Treatment of cyanide wastewater from gold mines and resource regeneration methods

Through the segmented treatment and coupled catalytic technology of cyanide-reducing precipitation agent and deep purification treatment agent, the removal of cyanide and copper ions in cyanide-containing wastewater in gold mines is solved, efficient pollutant removal and resource recovery are achieved, and treatment is reduced The cost reaches zero generation of wastewater and waste residue.

CN118724389BActive Publication Date: 2024-11-29CHANGCHUN GOLD RES INST

Patent Information

Application Number
CN202411224939.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-29
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The existing gold mine cyanide wastewater treatment methods consume a large amount of agents, cyanide impurities in the precipitates are prone to environmental damage, and the recovery rate of valuable substances is low, making it difficult to achieve efficient utilization of resources.

Method used

The copper-containing cyanide wastewater is treated in segments using cyano-reducing precipitation agents and deep purification treatment agents. Total cyanide and copper ions are removed through coupled catalytic technology to achieve efficient pollutant removal and resource recovery.

Benefits of technology

The total cyanide removal rate is greater than 99%, and the copper ion removal rate is greater than 99%, which reduces the treatment cost, improves the resource recovery rate, and achieves zero generation of wastewater and waste residue during the treatment process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724389B_ABST
    Figure CN118724389B_ABST
Patent Text Reader

Abstract

The invention provides a method for treating cyanide-containing wastewater in a gold mine and regenerating resources, and relates to the technical field of environmental protection and water treatment. The method first uses a cyanide-reducing precipitation agent to treat copper-cyanide-containing wastewater to obtain a cyanide-reducing precipitation slag, cyanide is destroyed, and copper ions generate copper hydroxide and cuprous hydroxide precipitation; then a deep purification treatment agent is used to deeply purify the overflow liquid. Then, the cyanide in the cyanide-reducing precipitation slag and the deep purification slag is subjected to coupled catalytic treatment by using the cyanide-reducing precipitation agent and the deep purification treatment agent under the reaction conditions of the catalyst, so that the thiocyanate and cyanide in the cyanide-reducing precipitation slag and the deep purification slag are destroyed by the reaction of the agent under the catalytic conditions. Then, the deep treatment liquid is used to elute the crude copper product after the coupled catalytic treatment, and the cyanide, salt and other impurities in the copper slag are further removed to obtain a refined copper product. The total cyanide removal rate of the method is greater than 99%, and the copper ion removal rate is greater than 99%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental protection and water treatment, and in particular to a method for treating cyanide-containing wastewater in a gold mine and regenerating resources. Background Art

[0002] In the gold industry, the cyanide gold extraction process is often used for the more common copper-gold ores. This process adds a large amount of sodium cyanide to leach the gold in the ore. At the same time, the metallic copper in the ore is also leached, which produces copper-cyanide wastewater. In order to avoid adverse effects on the environment, economical and efficient treatment is required.

[0003] At present, the treatment of this type of cyanide-containing wastewater mainly adopts the bleaching powder / hydrogen peroxide method, the Inco method, the ozone oxidation method, etc. These methods not only consume a large amount of reagents, but also produce precipitates containing cyanide impurities, which can easily cause environmental damage problems. At the same time, the content of valuable substances in the precipitates is low and difficult to be recycled.

[0004] In order to achieve green development and reduce costs and increase efficiency, the environmental protection management process should first consider recycling and creating high value-added resources from waste, and then adopt targeted, efficient and low-cost treatment technologies.

[0005] In view of this, it is necessary to propose a method for treating cyanide-containing wastewater in gold mines and regenerating resources to solve the above problems. Summary of the invention

[0006] In view of the defects of the above-mentioned prior art, the purpose of the present invention is to provide a method for treating cyanide-containing wastewater in gold mines and regenerating resources. The method adopts a cyanide-reducing precipitation agent and a deep purification treatment agent to treat copper-cyanide-containing wastewater in stages, and the total cyanide removal rate is greater than 99%, and the copper ion removal rate is greater than 99%; the treatment process is energy-saving and environmentally friendly, and the pollutant treatment efficiency is high. It has the advantages of agent utilization, high treatment efficiency, and recyclable resources, and zero generation of wastewater and waste residue can be achieved in the treatment process.

[0007] To achieve the above object, the present invention provides a method for treating cyanide-containing wastewater in a gold mine and regenerating resources, comprising the following steps:

[0008] S1, cyanide reduction precipitation treatment: adding cyanide reduction precipitation agent to treat copper-cyanide wastewater, stirring to make the agent and water fully mixed, after the reaction is complete, entering the precipitation tank for natural sedimentation, and obtaining cyanide reduction precipitation residue and overflow liquid; wherein the overflow liquid enters step S2 for deep purification treatment, and the cyanide reduction precipitation residue enters step S3 for coupled catalytic treatment; the cyanide reduction precipitation agent is composed of sodium isoVC, sodium citrate, CaS x Two or three of the following:

[0009] The total cyanide concentration in the copper-cyanide wastewater is lower than 350 mg / L, the easily releasable cyanide concentration is lower than 300 mg / L, the copper ion concentration is lower than 600 mg / L, and the pH value of the copper-cyanide wastewater is between 7 and 9;

[0010] S2, deep purification treatment: adding deep purification treatment reagent to the overflow liquid obtained in step S1 for treatment, so that it fully reacts, and then performing solid-liquid separation through a filter to obtain a solid phase of deep purification slag and a liquid phase of deep treatment liquid; the deep treatment liquid meets the standards for discharge or reuse, and part of the deep treatment liquid enters step S4 to elute the crude copper product after the coupled catalytic treatment;

[0011] S3, slag coupled catalytic treatment: drying, grinding, and oxidizing in an oxygen-rich atmosphere the cyanide-reduced slag obtained in step S1 and the deep purified slag obtained in step S2, and then subjecting them to coupled catalytic treatment to obtain a crude copper product;

[0012] S4, return water elution treatment: the crude copper product obtained in step S3 is eluted with the deep treatment liquid obtained in step S2 to obtain a refined copper product. The washing water re-enters step S2 for deep purification treatment and then meets the discharge standards.

[0013] Furthermore, in step S2, the deep purification treatment agent is composed of one or more of sodium isoVC, calcium aluminum sulfate, and ferrous sulfide.

[0014] Furthermore, the deep purification treatment agent is composed of sodium isoVC and calcium aluminum sulfate. In step S2, the mass ratio of sodium isoVC to total cyanide in the added deep purification treatment agent is (2.3-3.0):1, and the mass ratio of calcium aluminum sulfate to copper ions is (1.7-2.5):1.

[0015] Further, the cyanide-reducing precipitation agent includes sodium isoVC, sodium citrate and CaS x In step S1, the mass ratio of sodium isoVC to total cyanide in the added cyanide reduction precipitation agent is (1.5-3.5):1, the mass ratio of sodium citrate to copper ion is (0.9-1.5):1, and the mass ratio of CaS x The mass ratio to total cyanide is (0.4-0.8):1.

[0016] Furthermore, in step S3, the coupled catalytic treatment refers to: using a cyanide-reducing precipitation agent and a deep purification treatment agent, the cyanide in the cyanide-reducing precipitation slag and the deep purification slag is subjected to coupled catalytic treatment under catalyst-catalyzed reaction conditions, and the reaction time is 30-90 min. The thiocyanate and cyanide in the cyanide-reducing precipitation slag and the deep purification slag react with the agent and are destroyed under catalyst-catalyzed conditions.

[0017] Furthermore, in step S3, the mass ratio of the total mass of the cyanide-reducing precipitation agent and the deep purification treatment agent to the total cyanide is (0.5-0.8):1; the cyanide-reducing precipitation slag and the deep purification slag contain the remaining cyanide-reducing precipitation agent and the deep purification treatment agent in step S1 and step S2; if the mass ratio of the total mass of the remaining cyanide-reducing precipitation agent and the deep purification treatment agent to the total cyanide is less than 0.5, the cyanide-reducing precipitation agent is added until the mass ratio of the two is (0.5-0.8):1.

[0018] Furthermore, in step S1, the complete reaction means that the redox reaction of the reagent is completed, the ORP in the water no longer changes, the generated cyanide-reducing precipitate is recovered, the cyanide is destroyed, the copper ions and cuprous ions generate copper hydroxide and cuprous hydroxide precipitates respectively, and most of the copper is recovered in this process.

[0019] Furthermore, in the elution treatment of step S4, the mass ratio of the crude copper product to the deep treatment liquid is 1:(3.0-8.0).

[0020] Furthermore, in step S4, the mass ratio of the deep purification treatment agent to the total cyanide in the deep treatment liquid is (0.2-0.4):1; the deep treatment liquid contains the deep purification treatment agent remaining in step S2; if the mass ratio of the remaining deep purification treatment agent to the total cyanide is less than 0.2, sodium isoVC is added to make the mass ratio of the deep purification treatment agent to the total cyanide (0.2-0.4):1. This process mainly removes impurities such as cyanide and salts in copper slag.

[0021] Furthermore, in step S3, the catalyst carrier is one or a combination of transition metals and their oxides, and the catalyst active ingredient is a copper-containing porous material.

[0022] Furthermore, in step S3, the main components of the cyanide-reducing precipitated slag and the deep purification slag are copper hydroxide, and the impurities are mainly thiocyanate, cyanide, sodium salt, etc. In the oxygen-enriched atmosphere oxidation treatment, the temperature in the reactor is appropriately increased to 150°C-200°C; the gas introduced is air or oxygen, and the mass ratio of oxygen to precipitated slag is (5.0-7.0): 1. In this process, copper hydroxide and cuprous hydroxide are oxidized and decomposed into copper oxide. Among them, the mass of the precipitated slag is the total mass of the cyanide-reducing precipitated slag and the deep purification slag.

[0023] The beneficial effects of the present invention are:

[0024] 1. The method for treating cyanide-containing wastewater in gold mines and regenerating resources provided by the present invention adopts a cyanide-reducing precipitation agent and a deep purification treatment agent to treat the copper-cyanide-containing wastewater in stages, and then obtains a refined copper product through coupled catalysis and process effluent washing. The main component of the refined copper product is copper oxide with a content of more than 99%, which can be directly recycled.

[0025] Specifically, firstly, a cyanide-reducing precipitation agent is used to treat copper-cyanide-containing wastewater to obtain a cyanide-reducing precipitation residue, cyanide is destroyed, and copper ions generate copper hydroxide and cuprous hydroxide precipitation; then, a deep purification agent is used to perform deep purification on the overflow liquid, and the obtained deep treatment liquid meets the discharge standards; the remaining cyanide-reducing precipitation agent and deep purification agent in steps S1 and S2 are subjected to coupled catalytic treatment on cyanide in the cyanide-reducing precipitation residue and the deep purification residue under the reaction conditions of the catalyst in step S3, and the thiocyanate and cyanide in the cyanide-reducing precipitation residue and the deep purification residue react with the agent under the conditions of the catalyst and are destroyed; part of the deep treatment liquid obtained in step S2 enters step S4 to perform elution treatment on the crude copper product after the coupled catalytic treatment, and further removes cyanide, salts and other impurities in the copper slag to obtain a refined copper product.

[0026] The entire process is reasonably set up, the reaction parameters are easy to control, the operation is simple, and the operating cost is low; the treatment process is energy-saving and environmentally friendly, and has the advantages of chemical utilization, high treatment efficiency, high resource recovery rate, and recyclable resources, and zero generation of wastewater and waste residue can be achieved during the treatment process.

[0027] 2. The present invention reasonably controls the cyanide-reducing precipitation agents, sodium isoVC, sodium citrate, CaS x As well as the dosage of deep purification treatment agents such as sodium isoVC, calcium aluminum sulfate and ferrous sulfide, a total cyanide removal rate of more than 99% and a copper ion removal rate of more than 99% were achieved, with high pollutant treatment efficiency and low treatment cost.

[0028] 3. The present invention has a good treatment effect on cyanide, can achieve 100% recovery of valuable substances such as copper, and has extremely high added value. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The present invention provides a process flow diagram of the method for treating cyanide-containing wastewater in gold mines and regenerating resources. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0031] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0032] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0033] See also Figure 1 As shown, the present invention provides a method for treating cyanide-containing wastewater in a gold mine and regenerating resources, comprising the following steps:

[0034] S1, cyanide reduction precipitation treatment: adding cyanide reduction precipitation agent to treat copper-cyanide wastewater, stirring to make the agent and water fully mixed, after the reaction is complete, entering the precipitation tank for natural sedimentation, and obtaining cyanide reduction precipitation residue and overflow liquid; wherein the overflow liquid enters step S2 for deep purification treatment, and the cyanide reduction precipitation residue enters step S3 for coupled catalytic treatment; the cyanide reduction precipitation agent is composed of sodium isoVC, sodium citrate, CaS x Two or three of the following:

[0035] The total cyanide concentration in the copper-cyanide-containing wastewater is lower than 350 mg / L, the easily releasable cyanide concentration is lower than 300 mg / L, the copper ion concentration is lower than 600 mg / L, and the pH value of the copper-cyanide-containing wastewater is between 7 and 9.

[0036] Specifically, in step S1, a cyanide-reducing precipitation agent is added to the copper-cyanide wastewater, and the mixture is evenly mixed by a stirring device. The reaction time is 60-120 min, and the reaction is carried out until the ORP no longer changes. The generated cyanide-reducing precipitation residue is recovered, cyanide is destroyed, and copper ions are precipitated into copper hydroxide. Most of the copper is recovered in this process.

[0037] Preferably, the cyanide-reducing precipitation agent includes sodium isoVC, sodium citrate and CaS x .

[0038] In step S1, the mass ratio of sodium isoVC to total cyanide in the added cyanide reduction precipitation agent is (1.5-3.5):1, the mass ratio of sodium citrate to copper ion is (0.9-1.5):1, and the mass ratio of CaS x The mass ratio to total cyanide is (0.4-0.8):1.

[0039] S2, deep purification treatment: add deep purification treatment reagent to the overflow liquid obtained in step S1 for treatment, make it fully react, and then separate the solid and liquid through the filter to obtain deep purification slag in the solid phase and deep treatment liquid in the liquid phase; the deep treatment liquid meets the discharge standards or is reused, and part of the deep treatment liquid enters step S4 to elute the crude copper product after the coupled catalytic treatment.

[0040] Specifically, in step S2, the deep purification treatment agent is composed of one or more of sodium isocyanate, calcium aluminum sulfate, and ferrous sulfide.

[0041] Preferably, the deep purification treatment agent consists of sodium isoVC and calcium aluminum sulfate.

[0042] In step S2, the mass ratio of sodium isoVC to total cyanide in the added deep purification treatment agent is (2.3-3.0):1, and the mass ratio of calcium aluminum sulfate to copper ions is (1.7-2.5):1.

[0043] The process mainly uses a combination of chemicals to treat the remaining copper-cyanide complex in the water. The chemicals first adsorb cyanide, then release free radicals to oxidize, destroy, and precipitate cyanide. The purpose is to deeply treat pollutants and purify them in multiple stages.

[0044] S3, coupled catalytic treatment of slag: drying, grinding, and oxidizing in an oxygen-rich atmosphere the cyanide-reduced slag obtained in step S1 and the deep-purified slag obtained in step S2, and then subjecting them to coupled catalytic treatment to obtain a crude copper product.

[0045] Specifically, in step S3, the main components of the cyanide-reducing precipitated slag and the deep purification slag are copper hydroxide, and the impurities are mainly thiocyanate, cyanide, sodium salt, etc. In the oxygen-enriched atmosphere oxidation treatment, the temperature in the reactor is appropriately increased to 150°C-200°C; the gas introduced is air or oxygen, and the mass ratio of oxygen to precipitated slag is (5.0-7.0): 1. In this process, copper hydroxide and cuprous hydroxide are oxidized and decomposed into copper oxide. Among them, the mass of the precipitated slag is the total mass of the cyanide-reducing precipitated slag and the deep purification slag.

[0046] The coupled catalytic treatment refers to the use of cyanide-reducing precipitation agents and deep purification treatment agents to carry out coupled catalytic treatment on the cyanide in the cyanide-reducing precipitation slag and the deep purification slag under the reaction conditions of the catalyst. The reaction time is 30-90 minutes. The thiocyanate and cyanide in the cyanide-reducing precipitation slag and the deep purification slag react with the agents and are destroyed under the catalytic conditions.

[0047] In step S3, the mass ratio of the total mass of the cyanide-reducing precipitation agent and the deep purification treatment agent to the total cyanide is (0.5-0.8):1.

[0048] The cyanide-reducing precipitation slag and the deep purification slag contain the remaining cyanide-reducing precipitation agent and the deep purification agent in step S1 and step S2; if the mass ratio of the total mass of the remaining cyanide-reducing precipitation agent and the deep purification agent to the total cyanide is less than 0.5, the cyanide-reducing precipitation agent is added to the mass ratio of the two to (0.5-0.8): 1. If the mass ratio of the two satisfies (0.5-0.8): 1, the reaction is directly carried out.

[0049] The catalyst carrier is one or a combination of transition metals and their oxides, and the catalyst active component is a porous material containing copper, such as a porous material containing copper oxide as a catalyst and carrier, or a composite of manganese oxide and iron oxide as a catalyst carrier.

[0050] S4, return water elution treatment: the crude copper product obtained in step S3 is eluted with the deep treatment liquid obtained in step S2 to obtain a refined copper product. The washing water re-enters step S2 for deep purification treatment and then meets the discharge standards.

[0051] Specifically, in the elution treatment of step S4, the mass ratio of the crude copper product to the deep treatment liquid is 1:(3.0-8.0).

[0052] The mass ratio of the deep purification treatment agent to the total cyanide in the deep treatment liquid is (0.2-0.4):1. The deep treatment liquid contains the deep purification treatment agent remaining in step S2; if the mass ratio of the remaining deep purification treatment agent to the total cyanide is less than 0.2, sodium isoVC is added to make the mass ratio of the deep purification treatment agent to the total cyanide (0.2-0.4):1. This process mainly removes impurities such as cyanide and salts in the copper slag.

[0053] The entire process is reasonably set up, the reaction parameters are easy to control, the operation is simple, and the operating cost is low; the treatment process is energy-saving and environmentally friendly, and has the advantages of chemical utilization, high treatment efficiency, high resource recovery rate, and recyclable resources, and zero generation of wastewater and waste residue can be achieved during the treatment process.

[0054] The gold mine cyanide wastewater treatment and resource regeneration method provided by the present invention is described below in conjunction with specific embodiments.

[0055] Example 1

[0056] The total cyanide concentration in the cyanide-containing wastewater of a gold mine is 220 mg / L, the easily releasable cyanide concentration is 180 mg / L, the copper ion concentration is 423 mg / L, and the pH value of the cyanide-containing wastewater is 8.9.

[0057] A method for treating cyanide-containing wastewater in a gold mine and regenerating resources comprises the following steps:

[0058] S1, adding a cyanide-reducing precipitation agent into a cyanide-reducing precipitation reactor to treat the copper-cyanide-containing wastewater, and stirring to make the cyanide-reducing precipitation agent and the water body fully and evenly mixed.

[0059] Cyanide-reducing precipitation agents include sodium isoVC, sodium citrate and CaS x The mass ratio of sodium isoVC to total cyanide in the added cyanide reduction precipitation agent is 2.5:1, the mass ratio of sodium citrate to copper ion is 1.2:1, and the mass ratio of CaS x The mass ratio to total cyanide is 0.5:1.

[0060] The reaction was stirred for 1 h to destroy the cyanide and generate precipitates. After solid-liquid separation, the mass of the cyanide-reducing precipitate was 3.2% of the amount of cyanide-containing wastewater treated. The crude copper product was obtained by coupled catalytic treatment. The total cyanide concentration in the liquid phase after treatment was 0.72 mg / L, and the copper ion concentration was 3.6 mg / L, and deep purification treatment was carried out.

[0061] S2, the liquid phase of step S1 flows into a deep purification treatment reactor, and a deep purification treatment agent is added into the deep purification treatment reactor. The deep purification treatment agent includes sodium isoVC and calcium aluminum sulfate.

[0062] The mass ratio of sodium isoVC addition to total cyanide is 2.5:1, and the mass ratio of calcium aluminum sulfate addition to copper ion is 2.0:1. The reaction is fully reacted for 0.5 h. After the reaction, the solid-liquid separation is carried out through the filter. After liquid phase treatment, the total cyanide concentration is 0.16 mg / L, and the copper ion concentration is 0.92 mg / L, which meets the production requirements and can be reused in the front-end production system. The solid phase deep purification slag is coupled catalytic treatment.

[0063] S3, drying, grinding, and oxidizing in an oxygen-rich atmosphere the cyanide-reducing precipitated slag obtained in step S1 and the deep-purified slag obtained in step S2, and then performing coupled catalytic treatment, adding a cyanide-reducing precipitating agent to the slag so that the mass ratio of the agent to the total cyanide is 0.5:1.

[0064] A porous material of copper oxide was used as a catalyst and carrier, oxygen was introduced, the mass ratio of oxygen to precipitated slag was 5.0:1, the temperature in the reactor was raised to 200°C, and the coupled catalytic reaction was carried out for 90 minutes to obtain a crude copper product with a copper oxide content of 86.3%.

[0065] S4, eluting the crude copper product: adding the deep treatment liquid obtained in step S2 to wash the crude copper product; the mass ratio of the crude copper product to the deep treatment liquid is 1.0:7.0, and sodium isoVC is added so that the mass ratio of the reagent mass in the deep treatment liquid (the total amount of sodium isoVC and calcium aluminum sulfate) to the total cyanide in the crude copper product is 0.2:1, and after washing with water, a refined copper product is obtained, and the copper oxide content is 99.3%.

[0066] The total cyanide concentration in the obtained washing water was 4.62 mg / L, and the copper ion concentration was 0.6 mg / L. It was re-deeply purified by adding deep purification treatment agents and fully reacting for 0.5 h. After treatment, it met the discharge standards.

[0067] Example 2 and Comparative Example 1

[0068] The gold mine cyanide wastewater treatment and resource regeneration method of Example 2 and Comparative Example 1 is different from Example 1 mainly in that the amount of the cyanide-reducing precipitation agent in step S1 is changed, as shown in Table 1. The other operations are generally the same as those in Example 1 and will not be repeated here.

[0069] The reaction time of step S1 is 1.5 h. After solid-liquid separation, the mass of the cyanide-reducing precipitate is 2.8% of the treated water volume. After the filtrate enters the back-end unit for treatment, it meets the production requirements and can be reused in the front-end production system. The device can operate well and stably.

[0070] Example 3

[0071] The gold mine cyanide wastewater treatment and resource regeneration method of Example 3 is different from that of Example 1 mainly in that the dosage of the cyanide-reducing precipitation agent in step S1 is changed, as shown in Table 1. The other operations are generally the same as those in Example 1 and will not be described in detail here.

[0072] The reaction time of step S1 is 2 h. After solid-liquid separation, the mass of the cyanide-reducing precipitate is 4.0% of the treated water volume. Similarly, after the filtrate enters the back-end unit for treatment, it meets the production requirements and can be reused in the front-end production system. The device can operate well and stably.

[0073] Table 1

[0074]

[0075] Experiments show that under the conditions of Comparative Example 1, the mass of the cyanide-reducing precipitate after filtration is only 1.2% of the treated water volume, the total cyanide concentration in the liquid phase after treatment is 21.4 mg / L, and the copper ion concentration is 34.5 mg / L. After deep purification treatment, the discharge or reuse requirements cannot be met. The precipitate is crudely processed and then washed with water, resulting in a product with poor purity.

[0076] The reason is that the amount of cyanide-reducing precipitation agent added in Comparative Example 1 is insufficient. The agent breaks the complex in the water through coupling, and the advanced free radical oxidation destroys the copper cyanide complex in the precipitated water. Due to the insufficient agent, the cyanide treatment effect is not good, the recovery rate of copper is reduced, and the final product purity is poor.

[0077] Comparative Example 2

[0078] The difference between Comparative Example 2 and Example 1 is mainly that: in step S3, when the coupled catalytic treatment is performed, the mass ratio of the cyanide-reducing precipitation agent to the total cyanide in the slag is 0.1: 1. Other operations are generally the same as those in Example 1 and will not be repeated here.

[0079] Experiments show that after coupled catalytic treatment, the purity of the crude copper product is poor, with a copper oxide content of 72.3%. After refining, the copper oxide content is only 86.7%.

[0080] The reason is that during the coupled catalytic treatment process, the amount of cyanide-reducing precipitation agent is low, and the agent fails to fully destroy the residual cyanide in the slag under catalytic conditions, resulting in copper cyanide impurities in the copper oxide, making the product purity poor.

[0081] Comparative Example 3

[0082] The difference between Comparative Example 3 and Example 1 is mainly that: in step S3, when the coupled catalytic treatment is performed, the catalytic temperature in the coupled catalytic reaction device is 100° C. Other operations are substantially the same as those in Example 1 and will not be described in detail here.

[0083] Experiments show that under this condition, after coupled catalytic treatment, the purity of the crude copper product is poor, with a copper oxide content of 61.5%. At the same time, after refining, the copper oxide content is only 76.9%.

[0084] The reason is that the temperature in the reaction device is low, so cupric hydroxide and cuprous hydroxide cannot be fully decomposed into copper oxide, resulting in a decrease in the content of copper oxide.

[0085] Example 4

[0086] The gold mine cyanide wastewater treatment and resource regeneration method of Example 4 is different from that of Example 1 mainly in that the dosage of the deep purification treatment agent in step S2 is changed, as shown in Table 2. The other operations are generally the same as those in Example 1 and will not be repeated here.

[0087] The reaction time of step S2 is 1 h. At this time, the total cyanide concentration of the effluent is 0.04 mg / L, and the copper ion concentration is 0.43 mg / L.

[0088] Table 2

[0089]

[0090] Example 5

[0091] The difference between Example 5 and Example 1 is that the water quality of the treatment object fluctuates, and its water quality indicators are: total cyanide concentration is 310 mg / L, easily releasable cyanide concentration is 294 mg / L, and copper ion concentration is 523 mg / L.

[0092] During the treatment process, in step S1, the mass ratio of sodium isoVC to total cyanide in the cyanide reduction precipitation agent is 2.5:1, the mass ratio of sodium citrate to copper ion is 1.5:1, and the mass ratio of CaS x The mass ratio of the reaction mixture to the total cyanide was 0.8:1, the reaction time was 2 h, and the other process conditions remained the same.

[0093] The effluent from the deep purification treatment meets the production requirements and can be reused in the front-end production system. The copper oxide content of the refined copper product obtained is 99.3%, which meets the industrial grade standard.

[0094] Example 6

[0095] The total cyanide concentration in the cyanide-containing wastewater of a gold mine is 120 mg / L, the easily releasable cyanide concentration is 115 mg / L, and the copper ion concentration is 223 mg / L.

[0096] S1, adding cyanide-reducing precipitation agent to treat copper-cyanide wastewater, wherein the mass ratio of sodium isoVC to total cyanide is 1.8:1, the mass ratio of sodium citrate to copper ion is 0.9:1, and CaS x The mass ratio to total cyanide is 0.4:1.

[0097] The reaction was stirred thoroughly for 1 h. The mass of the cyanide-reducing precipitate after filtration was 2.8% of the amount of copper-cyanide wastewater treated, and the total cyanide concentration in the treated liquid phase was 0.86 mg / L, and the copper ion concentration was 5.4 mg / L.

[0098] S2, adding a deep purification treatment agent to the overflow liquid obtained in step S1 for treatment; the mass ratio of the added amount of sodium isoVC to the total cyanide is 2.4:1, the mass ratio of the added amount of calcium aluminum sulfate to the copper ion is 1.8:1, and the reaction is carried out for 0.6 h.

[0099] After solid-liquid separation, the total cyanide concentration after liquid phase treatment was 0.14 mg / L, and the copper ion concentration was 0.76 mg / L, which met the reuse requirements.

[0100] S3, drying, grinding, and oxidizing the precipitated slag (the cyanide-reducing precipitated slag obtained in step S1 and the deep purification slag obtained in step S2), and then performing coupled catalytic treatment, wherein the mass ratio of the cyanide-reducing precipitating agent in the slag to the total cyanide is 0.5:1, a composite of manganese oxide and iron oxide is used as a catalyst carrier, and a copper-containing porous material is used as a catalyst. The mass ratio of the oxygen introduced to the precipitated slag is 6.0:1, the temperature in the reactor is 200° C., and the coupled catalytic reaction is performed for 80 minutes to obtain a crude copper product, wherein the copper oxide content is 87.2%.

[0101] S4, eluting the crude copper product: adding the deep treatment liquid obtained in step S2 to wash the crude copper product; the mass ratio of the crude copper product to the deep treatment liquid is 1.0:8.0;

[0102] The mass ratio of sodium isoVC reagent to total cyanide in the slag is 0.25:1, and the copper oxide content in the copper product after water washing is 99.4%.

[0103] The total cyanide concentration in the obtained washing water was 6.87 mg / L, and the copper ion concentration was 0.97 mg / L. It was re-deeply purified by adding deep purification treatment agents and fully reacting for 0.5 h. After treatment, it met the discharge standards.

[0104] Comparative Example 4

[0105] The difference between Comparative Example 4 and Example 6 is mainly that in step S3, in the oxygen-enriched atmosphere oxidation step, the mass ratio of oxygen to precipitated slag is 1.0: 1. Other operations are substantially the same as those in Example 1 and will not be described in detail here.

[0106] Experiments show that after reaction treatment, the purity of the crude copper product is poor, with a copper oxide content of 71.2%. At the same time, after refining, the copper oxide content is only 85.3%.

[0107] The reason is that in the oxygen-rich atmosphere oxidation step, the amount of oxygen introduced into the system is insufficient, and the corresponding oxidizing atmosphere is not created, resulting in insufficient oxidation of the cuprous ions in the slag, leading to a decrease in the copper oxide content in the slag.

[0108] Example 7

[0109] The main difference between Example 7 and Example 6 is that in step S3, the mass ratio of the cyanide-reducing precipitation agent to the total cyanide in the precipitated slag is 0.8:1.

[0110] The results show that a higher purity crude copper product can be obtained, and the oxidizable copper content after refining is 99.8%, which can meet industrial grade standards.

[0111] Example 8

[0112] The main difference between Example 8 and Example 6 is that in step S2, the mass ratio of the added amount of sodium isoVC to the total cyanide is 3.0:1, the mass ratio of the added amount of calcium aluminum sulfate to copper ions is 2.0:1, and the reaction is carried out for 1 h.

[0113] After solid-liquid separation, the total cyanide concentration after liquid phase treatment is 0.05 mg / L, and the copper ion concentration is 0.2 mg / L, which meets the reuse requirements and emission standards, and the device can operate well and stably.

[0114] Example 9

[0115] The total cyanide concentration in the cyanide-containing wastewater of a gold mine is 80 mg / L, the easily releasable cyanide concentration is 75 mg / L, and the copper ion concentration is 123 mg / L.

[0116] S1, adding cyanide-reducing precipitation agent to the cyanide-reducing precipitation reactor to treat the copper-cyanide-containing wastewater; wherein the mass ratio of sodium isoVC to total cyanide is 1.5:1, the mass ratio of sodium citrate to copper ion is 1.0:1, and CaS x The mass ratio to total cyanide is 0.5:1.

[0117] The reaction was stirred thoroughly for 1 h. The mass of the cyanide-reducing precipitate after filtration was 2.5% of the amount of cyanide-containing wastewater treated, and the total cyanide concentration in the treated liquid phase was 1.24 mg / L and the copper ion concentration was 9.6 mg / L.

[0118] S2, the liquid phase of step S1 flows into a deep purification treatment reactor, and a deep purification treatment agent is added into the deep purification treatment reactor. The deep purification treatment agent includes sodium isoVC and calcium aluminum sulfate.

[0119] The mass ratio of the addition amount of sodium isoVC to the total cyanide was 2.3:1, the mass ratio of the addition amount of calcium aluminum sulfate to copper ions was 1.7:1, and the reaction time was 0.8 h.

[0120] After solid-liquid separation, the total cyanide concentration after liquid phase treatment was 0.34 mg / L, and the copper ion concentration was 0.81 mg / L, which met the reuse requirements.

[0121] S3, drying, grinding, and oxidizing in an oxygen-rich atmosphere the cyanide-reducing precipitated residue obtained in step S1 and the deep-purified residue obtained in step S2, and then performing coupled catalytic treatment.

[0122] The mass ratio of the remaining cyanide-reducing precipitation agent in the precipitated slag to the total cyanide is 0.6. The composite of cobalt oxide and nickel oxide is used as a catalyst carrier, and the copper-containing porous material is used as a catalyst. The gas introduced is air, in which the mass ratio of oxygen to total cyanide is 6.0:1. The temperature in the reactor is 200°C, and the coupled catalytic reaction is carried out for 40 minutes to obtain a crude copper product with a copper oxide content of 85.2%.

[0123] S4, eluting the crude copper product: adding the deep treatment liquid obtained in step S2 to wash the crude copper product; the mass ratio of the crude copper product to the deep treatment liquid is 1.0:6.0, the mass ratio of the sodium isoVC reagent to the total cyanide in the slag is 0.3, and the copper oxide content in the copper product after washing is 99%.

[0124] The total cyanide concentration in the obtained washing water was 9.24 mg / L, and the copper ion concentration was 4.38 mg / L. It was re-deeply purified by adding deep purification treatment agents and fully reacting for 0.5 h. After treatment, it met the discharge standards.

[0125] In summary, the method for treating cyanide-containing wastewater in gold mines and regenerating resources provided by the present invention adopts a cyanide-reducing precipitation agent and a deep purification treatment agent to treat the copper-cyanide-containing wastewater in stages, and then obtains a refined copper product after coupled catalysis and process effluent washing. The refined copper product has a main component of copper oxide with a content of more than 99% and can be directly recycled. The method has a good treatment effect on cyanide, can achieve 100% recovery of valuable substances such as copper, and has extremely high added value.

[0126] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for treating cyanide wastewater from a gold mine and regenerating resources, characterized in that: The steps include: S1, cyanide reduction precipitation treatment: adding cyanide reduction precipitation agent to treat copper-cyanide wastewater, stirring to make the agent and water fully mixed, after the reaction is complete, entering the precipitation tank for natural sedimentation, and obtaining cyanide reduction precipitation residue and overflow liquid; wherein the overflow liquid enters step S2 for deep purification treatment, and the cyanide reduction precipitation residue enters step S3 for coupled catalytic treatment; the cyanide reduction precipitation agent includes sodium isoVC, sodium citrate and CaS x The mass ratio of sodium isoVC to total cyanide in the added cyanide reduction precipitation agent is (1.5-3.5):1, the mass ratio of sodium citrate to copper ion is (0.9-1.5):1, and CaS x The mass ratio to total cyanide is (0.4-0.8):1; The total cyanide concentration in the copper-cyanide wastewater is lower than 350 mg / L, the easily releasable cyanide concentration is lower than 300 mg / L, the copper ion concentration is lower than 600 mg / L, and the pH value of the copper-cyanide wastewater is between 7 and 9; S2, deep purification treatment: add deep purification treatment reagent to the overflow liquid obtained in step S1 for treatment, make it fully reacted, and then separate the solid and liquid through the filter to obtain the deep purification slag of the solid phase and the deep treatment liquid of the liquid phase; the deep treatment liquid is discharged or reused in compliance with the standards, and part of the deep treatment liquid enters step S4 to elute the crude copper product after the coupled catalytic treatment; the deep purification treatment reagent includes sodium isoVC and calcium aluminum sulfate; S3, slag coupled catalytic treatment: drying, grinding, and oxidizing in an oxygen-rich atmosphere the cyanide-reduced slag obtained in step S1 and the deep purified slag obtained in step S2, and then subjecting them to coupled catalytic treatment to obtain a crude copper product; S4, return water elution treatment: the crude copper product obtained in step S3 is eluted with the deep treatment liquid obtained in step S2 to obtain a refined copper product. The washing water re-enters step S2 for deep purification treatment and then meets the discharge standards.

2. The method for treating cyanide-containing wastewater in gold mines and regenerating resources according to claim 1, characterized in that: In step S3, the coupled catalytic treatment refers to: using a cyanide-reducing precipitation agent and a deep purification treatment agent to perform coupled catalytic treatment on the cyanide in the cyanide-reducing precipitation slag and the deep purification slag under catalyst-catalyzed reaction conditions, and the reaction time is 30-90 minutes. The thiocyanate and cyanide in the cyanide-reducing precipitation slag and the deep purification slag react with the agent and are destroyed under catalyst-catalyzed conditions.

3. The method for treating cyanide-containing wastewater in gold mines and regenerating resources according to claim 2, characterized in that: In step S3, the mass ratio of the total mass of the cyanide-reducing precipitation agent and the deep purification treatment agent to the total cyanide is (0.5-0.8):

1.

4. The method for treating cyanide wastewater from gold mines and regenerating resources according to claim 3, characterized in that: The cyanide-reducing precipitation slag and deep purification slag contain the remaining cyanide-reducing precipitation agent and deep purification agent in step S1 and step S2; if the mass ratio of the total mass of the remaining cyanide-reducing precipitation agent and deep purification agent to the total cyanide is less than 0.5, the cyanide-reducing precipitation agent is added until the mass ratio of the two is (0.5-0.8):

1.

5. The method for treating cyanide-containing wastewater in gold mines and regenerating resources according to claim 1, characterized in that: In the elution treatment of step S4, the mass ratio of the crude copper product to the deep treatment liquid is 1:(3.0-8.0).

6. The method for treating cyanide wastewater from gold mines and regenerating resources according to claim 5, characterized in that: In step S4, the mass ratio of the deep purification treatment agent to the total cyanide in the deep treatment liquid is (0.2-0.4):1; the deep treatment liquid contains the deep purification treatment agent remaining in step S2; if the mass ratio of the remaining deep purification treatment agent to the total cyanide is less than 0.2, sodium isoVC is added to make the mass ratio of the deep purification treatment agent to the total cyanide (0.2-0.4):

1.

7. The method for treating cyanide wastewater from gold mines and regenerating resources according to claim 2, characterized in that: In step S3, the catalyst carrier is one or a combination of transition metals and their oxides, and the catalyst active ingredient is a copper-containing porous material.

8. The method for treating cyanide wastewater from gold mines and regenerating resources according to claim 1, characterized in that: In step S3, during the oxygen-enriched atmosphere oxidation treatment, the gas introduced is air or oxygen; when oxygen is introduced, the mass ratio of oxygen to precipitated slag is (5.0-7.0):1; the mass of the precipitated slag is the total mass of the cyanide-reducing precipitated slag and the deep purification slag.

Citation Information

Patent Citations

  • Comprehensive treatment method for cuprous cyanide technique waste water

    CN101100328A

  • BR1106426B1

Cited By

  • Coprocessing and copper resource recycling method for copper-containing and cyanide-containing wastewater

    CN122010345A