Aluminum alloy material with easy chip breaking and high yield and preparation method thereof

By adjusting the chemical composition and process flow of aluminum alloy, an aluminum alloy with easy chip breakage and high yield is prepared, which solves the problems of long chip blockage and insufficient yield strength during the processing of aluminum alloy, and achieves high yield strength and short chip breakage length It is suitable for automotive gearbox components.

CN118639066BActive Publication Date: 2024-11-08D MAG KUNSHAN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411136346.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The existing aluminum alloy materials are prone to long chip blockage during processing, resulting in interruption of production process, and the yield strength of the existing high-strength materials is insufficient, which cannot meet the requirements for use of automobile transmission components.

Method used

Using 25%-35% extruded waste and balance as raw materials, the Si, Fe, Mg, Cu, Mn, Zn, Cr, Bi, Sn and other elements are allocated to control the Fe/Si ratio and the total content of Bi+Sn. Through processes such as melt casting, homogenization treatment, preheating, extrusion, online solution quenching, aging treatment and drawing, aluminum alloys that are easy to break and high yield are prepared.

Benefits of technology

The prepared aluminum alloy has high yield strength and short chip breaking length, which meets the use requirements of automotive transmission components and improves processing performance and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118639066B_ABST
    Figure CN118639066B_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum alloy material with easy chip breaking and high yield, which is configured with elements and content composition: Si: 0.4-0.8%; Fe: 0.1-0.3%; Mg: 0.8-1.2%; Cu: 0.15-0.4%; Mn: 0.15-0.20%; Zn: 0.05-0.25%; Cr: 0.04-0.14%; Bi: 0.4-0.7%; Sn: 0.4-1.2%, and the balance is Al. The invention also discloses a preparation method of the aluminum alloy material, including: melting and casting the original aluminum ingot and the intermediate alloy; homogenization treatment; preheating; extrusion; online solid solution quenching; artificial aging treatment; drawing; straightening, and obtaining an aluminum alloy product with easy chip breaking and high yield, the performance is tensile strength of 365-367MPa, yield strength of 356-359MPa, elongation of 9%-9.5%, and average chip breaking length is not more than 3cm, which meets the actual product and processing requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of aluminum alloy preparation and processing, and in particular to an aluminum alloy material with easy chip breaking and high yield and a preparation method thereof. Background Art

[0002] Aluminum alloy has the characteristics of low density, high specific strength, light weight, good electrical and thermal conductivity, good corrosion resistance, and easy forming and processing, which is suitable for lightweight design of automobiles. Considering the stability and safety of automobile driving, some parts of automobile gearboxes are made of 6 series + Sn aluminum alloy and should have a high yield strength. In the prior art, in order to reduce manufacturing costs, processing companies usually use automated equipment for turning and testing. If the chip length of aluminum alloy products is too long, it will block the transmission channel of the parts, resulting in interruption of the production process, and manual intervention for cleaning, which will lead to low production efficiency. The existing patent 202311050447.5 involves research on the use of 6082 material for high strength and easy chip breaking. Only high strength is used to meet the chip breaking needs, but at the same time, for the 6082 material, high strength requires strict on-site production technology and increased processing difficulty, which is not conducive to actual on-site production; Patent 202310922277.9 high-strength aluminum alloy material that is conducive to machining chip breaking and its preparation process uses low-melting point alloys to enhance the degree of chip breaking, but the yield strength is not high and cannot meet the use requirements of some existing gearbox components. Therefore, it is necessary to design an aluminum alloy product that meets both high yield strength and good cutting performance. Summary of the invention

[0003] In order to solve the technical problems of materials and preparation processes in the prior art, the present invention provides an easy-to-break high-yield aluminum alloy and a preparation method thereof. The preparation method is simple, and the prepared aluminum alloy has high yield strength and short chip breaking length.

[0004] In order to achieve the above technical objectives, the technical solution adopted by the embodiment of the present invention is:

[0005] In the first aspect, the present invention provides an aluminum alloy material with easy chip breaking and high yield, wherein 25%-35% of extrusion waste and the remainder are original aluminum ingots and intermediate alloy ingots as raw materials, and the elements and contents are configured as follows: Si: 0.4-0.8%; Fe: 0.1-0.3%; Mg: 0.8-1.2%; Cu: 0.15-0.4%; Mn: 0.15-0.20%; Zn: 0.05-0.25%; Cr: 0.04-0.14%; Bi: 0.4-0.7%; Sn: 0.4-1.2%, the impurity content is less than 0.1%, and the remainder is Al. At the same time, the Fe / Si ratio is controlled between 1:4 and 1:6; the total content of Bi+Sn is 1.4-1.7%.

[0006] The main functions of adding Bi elements: 1. Improve the strength and hardness of aluminum alloys. The strength and hardness of aluminum alloys are not strong enough to meet some high strength and high hardness requirements. Adding bismuth can improve its strength and hardness, making it more durable. Bismuth in aluminum alloys can form stable compounds, thereby increasing the strength and hardness of aluminum alloys. 2. Improve the corrosion resistance of aluminum alloys. Aluminum alloys will produce oxides under oxidation, which will affect them. Adding bismuth to aluminum alloys can promote the formation of stable oxides, improve their corrosion resistance, and enable them to be used in harsh environments. 3. Improve the processing properties of aluminum alloys. Adding bismuth to aluminum alloys can improve their processing properties and reduce the cost and time in material processing.

[0007] The main functions of adding Sn element are: 1. Improving strength and hardness: Adding a certain amount of tin element to aluminum alloy can significantly improve its strength and hardness, making the aluminum alloy more durable. 2. Improving corrosion resistance: Tin element can form stable compounds with other elements in aluminum to prevent the surface of aluminum alloy from being oxidized and corroded, thereby improving the corrosion resistance and durability of aluminum alloy. At the same time, by utilizing the low melting point of Sn, the possibility of long chips in the alloy during turning is reduced, and short chips are satisfied, thereby reducing the trouble of aluminum chips on the product surface and chip cleaning.

[0008] The present invention also provides a method for preparing an aluminum alloy with easy chip breaking and high yield, comprising the following steps:

[0009] Step S1, aluminum rod melting and casting: selecting aluminum alloy raw materials for melting and casting to obtain aluminum alloy cast rods;

[0010] Step S2, homogenization treatment: homogenizing the aluminum alloy cast rod obtained in step S1, then taking it out of the furnace and cooling it to room temperature with water mist;

[0011] Step S3, preheating: the preheating temperature of the aluminum alloy casting rod after homogenization in step S2 is 500-530°C, the preheating temperature of the extrusion die is 400-430°C, and the preheating temperature of the die barrel is 400-430°C;

[0012] Step S4, extrusion: using an extruder to extrude the cast rod preheated in step S3, the extrusion coefficient of the extruder is 25-60, the extrusion speed is 4-5 m / min, and the outlet temperature of the extrudate is 540-550° C.;

[0013] Step S5, online solution quenching: performing online solution quenching on the aluminum alloy extruded in step S4, using an online water cooling method;

[0014] Step S6, aging treatment: performing artificial aging treatment on the aluminum alloy obtained in step S5;

[0015] Step S7, drawing treatment: the aluminum alloy after artificial aging in step S6 is subjected to drawing treatment to obtain an aluminum alloy with easy chip breaking and high yield.

[0016] Furthermore, in step S1, before smelting, the aluminum-bismuth alloy is particularly remelted in a crucible at a remelting temperature of 950-1100°C, the cooling rate during solidification is increased (water cooling), and the size of the second phase is reduced, so as to ensure the dispersion distribution during the casting process. The smelting is carried out in a smelting furnace with an electromagnetic stirring function. The role of electromagnetic stirring is to make the temperature difference of the melt at various positions and different heights in the smelting furnace small, and the composition of each part is more uniform. During the electromagnetic stirring smelting process, the melt temperature range is: 670°C~730°C, and the temperature difference at various positions is ≤30°C. At the same time, it is required that aluminum-bismuth and aluminum-tin alloys are added to the furnace at different times during the smelting process to reduce burning loss; the refining adopts a fully automatic refining machine, and the refining machine adopts large rotor rotation and swinging, etc., to drive the flow of aluminum liquid more evenly and thoroughly, improve the cleanliness of the melt, and thus achieve better slag discharge and degassing functions.

[0017] Furthermore, in step S2, the homogenization conditions of the aluminum alloy casting rod are selected in two stages, the first stage is a low temperature stage, the temperature is 400-430°C, the time is 2-4 hours, and the second stage is a high temperature stage, the temperature is 550-565°C, the time is 10-12 hours.

[0018] Furthermore, in step S6, the aging temperature of the aluminum alloy product is 170-185° C., and the aging time is 6-9 hours.

[0019] Furthermore, in step S7, a drawing processing rate of 5-10% is set.

[0020] The technical solution provided by the embodiment of the present invention has the following beneficial effects:

[0021] The present invention adjusts the chemical composition of the aluminum alloy, adjusts the melting and casting process, and performs preheating before the extrusion step and other process settings. The aluminum alloy product prepared by the preparation method of the present invention has a tensile strength of 365-367MPa, a yield strength of 356-359MPa, an elongation of 9%-9.5%, and an average chip length of no more than 3cm, which meets the requirements of actual use and product surface quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The chip breaking shapes of Example 1 and Example 2;

[0023] Figure 2 The chip shapes of Comparative Examples 1 and 2 are shown. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0025] In a first aspect, an embodiment of the present invention provides an aluminum alloy material with easy chip breaking and high yield and a preparation method thereof, comprising the following steps:

[0026] Material:

[0027] The elements and content are configured as follows: Si: 0.4-0.8%; Fe: 0.1-0.3%; Mg: 0.8-1.2%; Cu: 0.15-0.4%; Mn: 0.15-0.20%; Zn: 0.05-0.25%; Cr: 0.04-0.14%; Bi: 0.4-0.7%; Sn: 0.4-1.2%, the impurity content is less than 0.1%, and the balance is Al. At the same time, the Fe / Si ratio is controlled between 1:4-1:6; the total content of Bi+Sn is 1.4-1.7%.

[0028] Its preparation method:

[0029] Step S1, aluminum rod casting: the aluminum-bismuth alloy is remelted in a crucible at a remelting temperature of 950-1100° C. for 2-3 hours, and water cooling is used during solidification. Aluminum alloy raw materials are selected for melting and casting to obtain aluminum alloy cast rods;

[0030] Step S2, homogenization treatment: homogenizing the aluminum alloy cast rod obtained in step S1, then taking it out of the furnace and water cooling it to room temperature;

[0031] Step S3, preheating: the preheating temperature of the aluminum alloy cast rod after homogenization in step S2 is 500-530°C, for example, 500°C, 510°C, 520°C, 530°C, etc., the preheating temperature of the extrusion die is 400-430°C, for example, 400°C, 410°C, 420°C, 430°C, etc.; the preheating temperature of the die barrel is 400-430°C, for example, 400°C, 412°C, 424°C, etc.;

[0032] Step S4, extrusion: the cast rod preheated in step S3 is extruded by an extruder, the extrusion coefficient of the extruder is 25-60, for example, 25, 30, 35, 50, 60, etc., the extrusion speed is 4-5 m / min, for example, 4 m / min, 4.3 m / min, 4.5 m / min, 4.7 m / min, 5 m / min, etc., and the outlet temperature of the extrudate is 540-550° C., for example, 540° C., 545° C., 550° C., etc.;

[0033] Step S5, online solution quenching: performing online solution quenching on the aluminum alloy extruded in step S4, using online water mist cooling;

[0034] Step S6, aging treatment: performing artificial aging treatment on the aluminum alloy obtained in step S5;

[0035] Step S7, drawing treatment: the aluminum alloy after artificial aging in step S6 is subjected to drawing treatment to obtain an aluminum alloy with easy chip breaking and high yield.

[0036] Furthermore, in step S1, the aluminum-bismuth alloy is remelted in a crucible at a remelting temperature of 950-1100° C. for 2-3 hours. Water cooling is used during solidification. The elements and contents thereof are configured as follows, in terms of mass percentage: Si: 0.4-0.8%; Fe: 0.1-0.3%; Mg: 0.8-1.2%; Cu: 0.15-0.4%; Mn: 0.15-0.20%; Zn: 0.05-0.25%; Cr: 0.04-0.14%; Bi: 0.4-0.7%; Sn: 0.4-1.2%, the impurity content is less than 0.1%, and the balance is Al.

[0037] Furthermore, in step S2, the aluminum alloy casting rod is homogenized in two stages, the first stage is a low temperature stage with a temperature of 400-430°C for 2-4 hours, for example, 400°C, 410°C, 430°C, etc., for 2-4 hours.

[0038] The second stage is a high temperature stage at 550-565°C for 10-12 hours, for example, 555°C, 560°C, 565°C, etc. for 10-12 hours.

[0039] Furthermore, in step S7, the aging temperature of the aluminum alloy product is 170-185°C, for example, 170°C, 175°C, 180°C, 185°C; and the aging time is 6-9h, for example, 6h, 8h, 9h.

[0040] Example 1

[0041] A method for preparing an aluminum alloy material with easy chip breaking and high yield, comprising the following steps:

[0042] Step S1, aluminum rod casting: the aluminum-bismuth alloy is remelted in a crucible at a remelting temperature of 1100°C for 2 hours, and water-cooled during solidification, and then the aluminum alloy raw materials are melted and cast into cast rods. The aluminum alloy includes the following components by mass percentage: Si: 0.7%; Fe: 0.15%; Mg: 0.9%; Cu: 0.25%; Mn: 0.15%; Zn: 0.05%; Cr: 0.09%; Bi: 0.52%; Sn: 0.95%, and the balance is Al. The Fe / Si ratio is 1:4.67; and the total content of Bi+Sn is 1.47%.

[0043] Step S2, homogenization treatment: the aluminum alloy cast rod obtained in step S1 is homogenized, the first stage is 400°C, the time is 2.5h; the second stage is 565°C, the time is 10h, and then it is taken out of the furnace and water-cooled to room temperature.

[0044] Step S3, preheating: the preheating temperature of the aluminum alloy cast rod after homogenization in step S2 is 530°C, the preheating temperature of the extrusion die is 430°C, and the preheating temperature of the die barrel is 410°C.

[0045] Step S4, extrusion: the cast rod preheated in step S3 is extruded by an extruder, the extrusion coefficient of the extruder is 42, the extrusion speed is 4.5 m / min, and the outlet temperature of the extrudate is 545°C.

[0046] Step S5, online solution quenching: the aluminum alloy extruded in step S4 is subjected to online solution quenching by using an online water cooling method.

[0047] Step S6, aging treatment: performing artificial aging treatment on the aluminum alloy obtained in step S5 at 185° C. for 6 hours.

[0048] Step S7, drawing treatment: the aluminum alloy after artificial aging in step S6 is subjected to drawing treatment, and the drawing processing rate is set to 5%, so as to obtain an aluminum alloy with easy chip breaking and high yield.

[0049] Example 2

[0050] A method for preparing an aluminum alloy with easy chip breaking and high yield, comprising the following steps:

[0051] Step S1, aluminum rod casting: the aluminum-bismuth alloy is remelted in a crucible at a remelting temperature of 1100°C for 2 hours. Water cooling is used during solidification. The aluminum alloy includes the following components by mass percentage: Si: 0.7%; Fe: 0.15%; Mg: 0.9%; Cu: 0.25%; Mn: 0.15%; Zn: 0.05%; Cr: 0.09%; Bi: 0.52%; Sn: 0.95%, and the balance is Al. The Fe / Si ratio is 1:4.67; and the total content of Bi+Sn is 1.47%.

[0052] Step S2, homogenization treatment: the aluminum alloy cast rod obtained in step S1 is homogenized, the first stage is 420°C, the time is 2h; the second stage is 561°C, the time is 12h, and then it is taken out of the furnace and water-cooled to room temperature.

[0053] Step S3, preheating: the preheating temperature of the aluminum alloy cast rod after homogenization in step S2 is 520°C, the preheating temperature of the extrusion die is 430°C, and the preheating temperature of the die barrel is 410°C.

[0054] Step S4, extrusion: the cast rod preheated in step S3 is extruded by an extruder, the extrusion coefficient of the extruder is 42, the extrusion speed is 4.5 m / min, and the outlet temperature of the extrudate is 545°C.

[0055] Step S5, online solution quenching: the aluminum alloy extruded in step S4 is subjected to online solution quenching by using an online water cooling method.

[0056] Step S6, aging treatment: the aluminum alloy obtained in step S5 is subjected to artificial aging treatment at 175° C. for 9 hours.

[0057] Step S7, drawing treatment: the aluminum alloy after artificial aging in step S6 is subjected to drawing treatment, and the drawing processing rate is set to 8%, so as to obtain an aluminum alloy with easy chip breaking and high yield.

[0058] Comparative Example 1

[0059] A method for preparing an aluminum alloy comprises the following steps:

[0060] Step S1, aluminum rod melting and casting: the aluminum alloy raw material includes the following components by mass percentage: Si: 0.65%; Fe: 0.21%; Mg: 0.89%; Cu: 0.21%; Mn: 0.04%; Zn: 0.04%; Cr: 0.11%; Bi: 0.45%; Sn: 0.47%, and the balance is Al.

[0061] Step S2, homogenization treatment: the aluminum alloy cast rod obtained in step S1 is homogenized, the first stage is 410°C, the time is 2h; the second stage is 560°C, the time is 12h, and then it is taken out of the furnace and water-cooled to room temperature.

[0062] Step S3, preheating: the preheating temperature of the aluminum alloy cast rod after homogenization in step S2 is 520°C, the preheating temperature of the extrusion die is 430°C, and the preheating temperature of the die barrel is 410°C.

[0063] Step S4, extrusion: the cast rod preheated in step S3 is extruded by an extruder, the extrusion coefficient of the extruder is 42, the extrusion speed is 4.5 m / min, and the outlet temperature of the extrudate is 545°C.

[0064] Step S5, online solution quenching: the aluminum alloy extruded in step S4 is subjected to online solution quenching by using an online water cooling method.

[0065] Step S6, straightening: the aluminum alloy obtained in step S5 is artificially aged at 175° C. for 9 hours to obtain an aluminum alloy.

[0066] Comparative Example 2

[0067] A method for preparing an aluminum alloy comprises the following steps:

[0068] Step S1, aluminum rod casting: melt and cast a raw material of aluminum alloy with grade 6082 into a cast rod. The aluminum alloy includes the following components by mass percentage: Si: 0.95%, Fe: 0.15%, Cu: 0.05%, Mn: 0.65%, Mg: 0.75%, Cr: 0.01%, Zn: 0.02%, Ti: 0.04%, other impurity single elements: less than 0.05%, other impurity elements total: 0.15%, and the balance is Al.

[0069] Step S2, homogenization treatment: homogenize the aluminum alloy cast rod obtained in step S1 at 565°C for 10 hours, then remove from the furnace and water-cool to room temperature;

[0070] Step S3, preheating: the preheating temperature of the aluminum alloy cast rod after homogenization in step S2 is 520°C, the preheating temperature of the extrusion die is 430°C, and the preheating temperature of the die barrel is 410°C.

[0071] Step S4, extrusion: the cast rod preheated in step S3 is extruded by an extruder, the extrusion coefficient of the extruder is 42, the extrusion speed is 4.5 m / min, and the outlet temperature of the extrudate is 545°C.

[0072] Step S5, online solution quenching: the aluminum alloy extruded in step S4 is subjected to online solution quenching by using an online water cooling method.

[0073] Step S6, aging treatment: the aluminum alloy obtained in step S5 is subjected to artificial aging treatment at 175° C. for 9 hours.

[0074] Step S7, drawing treatment: the aluminum alloy after artificial aging in step S6 is subjected to drawing treatment, and the drawing processing rate is set to 8% to obtain an aluminum alloy.

[0075] Application Examples

[0076] This application tests the tensile properties and chip length of the aluminum alloys provided in Example 1, Example 2, Comparative Example 1, and Comparative Example 2. Specifically, the aluminum alloys obtained in Example 1, Example 2, Comparative Example 1, and Comparative Example 2 of the same mass are selected as samples, and the tensile properties of the samples are tested according to the method provided in the standard "GB / T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method". The samples are cut and the length of the chip generated during the cutting is measured ( Figure 1 and Figure 2 ). Specific test parameters of the aluminum alloys obtained in Example 1, Example 2, Comparative Example 1, and Comparative Example 2 are shown in Table 1 below.

[0077] Table 1 Performance test table of aluminum alloy

[0078]

[0079] As can be seen from Table 1, in Comparative Example 1, the alloy content is changed and the drawing process is cancelled, which significantly reduces the yield strength and also affects the cutting performance. In Comparative Example 2, due to the selection of different materials, the material properties and cutting aluminum chips cannot meet the use requirements; Comparative Example 1 and Comparative Example 2 both result in the aluminum alloy yield strength being too low and the chip length being too long, which cannot meet the actual use requirements.

[0080] The aluminum alloy bars prepared in Example 1 and Example 2, by controlling the preheating temperature of the cast bars at 515-535°C in steps S1-S7, and controlling the extrusion speed at 4-5m / min and the outlet temperature of the extrudate at 535-550°C in step S4 extrusion molding, can simultaneously meet the following requirements: tensile strength of 365-367MPa, yield strength of 356-359MPa, elongation of 9%-9.5%, and average chip length ≤3cm. While meeting the requirements of mechanical properties, it also takes into account machinability and meets the use requirements, and can be used in automotive transmission parts.

[0081] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing an aluminum alloy with easy chip breaking and high yield, It is characterized in that The following steps are involved: Step S1, aluminum rod casting: select aluminum alloy raw materials for melting and casting to obtain aluminum alloy cast rods; before melting, the alloy is remelted at a remelting temperature of 950-1100°C; Step S2, homogenization treatment: homogenize the aluminum alloy cast rod obtained in step S1, and then cool it to room temperature by water mist after it is taken out of the furnace; the homogenization conditions of the aluminum alloy cast rod are selected into a two-stage type, the first stage is a low temperature stage, the temperature is 400-430°C, the time is 2-4h, and the second stage is a high temperature stage, the temperature is 550-565°C, and the time is 10-12h; Step S3, preheating: the preheating temperature of the aluminum alloy casting rod after homogenization in step S2 is 500-530°C, the preheating temperature of the extrusion die is 400-430°C, and the preheating temperature of the die barrel is 400-430°C; Step S4, extrusion: using an extruder to extrude the cast rod preheated in step S3, the extrusion coefficient of the extruder is 25-60, the extrusion speed is 4-5 m / min, and the outlet temperature of the extrudate is 540-550° C.; Step S5, online solution quenching: performing online solution quenching on the aluminum alloy extruded in step S4, using an online water cooling method; Step S6, aging treatment: performing artificial aging treatment on the aluminum alloy obtained in step S5; Step S7, drawing treatment: drawing the aluminum alloy after artificial aging in step S6 to obtain an aluminum alloy with easy chip breaking and high yield; Aluminum alloy selects 25%-35% of extrusion waste and the rest is original aluminum ingot and intermediate alloy ingot as raw materials, and is configured with elements and content composition: Si: 0.4-0.8; Fe: 0.1-0.3; Mg: 0.8-1.2; Cu: 0.15-0.4; Mn: 0.15-0.20; Zn: 0.05-0.25; Cr: 0.04-0.14; Bi: 0.4-0.7; Sn: 0.4-1.2, impurity content is less than 0.1%, the balance is Al, and the Fe / Si ratio is controlled between 1:4-1:6; the total content of Bi+Sn is 1.4-1.

7.

2. The method for preparing the aluminum alloy with easy chip breaking and high yield according to claim 1, It is characterized in that In step S6, the aging temperature of the aluminum alloy product is 170-185° C., and the aging time is 6-9 hours.

3. The method for preparing the aluminum alloy with easy chip breaking and high yield according to claim 1, It is characterized in that In step S7, a drawing processing rate of 5-10% is set.