring needle of the stirring head.
[0019] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0021] Figure 1 A top view of a multi-jointed interface;
[0022] Figure 2 It is a side view of a multi-joint interface;
[0023] Figure 3 A schematic diagram of a welding path for a multi-joint interface;
[0024] Figure 4 A schematic diagram of another welding path for a multi-joint interface;
[0025] Figure 5 A schematic diagram of another welding path for a multi-joint interface;
[0026] Figure 6 It is a top view of another multi-joint interface;
[0027] Figure 7 It is a side view of another multi-joint interface;
[0028] Figure 8 A schematic diagram of a welding path for another multi-joint interface;
[0029] Fig. 9 A schematic diagram of another welding path for another multi-joint interface;
[0030] Fig.10 A schematic diagram of another welding path of another multi-joint interface;
[0031] Fig.11 A top view of another multi-joint interface;
[0032] Fig.12 A side view of yet another multi-joint interface;
[0033] Fig.13 A schematic diagram of a welding path for another multi-joint interface;
[0034] Fig.14 A schematic diagram of another welding path for a multi-joint interface;
[0035] Fig.15 A schematic diagram of yet another welding path for yet another multi-joint interface;
[0036] Fig.16 It is a top view of another multi-joint interface;
[0037] Fig.17 It is a side view of yet another multi-joint interface;
[0038] Fig.18 A schematic diagram of a welding path for another multi-joint interface;
[0039] Fig.19A schematic diagram of another welding path of yet another multi-joint interface;
[0040] Fig. 20 is a schematic diagram of yet another welding path for yet another multi-joint interface;
[0041] Fig.21 It is a top view of a multi-joint interface, wherein two welded parts are narrow frame parts;
[0042] Fig. 22 It is a side view of a multi-joint interface, wherein two welded parts are narrow frame parts;
[0043] Fig.23 A schematic diagram of a welding path of a multi-joint interface, wherein two welded parts are narrow frame parts;
[0044] Fig.24 is a schematic diagram of another welding path of a multi-joint interface, wherein two welded parts are narrow frame parts;
[0045] Fig.25 is a schematic diagram of another welding path of a multi-joint interface, wherein two welded parts are narrow frame parts;
[0046] Fig.26 for Fig.21 and Fig. 22 Electron microscope image of the weld formed by welding the splicing interface using the welding path before optimization;
[0047] Fig. 27 for Fig.21 and Fig. 22 SEM image of the weld formed by welding the splicing interface using the optimized welding path.
[0048] Reference numerals:
[0049] Splicing interface 10; butt-jointing interface 101; secondary welding interface 102;
[0050] Stirring head 20; Stirring needle 30;
[0051] Welding path 40;
[0052] Deviation path 401; stable welding path 402; arc path 403; circular path 404;
[0053] Narrow frame member 50; rigid constraint member 60; part to be welded 70. DETAILED DESCRIPTION
[0054] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by technicians in the technical field of the present invention; the terms used in the present invention and the specification of the invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention; the terms "including" and "having" and any variations thereof in the specification and claims of the present invention and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of the present invention or the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship.
[0056] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", and "attached" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0057] The term "and / or" in the present invention is only a description of the association relationship of the associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in the present invention generally indicates that the associated objects before and after are in an "or" relationship.
[0058] In the embodiments of the present invention, the same reference numerals represent the same components, and for the sake of brevity, detailed descriptions of the same components are omitted in different embodiments. It should be understood that the thickness, length, width and other dimensions of various components in the embodiments of the present invention shown in the drawings, as well as the overall thickness, length, width and other dimensions of the integrated device are only exemplary and should not constitute any limitation to the present invention.
[0059] The term “plurality” used in the present invention refers to two or more (including two).
[0060] Combine the following Figures 1 to 27 The friction stir welding method of the present invention will be described.
[0061] The friction stir welding method according to the embodiment of the present invention is used for welding a plurality of connected joint interfaces 10, at least one of which is a butt joint interface 101 to be welded.
[0062] The joint interface 10 located on one side of the butt interface 101 to be welded is a secondary welding interface 102 . The friction stir welding method includes: controlling the welding path 40 of the stirring head 20 to deviate toward the secondary welding interface 102 to weld the secondary welding interface 102 .
[0063] Alternatively, the splicing interfaces 10 located on both sides of the butt interface 101 to be welded are secondary welding interfaces 102, and the stir friction welding method includes: controlling the welding path 40 of the stirring head 20 to be offset relative to the butt interface 101 to be welded at least toward the forward side of the butt interface 101 to be welded, so as to weld the part of the secondary welding interface 102 located on the forward side.
[0064] The multiple splicing interfaces 10 are connected, which means that there is an edge overlap between the multiple splicing interfaces 10. At least one splicing interface 10 is a butt interface 101 to be welded, that is, only one splicing interface 10 among the multiple splicing interfaces 10 can be a butt interface 101 to be welded, or there can be multiple splicing interfaces 10 to be welded. When the stirring head 20 welds the multiple splicing interfaces 10 along the welding path 40, at least part of the welding path 40 is along the butt interface 101 to be welded, so as to form a weld at the splicing interface 10.
[0065] Taking the butt interface 101 to be welded as the boundary, the two sides of the butt interface 101 to be welded are respectively the forward side and the backward side. When the stirring head 20 is located at the butt interface 101 to be welded, on the forward side, the rotation direction of the stirring head 20 is consistent with the forward direction of the stirring head 20, and on the backward side, the rotation direction of the stirring head 20 is opposite to the forward direction of the stirring head 20.
[0066] Specifically, the multiple splicing interfaces 10 may include multiple butt interfaces, at least one butt interface is a butt interface 101 to be welded, and at least one butt interface is connected to the butt interface 101 to be welded and is a secondary welding interface 102; or, the multiple splicing interfaces 10 include butt interfaces and overlapping interfaces, at least one butt interface is an interface to be welded, and the secondary welding interface 102 includes an overlapping interface, wherein the overlapping interface extends along a horizontal plane and the butt interface extends along a vertical plane.
[0067] In the related art, when multiple splicing interfaces are overlapping interfaces and butt interfaces, during the welding process, due to the stirring action of the stirring head, the material at the overlapping interface will migrate upward along the axial direction of the stirring head under the stirring and extrusion action of the stirring head, forming a hook-shaped defect. The occurrence of this defect will reduce the effective plate thickness of the material around the weld. Usually, the hook-shaped defect is formed on the forward side of the weld; at the same time, the effective connection width of the overlapping interface is small, forming a cold overlapping defect.
[0068] When multiple joint interfaces are three-joint joint interfaces and multiple-joint joint interfaces, under the action of the stirring head during welding, in the horizontal direction, the secondary welding interface will migrate along the rotation direction of the stirring head, forming weak connection defects such as cracks inside the weld. In the direction of the stirring needle axis, the material flows along the side of the stirring needle, and the material near the overlapping interface will flow upward or downward, forming weak connection or hook-shaped defects.
[0069] In the present invention, the joint interface 10 located on one side of the butt interface 101 to be welded is a secondary welding interface 102 , and the friction stir welding method includes: controlling the welding path 40 of the stirring head 20 to deviate toward the secondary welding interface 102 to weld the secondary welding interface 102 .
[0070] It should be noted that if only one side of the butt interface 101 to be welded (here, one side of the butt interface 101 to be welded refers to the side of the same position of the butt interface 101 to be welded) is provided with a secondary welding interface 102, then the welding path 40 of the stirring head 20 is controlled to be offset toward the secondary welding interface 102, so as to increase the volume of the material stirred by the stirring needle 30 of the stirring head 20 at the junction of the butt interface 101 to be welded and the secondary welding interface 102. Compared with the welding effect of a straight weld, after the welding path 40 of the stirring head 20 is offset, the material at the junction of the butt interface 101 to be welded and the secondary welding interface 102 is stirred more violently and the stirring area is larger, which is beneficial to increase the effective connection width of the secondary welding interface 102, thereby reducing weak connections and cold lap defects at the junction.
[0071] In the present invention, the splicing interfaces 10 located on both sides of the butt interface 101 to be welded and coplanar are secondary welding interfaces 102, and the splicing interfaces 10 located on both sides of the butt interface 101 to be welded refer to the two sides of the same position of the butt interface 101 to be welded, and the edges of the splicing interfaces 10 located on both sides of the butt interface 101 to be welded overlap with the edges of the butt interface 101 to be welded, and the splicing interfaces 10 located on both sides of the butt interface 101 to be welded may be coplanar or non-coplanar.
[0072] The friction stir welding method includes: controlling the welding path 40 of the stirring head 20 to be offset relative to the butt interface 101 to be welded at least toward the forward side of the butt interface 101 to be welded, so as to weld the portion of the secondary welding interface 102 located on the forward side. Since the hook-shaped defect is usually formed on the forward side of the weld, the welding path 40 of the stirring head 20 is offset toward the forward side of the butt interface 101 to be welded, so that it is beneficial to eliminate the hook-shaped defect by increasing the number of stirring times of the material located on the forward side of the butt interface 101 to be welded or changing the stirring direction of the material multiple times, and at the same time, it can also increase the volume of the material stirred by the stirring needle 30 of the stirring head 20 at the junction of the butt interface 101 to be welded and the secondary welding interface 102. Compared with the welding effect of the straight weld, after the welding path 40 of the stirring head 20 is offset, the material stirring at the junction of the butt interface 101 to be welded and the secondary welding interface 102 is more intense, and the stirring area is larger, which is beneficial to increase the effective connection width of the secondary welding interface 102, thereby reducing the weak connection and cold lap defects at the junction.
[0073] According to the friction stir welding method of the embodiment of the present invention, by optimizing the welding path 40 of the stirring head 20, the welding path 40 of the stirring head 20 is offset toward the secondary welding interface 102 or the forward side of the butt interface 101 to be welded, thereby changing the flow trend of the material at the connection between the secondary welding interface 102 and the butt interface 101 to be welded, and increasing the stirring effect and stirring area of the stirring head 20 on the material at the junction of the butt interface 101 to be welded and the secondary welding interface 102, thereby facilitating reducing the generation of welding defects, improving the connection effect between multiple splicing interfaces 10, and further ensuring the microstructure and mechanical properties of the formed weld.
[0074] According to some embodiments of the present invention, reference may be made to Figure 3 , Figure 8 , Fig.13 , Fig.18 , Fig.23 As shown, the joint interfaces 10 located on both sides of the butt interface 101 to be welded and coplanar are secondary welding interfaces 102, and the friction stir welding method includes: controlling the stirring head 20 to offset toward the forward side and the backward side of the butt interface 101 to be welded relative to the butt interface 101 to be welded so as to weld the portion of the secondary welding interface 102 located on the forward side and the portion of the secondary welding interface 102 located on the backward side.
[0075] Here, the friction stir welding method may include first controlling the stirring head 20 to offset toward the forward side of the butt interface 10 to be welded relative to the butt interface 10 to be welded, and then controlling the stirring head 20 to offset toward the backward side of the stirring head 20 relative to the butt interface 101 to be welded; or, it may include first controlling the stirring head 20 to offset toward the backward side of the stirring head 20 relative to the butt interface 101 to be welded, and then controlling the stirring head 20 to offset toward the forward side of the stirring head 20 relative to the butt interface 10 to be welded; or, it may also include controlling the stirring head 20 to offset back and forth between the forward side and the backward side of the butt interface 101 to be welded.
[0076] The stirring head 20 is controlled to be offset toward the forward side and the backward side of the butt interface 101 to be welded, so that the stirring head 20 can stir and weld the part of the secondary welding interface 102 located on the forward side, and can also weld the part of the secondary welding interface 102 located on the backward side. In this way, the volume of the material stirred by the stirring needle 30 of the stirring head 20 at the connection between the secondary welding interface 102 and the butt interface 101 to be welded can be further increased, which is beneficial to increase the effective connection width of the secondary welding interface 102, and is also beneficial to eliminate hook defects and improve the connection effect between multiple splicing interfaces 10.
[0077] For example, reference may be made to Figures 1 to 5 As shown, multiple splicing interfaces 10 include a first docking interface and a first overlapping interface, the first overlapping interface is located on one side of the first docking interface in the horizontal direction, the docking interface 101 to be welded is the first docking interface, the first overlapping interface is the secondary welding interface 102, the tip of the stirring needle 30 of the stirring head 20 is located on the lower side of the first overlapping interface, and the stir friction welding method includes controlling the welding path 40 of the stirring head 20 to deviate from the first docking interface at least partially toward the first overlapping interface.
[0078] For example, reference may be made to Figures 6 to 10 As shown, multiple splicing interfaces 10 include a second overlapping interface, a second overlapping interface and a third overlapping interface, the second overlapping interface and the third overlapping interface are coplanar, the secondary welding interface 102 includes a second overlapping interface and a third overlapping interface, the second overlapping interface is located on the upper side of the second overlapping interface and the third overlapping interface, the butt interface 101 to be welded is the second overlapping interface, the tip of the stirring needle 30 of the stirring head 20 is located on the lower side of the second overlapping interface and the third overlapping interface, and the stir friction welding method includes controlling the welding path 40 of the stirring head 20 to deviate from the second overlapping interface at least partially toward the second overlapping interface and / or at least partially deviate from the second overlapping interface toward the third overlapping interface.
[0079] For example, reference may be made to Figures 11 to 15As shown, multiple splicing interfaces 10 include a third docking interface, a fourth docking interface and a fifth docking interface, the fifth docking interface is located on one side of the third docking interface and the fourth docking interface in the horizontal direction, the third docking interface and the fourth docking interface are coplanar and are the docking interface 101 to be welded, and the stir friction welding method includes controlling the welding path 40 of the stirring head 20 to deviate at least partially from the docking interface 101 to be welded toward the fifth docking interface.
[0080] For example, reference may be made to Figures 16 to 20 As shown, multiple splicing interfaces 10 include a fourth overlapping interface, a fifth overlapping interface and a sixth overlapping interface, the fourth overlapping interface and the fifth overlapping interface are coplanar and are secondary welding interfaces 102, the sixth overlapping interface is located below the fourth overlapping interface and the fifth overlapping interface, the sixth overlapping interface is a butt interface to be welded 101, the tip of the stirring needle 30 of the stirring head 20 is located on the lower side of the fourth overlapping interface and the fifth overlapping interface, and the stir friction welding method includes controlling the welding path 40 of the stirring head 20 to deviate at least partially from the sixth overlapping interface toward the fourth overlapping interface and / or at least partially from the sixth overlapping interface toward the fifth overlapping interface.
[0081] According to some embodiments of the present invention, the portion of the welding path 40 of the stirring head 20 that deviates from the butt interface 101 to be welded is formed as a deviated path 401, and the portion of the welding path 40 of the stirring head 20 that is along the butt interface 101 to be welded is formed as a stable welding path 402. Figure 5 , Fig.10 , Fig.15 , Fig. 20 and Fig.25 As shown, the deviation path 401 can be an arc path 403 to increase the volume of the material stirred by the stirring needle 30 of the stirring head 20 at the portion where the secondary welding interface 102 connects with the butt interface 101 to be welded, thereby facilitating increasing the effective welding connection width of the secondary welding interface 102.
[0082] According to some embodiments of the present invention, the deviation path 401 may be an annular path 404, the starting end and the end of the annular path 404 coincide with each other, and the starting end and the end of the annular path 404 are both connected to the stable welding path 402. The annular path 404 may be a circular annular path, a rectangular path, or a rounded rectangular path. Figure 4 , Fig. 9 , Fig.14 , Fig.19 , Fig.24 As shown, the annular path 404 is a rounded rectangular path. The annular path 404 is located on one side of the stable welding path 402 and the starting end and the end of the annular path 404 are respectively connected to the stable welding path 402 .
[0083] In some embodiments, the deviation path 401 may be a combination of multiple types of arc path 403, circular path 404, and straight path. Figure 3 , Figure 8 , Fig.13 , Fig.18 , Fig.23 As shown, the deviation path 401 includes a circular path 404 and two arc paths 403, one end of the two arc paths 403 are respectively connected to the starting end and the end of the circular path 404, and the other ends of the two arc paths 403 are connected to the stable welding path 402, the two arc paths 403 and part of the circular path 404 are located on one side of the stable welding path 402, and the other part of the circular path 404 is located on the other side of the stable welding path 402.
[0084] In an embodiment of the present invention, the deviated path 401 includes an annular path 404, or a combination of multiple connected arc paths 403, annular paths 404 and straight paths. In this way, the material of the portion where the secondary welding interface 102 is connected to the butt interface 101 to be welded is stirred multiple times during the movement of the stirring head 20 along the deviated path 401, and the multiple stirring directions are the same or different.
[0085] You can refer to Fig.14 As shown, the rotation direction of the stirring needle 30 of the stirring head 20 is clockwise, and the moving direction of the stirring needle 30 when moving along the butt interface 101 to be welded is from top to bottom in the figure. Since when the stirring head 20 moves along the annular path 404, the moving direction of the stirring head 20 when it moves in the part where the annular path 404 overlaps with the stable welding path 402 is opposite to the moving direction when it moves in the part of the annular path 404 away from the stable welding path 402. Therefore, the stirring direction of the stirring head 20 for the material at the secondary welding interface 102 located in the annular path 404 is also opposite, that is, the material flow direction is also opposite. For example, the material first rotates along a first direction to form a hook-shaped defect, and then the material rotates along a second direction, the first direction and the second direction are opposite. At this time, the material of the hook-shaped defect part can be re-screwed into the interior of the workpiece 70 to be welded, which is beneficial to eliminate the hook-shaped defect.
[0086] At the same time, the material can also flow in the same direction for multiple times, thereby increasing the degree of stirring at the junction of the secondary welding interface 102 and the butt interface 101 to be welded, and increasing the effective connection width of the secondary welding interface 102; and the cracks formed by the migration of the secondary welding interface 102 during the first stirring can also be broken under the multiple stirring actions of the stirring head 20, thereby increasing the degree of material mixing at the junction of the butt interface 101 to be welded and the secondary welding interface 102, thereby improving the microstructure and mechanical properties of the weld area.
[0087] This application is for Figure 21 to Figure 25As shown, a welding test is conducted on a plurality of joint interfaces 10 formed by a plurality of welded parts 70, one of which is a narrow frame part 50 and is surrounded by a rigid constraint part 60. The narrow frame part 50 is defined as a narrow frame part 50 whose width is smaller than the shoulder radius of the stirring head 20. When welding the narrow frame part 50, the quality of the weld is particularly critical because the narrow frame part 50 itself is thin and the stress is weak.
[0088] Fig.26 for Fig.21 and Fig. 22 Electron microscope image of the weld formed by welding the splicing interface using the welding path before optimization; Fig. 27 for Fig.21 and Fig. 22 SEM image of the weld formed by welding the splicing interface using the optimized welding path. Fig.26 When the welding path is not optimized, the distance between the end D1 of the secondary welding interface 102 away from the butt interface 101 to be welded and the end D2 of the crack formed by the migration of the secondary welding interface 102 away from the butt interface 101 to be welded is 3134 microns. Fig. 27 The figure shows that after the welding path is optimized, the distance between the end D3 of the secondary welding interface 102 away from the butt interface 101 to be welded and the end D4 of the crack formed by the migration of the secondary welding interface 102 away from the butt interface 101 to be welded is 940 microns. Fig. 27 It can be seen that the secondary welding interface 102 hardly migrates. Fig.26 and Fig. 27 It can be seen that the interface migration problem has been significantly improved through the optimization of the welding path.
[0089] According to some embodiments of the present invention, the speed of moving along the butt interface 101 to be welded is a first speed, and the speed of the stirring head 20 moving away from the butt interface 101 to be welded is a second speed, and the second speed is less than the first speed.
[0090] The welding path 40 of the stirring head 20 includes a stable welding path 402 and a deviated path 401. The welding path 40 of the stirring head 20 is formed as a stable welding path 402 along the butt interface 101 to be welded, and the welding path 40 of the stirring head 20 deviates from the butt interface 101 to be welded to form a deviated path 401. That is to say, the speed of the stirring head 20 when moving along the deviated path 401 is slow, which can increase the number of stirring times of the material at the junction of the butt interface 101 to be welded and the secondary welding interface 102, so that the material stirring at this location is more intense, which is beneficial to increase the uniformity of the material at this location, thereby improving the welding connection effect, reducing the generation of defects, and further ensuring the microstructure and mechanical properties of the weld.
[0091] According to some embodiments of the present invention, the ratio of the second speed to the first speed is α, 0.2<α<1. For example, the ratio of the second speed to the first speed is 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or any value between any adjacent values therein, etc.
[0092] The ratio of the second speed to the first speed is within this range. On the one hand, the second speed will not be too small, and will not increase the welding time too much, or cause plastic deformation of the material around the junction of the butt interface 101 to be welded and the secondary welding interface 102; on the other hand, the number of stirring times for the material at the junction of the butt interface 101 to be welded and the secondary welding interface 102 can be increased, so that the material at the junction is stirred more violently, which is beneficial to increase the uniformity of the material at the junction, thereby improving the welding connection effect, reducing the generation of defects, and further ensuring the microstructure and mechanical properties of the weld.
[0093] According to some embodiments of the present invention, the rotation speed of the stirring head 20 when moving along the butt interface 101 to be welded is a first rotation speed, and the rotation speed of the stirring head 20 when moving away from the butt interface 101 to be welded is a second rotation speed, and the second rotation speed is greater than the first rotation speed.
[0094] The welding path 40 of the stirring head 20 includes a stable welding path 402 and a deviated path 401. The welding path 40 of the stirring head 20 is formed as a stable welding path 402 along the butt interface 101 to be welded, and the welding path 40 of the stirring head 20 is formed as a deviated path 401 when it deviates from the butt interface 101 to be welded. That is to say, the stirring head 20 has a faster rotation speed when moving along the deviated path 401, which can increase the number of stirring times of the material at the junction of the butt interface 101 to be welded and the secondary welding interface 102, making the material stirring at this location more intense, which is beneficial to increase the uniformity of the material at this location, thereby improving the welding connection effect between multiple splicing interfaces 10, reducing the generation of defects, and thus ensuring the microstructure and mechanical properties of the weld.
[0095] According to some embodiments of the present invention, a ratio of the second rotation speed to the first rotation speed is β, 1<β<3.
[0096] For example, the ratio of the second rotation speed to the first rotation speed may be 1.2, 1.4, 1.6, 1.8, 2.0, 2.2, 2.4, 2.6, 2.8 or any value between any two values therein, and the like.
[0097] The ratio of the second rotation speed to the first rotation speed is within this range. On the one hand, the second rotation speed will not be too large to increase the cost of the stirring head 20. At the same time, the possibility of plastic deformation of the material around the junction of the butt interface 101 to be welded and the secondary welding interface 102 caused by the excessively fast rotation speed of the stirring head 20 can be reduced. On the other hand, the number of stirring times of the material at the junction of the butt interface 101 to be welded and the secondary welding interface 102 can be increased, so that the material at this location is stirred more violently, which is beneficial to increase the uniformity of the material at this location.
[0098] According to some embodiments of the present invention, the portion of the welding path 40 of the stirring head 20 that deviates from the butt interface 101 to be welded is formed as a deviated path 401, the deviated path 401 is an annular path 404, and the maximum distance L of the deviated path 401 from the butt interface 101 to be welded is 1 to 2 times the root diameter of the stirring needle 30. In other words, the maximum distance between the deviated path 401 and the butt interface 101 to be welded in a direction perpendicular to the butt interface 101 to be welded is 1 to 2 times the root diameter of the stirring needle 30 of the stirring head 20.
[0099] For example, the maximum distance L of the center of the stirring head 20 from the butt interface 101 to be welded can be 1 times, 1.2 times, 1.4 times, 1.6 times, 1.8 times, 2 times the root diameter of the stirring needle 30 or any value between any two of these values.
[0100] The maximum distance L of the center of the stirring head 20 deviating from the butt interface 101 to be welded is not less than the root diameter of the stirring needle 30. In this way, along the direction of the secondary welding interface 102, the stirring needle 30 can completely deviate from the position of the stirring needle 30 at the butt interface 101 to be welded, so that the partial material connected to the butt interface 101 to be welded by the secondary welding interface 102 can be stirred multiple times and the stirring direction is opposite, which is beneficial to the partial splicing interface 10 after the migration of the fragments, and increases the mixing degree of the splicing interface 10 and the surrounding materials, thereby improving the microstructure and mechanical properties of the weld area and reducing the generation of hook defects. The maximum distance L of the center of the stirring head 20 deviating from the butt interface 101 to be welded is not greater than twice the root diameter of the stirring needle 30. In this way, the distance of the stirring head 20 offset from the butt interface 101 to be welded will not be too far to increase the length of the welding path 40 too much, thereby reducing the welding production efficiency.
[0101] In some embodiments, when the deviation path 401 is an arc path 403 , the maximum distance L of the center of the stirring head 20 deviating from the butt interface 101 to be welded does not exceed the radius of the root of the stirring needle 30 to reduce the impact on the effective welding width of the butt interface 101 to be welded.
[0102] The friction stir welding method of the embodiment of the present invention can be used for connecting the same or different metal materials, and the metal materials include aluminum, magnesium, copper, titanium and alloy materials thereof.
[0103] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0104] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.
Claims
1. A friction stir welding method, characterized in that: Used for welding multiple connected splicing interfaces, at least one of the splicing interfaces is a butt interface to be welded, wherein: The splicing interface located on one side of the butt interface to be welded is a secondary welding interface, and the friction stir welding method comprises: controlling the welding path of the stirring head to deviate toward the secondary welding interface to weld the secondary welding interface; Alternatively, the splicing interfaces located on both sides of the butt interface to be welded are secondary welding interfaces, and the friction stir welding method comprises: controlling the welding path of the stirring head to be offset relative to the butt interface to be welded at least toward the advancing side of the butt interface to be welded, so as to weld the portion of the secondary welding interface located on the advancing side; The welding path of the stirring head includes a stable welding path and a deviated path, wherein the welding path of the stirring head along the butt interface to be welded forms a stable welding path, and the welding path of the stirring head deviates from the butt interface to be welded forms a deviated path, wherein: The deviated path is an annular path, the annular path is located on one side of the stable welding path and the starting end and the end of the annular path are respectively connected to the stable welding path; or, The deviation path includes a circular path and two arc paths, one end of the two arc paths are respectively connected to the starting end and the end of the circular path, the other ends of the two arc paths are connected to the stable welding path, the two arc paths and part of the circular path are located on one side of the stable welding path, and another part of the circular path is located on the other side of the stable welding path.
2. The friction stir welding method according to claim 1, characterized in that: The splicing interfaces located on both sides of the butt interface to be welded and on the same plane are secondary welding interfaces. The stir friction welding method includes: controlling the stirring head to offset toward the forward side and the backward side of the butt interface to be welded relative to the butt interface to be welded so as to weld the part of the secondary welding interface located on the forward side and the part of the secondary welding interface located on the backward side.
3. The friction stir welding method according to claim 1, characterized in that: The multiple splicing interfaces include multiple butt joint interfaces, at least one of the butt joint interfaces is a butt joint interface to be welded, and at least one of the butt joint interfaces is connected to the butt joint interface to be welded and is a secondary welding interface; or, the multiple splicing interfaces include butt joint interfaces and overlapping interfaces, at least one of the butt joint interfaces is a butt joint interface to be welded, and the secondary welding interface includes an overlapping interface, wherein the overlapping interface extends along a horizontal plane and the butt joint interface extends along a vertical plane.
4. The friction stir welding method according to claim 1, characterized in that: The portion of the welding path of the stirring head that deviates from the butt interface to be welded forms a deviated path, and the deviated path includes an arc path, an annular path, or a connected combination of multiple ones of the arc path, the annular path and the straight path.
5. The friction stir welding method according to claim 1, characterized in that: The speed when moving along the butt interface to be welded is a first speed, and the speed when the stirring head moves away from the butt interface to be welded is a second speed, and the second speed is less than the first speed.
6. The friction stir welding method according to claim 5, characterized in that: The ratio of the second speed to the first speed is α, 0.2<α<1.
7. The friction stir welding method according to claim 1, characterized in that: The rotation speed of the stirring head when it moves along the butt interface to be welded is a first rotation speed, and the rotation speed of the stirring head when it moves away from the butt interface to be welded is a second rotation speed, and the second rotation speed is greater than the first rotation speed.
8. The friction stir welding method according to claim 7, characterized in that: The ratio of the second rotation speed to the first rotation speed is β, 1<β<3.
9. The friction stir welding method according to claim 1, characterized in that: The portion of the welding path of the stirring head that deviates from the butt interface to be welded forms a deviation path, and the deviation path is an annular path. The maximum distance (L) that the deviation path deviates from the butt interface to be welded is 1 to 2 times the root diameter of the stirring needle of the stirring head.