Chemiluminescent composition as well as preparation method and application thereof
By developing a chemiluminescent composition combining nanoparticles with a core-shell structure and transition metal ions, the problem of magnetic particles' dependence on signal quenching and markers in the existing technology has been solved, and high sensitivity and low cost for exosomes have been achieved. detection, simplifying the operation process.
Patent Information
- Application Number
- CN202310329621.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-01
AI Technical Summary
In existing chemiluminescence detection technology, magnetic particles quench the signal, resulting in reduced detection sensitivity, and markers are often required. The operation is complex and costly, making it difficult to achieve high-sensitivity and low-cost detection of exosomes.
Develop nanoparticles with a core-shell structure. The core is Fe3O4, and the shell is noble metal and transition metal ions. They are combined with the compound of general formula (I) through covalent bonds and coordination bonds to form a chemiluminescent composition for wireless Marker detection.
It improves the intensity and stability of chemiluminescence signal, achieves high-sensitivity and low-cost detection of exosomes, simplifies the operation process, and reduces detection costs.
Smart Images

Figure CN118725846A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of chemiluminescence detection, and more specifically provides a composition that can be used for chemiluminescence detection of biological samples without using a marker, and a preparation method and use thereof. Background Art
[0002] Chemiluminescence is a type of molecular luminescence spectroscopic analysis. It is mainly based on the principle that the concentration of the analyte in the chemical detection system and the chemiluminescence intensity of the system are linearly quantitatively related under certain conditions, and uses instruments to detect the chemiluminescence intensity of the system to determine the content of the analyte. Chemiluminescence is widely used in trace metal ions, various inorganic compounds, organic compound analysis and biological fields. However, the chemiluminescence reagents currently used in chemiluminescence, especially the reagents used for label-free chemiluminescence detection, often have many defects in various aspects. For example, it is known in the prior art that if magnetic particles are used in chemiluminescence reagents, it will inevitably cause a significant quenching effect on the chemiluminescence signal, significantly reduce the intensity of the chemiluminescence signal, and thus make the detection sensitivity worse. In order to overcome the above problems, people adopt the practice of adding modifiers or catalysts in the chemiluminescence, but the addition of these modifiers or catalysts will significantly hinder the further connection of other recognition elements (such as antibodies, aptamers, etc.), and the chemiluminescence reagents developed in the prior art are also often prone to agglomeration and leakage loss, resulting in instability of the chemiluminescence system, which has a serious adverse effect on the performance of chemiluminescence analysis. Therefore, people still hope to develop a novel chemiluminescent system that can overcome the above-mentioned problems existing in the prior art, and especially hope that the chemiluminescent magnetic particles therein have excellent chemiluminescent properties, sufficient binding sites and good stability.
[0003] In addition, exosomes are nanoscale extracellular vesicles secreted by living cells, with a size of about 30-150nm. They are information molecules used for intercellular communication, carrying important molecular information of parent cells, such as proteins, nucleic acids, lipids, etc., and stably exist in body fluids such as blood, urine, saliva, and lymph. In recent years, it has been reported that exosomes produced by tumors play a very important role in tumor proliferation, metastasis, invasion, and drug resistance. People regard them as potential biomarkers for cancer diagnosis and can be used as non-invasive diagnostic objects in clinical diagnosis. If new technologies with high sensitivity, convenience, and low cost can be developed for exosomes, it will be of great value for the diagnosis, treatment effect monitoring, and efficacy prediction of tumor patients. In recent years, people have tried to use various technologies to detect exosomes, such as nanoparticle tracking analysis, protein immunoblotting technology, enzyme-linked immunosorbent assay, fluorescence, colorimetry, electrochemical method, surface enhanced Raman scattering, chemiluminescence, etc. Among them, chemiluminescence technology has the advantages of wide linear range, high sensitivity, and low cost, and is considered to be a technology with practical value for detecting exosomes. However, due to the defects of chemiluminescence technology in this application, most of the chemiluminescence detection tests for exosomes to date have to be based on labeling technology, which inevitably brings problems such as high operational complexity, high cost, and slow detection speed. Therefore, people also hope to develop a novel method for detecting exosomes, which can achieve low cost, simple operation, no need for labeling, and has excellent sensitivity to exosomes. Summary of the invention
[0004] In response to the existing technical problems, the inventors of the present invention invested a lot of energy and resources in research and successfully developed a novel chemiluminescent composition, in which the problems existing in the prior art were successfully overcome by developing a nanoparticle with a core-shell structure, while retaining or even further improving the beneficial effects of the prior art, thereby completing the present invention.
[0005] A first aspect of the present invention provides a chemiluminescent composition comprising:
[0006] (i) a nanoparticle having a core-shell structure, the core-shell structure comprising at least one core and at least one shell, the core comprising Fe3O4, the shell comprising at least one noble metal selected from the group consisting of gold, silver, ruthenium, rhodium, palladium, osmium, iridium and platinum;
[0007] (ii) transition metal ions; and
[0008] (iii) a compound of the general formula (I),
[0009]
[0010] Among them, the A ring represents C6-C 14 Aromatic rings;
[0011] R1 and R2 independently represent hydrogen, the terminal group is substituted by amino or is an unsubstituted straight chain or branched chain (C1-C 30 )alkyl, provided that the -NR1R2 moiety has at least one NH2 terminal group.
[0012] The second aspect of the present invention provides a method for preparing the chemiluminescent composition of the present invention, the method comprising the steps of:
[0013] 1) applying one or more shells containing precious metals on the surface of Fe3O4 particles to form nanoparticles with a core-shell structure;
[0014] 2) combining the nanoparticles having a core-shell structure with the transition metal ions and the compound of the general formula (I) to form the chemiluminescent composition.
[0015] A third aspect of the present invention provides a method for qualitative or quantitative analysis of an analyte, the method comprising the following steps:
[0016] Step 1: mixing a sample containing an analyte with the composition of the present application to obtain an analyte system, and optionally adding an additive before, during or after step 1, wherein the additive is selected from one or more of a pH adjuster, a pH buffer, an oxidant, a reductant, a stabilizer, a bactericide, a preservative, a chelating agent, and a complexing agent;
[0017] Step 2: using a sensor to detect the light emitted by the above analyte system;
[0018] The method does not involve labeling of the analyte. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In the following paragraphs, various embodiments of the present invention are discussed in conjunction with the accompanying drawings. However, it should be noted that the embodiments shown in the accompanying drawings and described in detail below are only some preferred embodiments of the present invention, and the protection scope of the present invention is defined by the claims, but not limited to these preferred embodiments.
[0020] Figure 1 A synthesis flow chart according to one embodiment of the present application is shown;
[0021] Figure 2 A schematic diagram of a process for preparing a CL immunosensor according to one embodiment of the present application and using the CL immunosensor to detect exosomes is shown;
[0022] FIG. 3A to FIG. 3D TEM images of aminated Fe3O4 magnetic particles, Fe3O4@Au, Fe3O4@Au / Ag and bfCL-Fe3O4@Au / Ag according to some embodiments of the present application are shown respectively;
[0023] Figure 4 The element mapping image of bfCL-Fe3O4@Au / Ag prepared in Example 1 is shown;
[0024] Figure 5 The fluorescence spectra of ABEI, Fe3O4@Au / Ag and bfCL-Fe3O4@Au / Ag according to some embodiments of the present application are shown, and the excitation wavelength is 270nm;
[0025] Fig. 6A The full-spectrum XPS spectra of aminated Fe3O4 magnetic particles, Fe3O4@Au, Fe3O4@Au / Ag and bfCL-Fe3O4@Au / Ag according to some embodiments of the present application are shown; Figures 6B to 6E The deconvoluted XPS spectra of Au 4f, Ag3d, N 1s, and Co 2p in bfCL-Fe3O4@Au / Ag are shown respectively;
[0026] Figure 7 The ζ points of different samples are shown, where (a) represents aminated Fe3O4 magnetic particles, (b) represents Fe3O4@Au, (c) represents Fe3O4@Au / Ag, and (d) represents bfCL-Fe3O4@Au / Ag;
[0027] Figure 8 The saturation magnetization curve of bfCL-Fe3O4@Au / Ag prepared in Example 1 is shown. Figure 8 The two inserted small figures show the photos of bfCL-Fe3O4@Au / Ag suspension before (left) and after (right) applying an external magnetic field.
[0028] Fig. 9 Characterization of dispersion stability of aqueous dispersions of various materials is shown;
[0029] FIG. 10A to FIG. 10C The CL properties of bfCL-Fe3O4@Au / Ag prepared in Example 1 and the comparative samples are shown;
[0030] Fig. 10D It shows the change of CL signal of bfCL-Fe3O4@Au / Ag prepared in Example 1 over time;
[0031] Fig.11A The effect of pH on CL performance is shown. Fig. 11BThe effect of H2O2 concentration on CL performance is shown;
[0032] Figures 12A to 12E TEM images of samples prepared using different nitrate dosages are shown;
[0033] Fig.12F Shows Figures 12A to 12E CL properties of samples with different silver shell thicknesses are shown;
[0034] Fig.13A The relationship between BSA solution treatment time and CL properties is shown. Fig. 13B The relationship between exosome culture time and CL properties is shown;
[0035] Fig.14A The relationship between the CL intensity of the bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA / exosome complex and the logarithm of the exosome concentration is shown;
[0036] Fig. 14B The CL intensity of different interfering proteins and their effects on the CL intensity of bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA / exosome complex are shown;
[0037] Fig.15 The changes in CL intensity of bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA / exosome complex over time are shown. DETAILED DESCRIPTION
[0038] "Range" disclosed herein is in the form of lower limit and upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges that can be defined in this way are inclusive and combinable, i.e. any lower limit can be combined with any upper limit to form a range. For example, a range of 60-120 and 80-110 is listed for a particular parameter, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5.
[0039] In the present invention, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" have been listed in this document, and "0-5" is just an abbreviation of these numerical combinations.
[0040] In the present invention, if there is no special description, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution. In the present invention, if there is no special description, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0041] In the present invention, unless otherwise specified, the term "comprising" mentioned herein may be open-ended or closed-ended. For example, the term "comprising" may mean that other components not listed may also be included, or may only include the listed components.
[0042] The chemiluminescent composition of the present invention is described in detail below in conjunction with some embodiments of the present invention.
[0043] According to one embodiment of the present application, in the composition of the present application, the nanoparticles, transition metal ions and the compound of the general formula (I) are directly or indirectly bonded to each other through covalent bonds and / or coordination bonds, rather than simply physically mixed. For example, according to an exemplary embodiment, the nanoparticles, transition metal ions and the compound of the general formula (I) are directly or indirectly bonded to each other through one or more of the following groups: amino, amine, hydroxyl, carboxyl, amide, thiol, etc. According to an exemplary embodiment, the nanoparticles, transition metal ions and the compound of the general formula (I) are directly or indirectly combined / bonded through coordination bonds and / or covalent bonds between metal-amino groups and / or metal ion-amino groups.
[0044] According to one embodiment of the present application, the core of the nanoparticles may be Fe3O4 nanoparticles, for example, the particle size thereof may be 20-500 nanometers, for example, 30-450 nanometers, or 50-400 nanometers, or 60-350 nanometers, or 80-300 nanometers, or 100-250 nanometers, or 120-220 nanometers, or 150-200 nanometers, or 150-180 nanometers, or may be within the numerical range obtained by combining any two of the above end values. In the present application, for the purpose of simplicity, Fe3O4 nanoparticles are referred to as Fe3O4MB, where "MB" means "magnetic beads".
[0045] According to another embodiment of the present application, the surface of the Fe3O4 nanoparticles as the core can be functionalized with one or more functional groups to improve the efficiency of the subsequent application of the precious metal shell layer on the surface of the Fe3O4 nanoparticles. The functional groups on the surface of the Fe3O4 nanoparticles can be selected from one or more of the following: hydroxyl, amino, (C1-C12) hydroxyalkyl, (C1-C12) alkylamino, carboxyl, sulfonic acid, thiol, amide, etc. According to an exemplary embodiment, the surface of the Fe3O4 nanoparticles is aminated. In the present application, "aminated" means that the surface of the Fe3O4 nanoparticles is functionalized with amino or (C1-C12) alkylamino (i.e., amine).
[0046] According to another embodiment of the present application, there may be one, two, three, four, five or six shell layers surrounding the core Fe3O4 nanoparticles in sequence, and the thickness of each shell layer may be 1-200 nanometers, for example, 1.5-150 nanometers, or 2-120 nanometers, or 2.5-100 nanometers, or 3-90 nanometers, or 3.5-80 nanometers, or 4-70 nanometers, or 4.5-60 nanometers, or 5-50 nanometers, or 5.5-40 nanometers, or 6-30 nanometers, or 6.5-20 nanometers, or 7-15 nanometers, or 7.5-10 nanometers, or 8-9 nanometers, or within the numerical range obtained by combining any two of the above end values. In the present application, each shell layer may completely cover the Fe3O4 nanoparticles or the shell layer previously deposited on the Fe3O4 nanoparticles, or may partially cover them. For example, the coverage rate achieved by each of the above shell layers (based on the surface area of the Fe3O4 nanoparticles or the shell layer previously deposited on the Fe3O4 nanoparticles) may be 10-100%, or 20-100%, or 30-100%, or 40-100%, or 50-100%, or 60-100%, or 70-100%, or 80-100%, or 90-100%, or 95-100%, or 98-100%, or the coverage rate may be within the numerical range obtained by combining any two of the above end values.
[0047] According to another embodiment of the present application, the core-shell structure includes a core, a first shell surrounding the core, and a second shell surrounding the first shell, the core includes Fe3O4, the first shell includes at least one precious metal selected from the following: gold, silver, ruthenium, rhodium, palladium, osmium, iridium and platinum, preferably gold; the second shell includes at least one precious metal selected from the following: gold, silver, ruthenium, rhodium, palladium, osmium, iridium and platinum, preferably silver; and the precious metal in the first shell is different from the precious metal in the second shell, preferably the first shell includes gold, and the second shell includes silver. According to one embodiment of the present application, the thickness of the second shell is greater than the thickness of the first shell. According to one embodiment of the present application, the thickness of the first shell portion is approximately 1-20 nanometers, for example 1.5-10 nanometers; and the thickness of the second shell portion is approximately 5-100 nanometers, or 8-90 nanometers, or 10-80 nanometers, or 20-70 nanometers, or 30-60 nanometers, or 40-50 nanometers; and the thickness of the second shell portion is greater than the thickness of the first shell portion.
[0048] According to one embodiment of the present application, the metals in the first shell and the second shell are both present in a valence state of 0. According to another embodiment of the present application, the first shell is elemental gold (valence state 0), and the second shell is elemental silver (valence state 0).
[0049] According to an exemplary embodiment of the present application, the nanoparticles include a core composed of Fe3O4, a first shell composed of elemental gold, and a second shell composed of elemental silver. In the present application, for the purpose of simplicity and convenience, the nanoparticles having such a structure and elemental composition are written as Fe3O4@Au / Ag. In addition, the material including a core composed of Fe3O4 and a first shell composed of elemental gold is abbreviated as Fe3O4@Au.
[0050] In the present application, the first shell and the second shell can be formed by reducing the soluble salt of the corresponding noble metal in the dispersion system in which the core is present; or the soluble salt of the corresponding noble metal can be first reduced to form noble metal nanoparticles, and then the dispersion of the core is mixed therewith, so that the newly formed noble metal nanoparticles are deposited on the core particles, thereby forming the first shell or the second shell. For example, the soluble salt of the noble metal can include nitrates, chlorates, cyanates, ammonia complexes, etc. of these noble metals, for example, examples thereof can include gold chlorate, silver nitrate, etc., and can also include hydrated salts thereof. The reduction can be carried out using various reducing agents, for example, the reducing agent can include one or more of the following: sodium borohydride, lithium aluminum hydride, formaldehyde, etc.
[0051] According to one embodiment of the present application, the transition metal ion is selected from the following group: Co 2+ 、Ni 2+ , Fe 3+ , Fe 2+ Cr 3+ , Cu 2+ , preferably Co 2+ According to one embodiment of the present invention, the transition metal ions are derived from soluble salts thereof, including but not limited to chlorides, sulfates, nitrates, phosphates, sulfites, etc. and combinations thereof.
[0052] In the present application, the compound of the general formula (I) has the structure shown below,
[0053]
[0054] Among them, the A ring represents C6-C 14 Aromatic ring; R1 and R2 independently represent hydrogen, the terminal group is substituted by amino or is an unsubstituted straight or branched chain (C1-C 30 ) alkyl, provided that the -NR1R2 portion has at least one NH2 terminal group. According to a preferred embodiment of the present invention, the A ring represents a C6-C 10 The aromatic ring is preferably a benzene ring, a naphthalene ring or an anthracene ring, and the R1 and R2 may independently represent hydrogen, the terminal groups may be substituted by amino groups, or may be unsubstituted straight or branched chains (C1-C 10 )alkyl, preferably the terminal group is substituted by amino or is an unsubstituted straight or branched (C1-C6)alkyl, provided that the -NR1R2 part has at least one NH2 terminal group. According to another preferred embodiment of the present invention, in the compound of general formula (I), ring A is a benzene ring or a naphthalene ring, and the -NR1R2 part is an amino group or N-(aminoC1-C6 alkylene)N-(C1-C6 alkyl)amino group. According to another preferred embodiment of the present invention, ring A is a benzene ring, and the -NR1R2 part is an amino group, N-(4-aminobutyl)N-(ethyl)amino group or (N-4-aminohexyl) (N-ethyl)amino group. According to a more preferred embodiment of the present invention, the compound of formula (I) has the structure shown in the following formulas (II), (III), and (IV):
[0055]
[0056] According to one embodiment of the present application, the CL composition of the present application can be formed by combining Fe3O4@Au / Ag nanoparticles with an aqueous solution of a transition metal and a compound of formula (I), so that the three are covalently bonded and / or coordinately bonded to each other. In the present application, for the purpose of simplicity, the chemiluminescent composition of the present invention formed by combining the above three components is written as bfCL-Fe3O4@Au / Ag, where "bf" means bi-functionalized, and "CL" means chemiluminescence, and bfCL-Fe3O4@Au / Ag also means bifunctionalized chemiluminescent Fe3O4@Au / Ag.
[0057] According to one embodiment of the present application, in the CL composition, the mass ratio of nanoparticles to transition metal ions is 100:1-1:20, for example, 90:1-1:19, or 85:1-1:15, or 80:1-1:12, or 70:1-1:11, or 60:1-1:10, or 50:1-1:10, or 40:1-1:10, or 30:1-1:10, or 20:1-1:10, or 18:1-1:9, or 16:1-1:8, or 15:1-1:7, or 14:1-1:6, or 12:1-1:4, or 11:1-1:2, or 10:1-1:1, or 9:1-2:1, or The mass ratio of the nanoparticles to the compound of formula (I) is 8:1-3:1, or 7:1-4:1, or 6:1-5:1, or within the range of values obtained by combining any two of the above end values. According to another embodiment of the present application, in the CL composition, the mass ratio of the nanoparticles to the compound of formula (I) is 20:1-1:10, for example, 18:1-1:9, or 16:1-1:8, or 15:1-1:7, or 14:1-1:6, or 12:1-1:4, or 11:1-1:2, or 10:1-1:1, or 9:1-2:1, or 8:1-3:1, or 7:1-4:1, or 6:1-5:1, or within the range of values obtained by combining any two of the above end values.
[0058] According to one embodiment of the present application, before the CL composition of the present application is used to analyze the object to be tested, one or more other functional components may be linked to it, and the functional components may include specific antigens or antibodies for the object to be tested. For example, according to an exemplary embodiment of the present application, the object to be tested may be an exosome, such as an exosome contained in a body fluid sample of a healthy person or a cancer patient. According to another embodiment of the present application, the functional component may be an antigen or antibody specific to exosomes. For example, in the case where the exosomes in the rabbit body fluid sample are the detection object, examples of the antigens or antibodies used may include, for example, rabbit anti-transmembrane tetramer protein family antibodies (CD63-Ab, CD9-Ab, CD81-Ab), rabbit anti-programmed cell death ligand 1 antibody (PD-L1-Ab) and rabbit anti-epidermal growth factor receptor antibody (EGFR-Ab), and when the object to be tested is an exosome in a body fluid sample from other species of mammals such as humans, monkeys, dogs, mice, etc., specific antigens or antibodies for exosomes of humans, monkeys, dogs, mice or other mammals may also be used. According to one embodiment of the present application, the mass ratio of the CL composition to the specific antigen or antibody is 50:1 to 10:1, for example, 48:1 to 11:1, or 45:1 to 12:1, or 42:1 to 15:1, or 40:1 to 18:1, or 35:1 to 20:1, or 32:1 to 22:1, or 30:1 to 25:1, or 28:1 to 26:1, or within the numerical range obtained by combining any two of the above end values. According to an exemplary embodiment, the product obtained after Fe3O4@Au / Ag is combined with a certain antibody or antigen is abbreviated as Fe3O4@Au / Ag / antibody or Fe3O4@Au / Ag / antigen. For example, when CD63-Ab antibody is used, the obtained product is written as Fe3O4@Au / Ag / CD63-Ab.
[0059] According to another embodiment of the present application, the functional component may include a site blocker, which is used to block the non-specific linking sites on the surface of the CL composition of the present application, such as bfCL-Fe3O4@Au / Ag, to improve its selective CL test for the target test object. An example of the site blocker includes bovine serum albumin (BSA), skim milk powder, casein, etc. According to one embodiment of the present application, the mass ratio of the CL composition, such as bfCL-Fe3O4@Au / Ag, to the site blocker is 200:1 to 10:1, for example, the mass ratio may be 190:1 to 12:1, or 180:1 to 15:1, or 170:1 to 20:1, or 160:1 to 30:1, or 150:1 to 40:1, or 140:1 to 50:1, or 130:1 to 60:1, or 120:1 to 70:1, or 110:1 to 80:1, or 100:1 to 90:1, or may be within the numerical range obtained by combining any two of the above end values. According to an exemplary embodiment of the present application, a CL composition that has been combined with a specific antigen / antibody and the above-mentioned blocking agent can be written as CL composition / antigen (antibody) / blocking agent, an example of which includes bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA.
[0060] According to another embodiment of the present application, before the CL composition of the present application, such as bfCL-Fe3O4@Au / Ag, is used for CL detection of exosomes, one or more additives may be added thereto. For example, the additive may be selected from one or more of a pH adjuster, a pH buffer, an oxidant, a reductant, a stabilizer, a bactericide, a preservative, a chelating agent, and a complexing agent.
[0061] According to an exemplary embodiment, the CL composition of the present application, such as bfCL-Fe3O4@Au / Ag, is successively combined with an exosome-specific antigen (or antibody) and a blocking agent as described above to obtain a CL composition / antigen (antibody) / blocking agent, which is then mixed with a sample containing exosomes to combine with the exosomes in the sample to form a CL composition / antigen (antibody) / blocking agent / exosomes (an example of which includes bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA / exosomes), and hydrogen peroxide (aqueous solution of H2O2) is added thereto to generate a CL signal, and the CL signal is detected using a detector, and the exosomes in the sample are qualitatively or quantitatively analyzed based on the detection result.
[0062] Example
[0063] In the following examples, the chemiluminescent composition of the present invention is prepared and its performance is characterized, and the performance of the chemiluminescent composition is compared with that of the existing chemiluminescent composition in the prior art. The following examples are only specific examples listed in this application, but the technical features of this application are not limited thereto. Any simple changes, equivalent substitutions or other modifications made based on this application to solve basically the same technical problems and achieve basically the same technical effects are all covered within the scope of protection of this application.
[0064] The following chemical reagents and materials were used in the following examples: The aminated Fe3O4 magnetic particles (MB) used as raw materials in the examples were purchased from Biomag Technology Co., Ltd., with an average particle size of about 150 nm; halogenated acid tetrahydrate (HAuCl4·4H2O), sodium citrate (Na3Cit), sodium borohydride (NaBH4), silver nitrate (AgNO3), formaldehyde (HCHO, about 38.0%), ammonia (NH3·H2O, 28.0%), sodium hydroxide (NaOH), hydrogen peroxide (30.0%) and cobalt chloride hexahydrate (CoCl2·6H2O) were purchased from Sinopharm Chemical Reagent Co., Ltd. (Shanghai, China). ABEI was purchased from Tokyo Chemical Industry Co., Ltd. (TCI), Japan, and the ABEI solution was prepared by dissolving ABEI in a 0.1M NaOH aqueous solution, and the ABEI solution was stored at 4°C. Bovine serum albumin (BSA) was purchased from Solarbio Technology Co., Ltd. (Beijing). 5,5-dimethyl-1-pyrroline-N-oxide (DMPO) was purchased from Dongren Chemical Technology (Shanghai) Co., Ltd. Phosphate buffered saline (PBS) buffer (pH 7.4), human immunoglobulin M (hIgM), human CD63 protein, human α-fetoprotein (AFP), human epidermal growth factor receptor 2 (HER2) and CD63-Ab were purchased from Sangon Biotechnology (Shanghai) Co., Ltd. Human lung cancer cell line (A549) was purchased from Wuhan Punosai Life Science Technology Co., Ltd. All reagents used in the examples were analytical grade. Ultrapure water prepared by the Milli-Q system (Milli-pore, France) was used in the experiments.
[0065] Example 1: Preparation and characterization of bfCL-Fe3O4@Au / Ag
[0066] Example 1 According to Figure 1 The synthetic flow chart shown in Figure 2 shows that bfCL-Fe3O4@Au / Ag was synthesized by a three-step method.
[0067] The first step is to apply the first shell of gold nanoparticles (AuNP) (Fe3O4@Au) on the aminated Fe3O4 magnetic particles (MB). Specifically, 1 mL of HAuCl4 aqueous solution with a concentration of 25 mM and 5 mL of Na3Cit aqueous solution with a concentration of 5 mM were added to 90 mL of deionized water, and the mixture was vigorously stirred. Then 2.5 mL of the just prepared NaBH4 solution with a concentration of 0.1 M was added thereto, and the color of the mixed solution was observed to change from colorless to orange after the addition. The mixed solution was then stirred at room temperature for 4 hours to obtain spherical AuNPs with a particle size of about 4 nm. 1 mg of aminated Fe3O4 magnetic particles was washed twice with ultrapure water and dispersed in 1 mL of ultrapure water. Then 3 mL of the AuNP suspension prepared above was added to the Fe3O4 magnetic particle suspension, the mixture was vigorously shaken for 2 minutes, and then transferred to a shaker and kept shaking at a temperature of 25°C to continue the reaction overnight. The Au-shelled Fe3O4 magnetic particles thus synthesized, hereinafter referred to as Fe3O4@Au, were washed three times with ultrapure water and stored at 4°C for subsequent applications.
[0068] The second step is to apply a second shell of silver on Fe3O4@Au. Specifically, 2 mg of Fe3O4@Au obtained in the first step was added to 20 mL of ultrapure water and subjected to ultrasonic treatment for 5 minutes to disperse it. Then, 1.2 mL of a 10 mM AgNO3 aqueous solution and 0.6 mL of a 10 mM Na3Cit aqueous solution were added thereto under vigorous stirring, and then about 40 μL of ammonia water was added thereto to adjust the pH value of the mixture to pH = 10. Then, a mixture of 0.4 mL of formaldehyde solution, 0.4 mL of water and 9.2 mL of ethanol was added dropwise thereto. The color of the mixture changed from orange to silver gray, and the product obtained in this step had a core including internally aminated Fe3O4 magnetic particles (MB), a first shell (gold) coated on the core, and a second shell (silver) coated on the first shell, which is written as Fe3O4@Au / Ag in this application.
[0069] The third step is to combine the transition metal and ABEI with the Fe3O4@Au / Ag synthesized in the second step above. Specifically, 0.1 mL of 5 mM CoCl2·6H2O aqueous solution and 0.2 mL of 4 mM ABEI aqueous solution were added to 1 mL of the Fe3O4@Au / Ag suspension prepared in the second step above, and the suspension was shaken on an oscillator for 3 hours. The solid material in the solution was then magnetically separated four times using a magnetic device (the device and operation method used in the magnetic separation step are described in detail below), and the separated solid material was dispersed in 1 mL of ultrapure water. The bifunctionalized chemiluminescent Fe3O4@Au / Ag was prepared by the above steps, hereinafter referred to as bfCL-Fe3O4@Au / Ag, which was stored at 4°C for subsequent characterization and application.
[0070] The bfCL-Fe3O4@Au / Ag prepared in Example 1 was characterized using the following techniques.
[0071] TEM images of the samples were obtained using a Talos F200X electron microscope (FEI). The Co in bfCL-Fe3O4@Au / Ag was determined by ICP-AES technique using an Optima 7300 DV plasma atomic emission spectrophotometer (PerkinElmer Instruments, Inc., PerkinElmer). 2+Concentration. XPS data were tested using a Thermo ESCALAB 250Xi electron spectrometer (VG Scientific, East Grinstead, UK), which uses Al Kα radiation as an X-ray source. The zeta potential was measured using an interface potential analyzer (Nano ZS90 Zetasizer, Malvern Instruments, Malvern, UK). The hysteresis loop of bfCL-Fe3O4@Au / Ag was determined using a vibrating sample magnetometer (Quantum Design Inc.). The CL spectrum was measured using a self-assembled chemiluminescence (CL) spectrum acquisition system, which consisted of a SpectraPro HRS-300 (Princeton, USA), which was equipped with a DU971P-BVF EMCCD detector (Andor, UK). Fluorescence spectra were measured using a fluorescence spectrometer (F-7000, Hitachi, Japan). The free radicals in the reaction of bfCL-Fe3O4@Au / Ag with H2O2CL were measured using an electron spin resonance spectrometer (ESR) (JES-FA200, JEOL, Japan), and the CL intensity was measured using a microplate chemiluminescence detector (LUMIstarOmega, BMGLABTECH, Ortenberg, Germany).
[0072] Chemiluminescence (CL) tests were performed in the following general manner: To study the CL properties of the material, a microplate with 96 wells was used, 100 μL of the bfCL-Fe3O4@Au / Ag suspension prepared as described above was added to each well, and then 100 μL of a solution of 1 mM H2O2 dissolved in 0.01 M NaOH aqueous solution was injected into each well at a gain of 2200 (for dissolved oxygen saturation experiments, CL intensity was measured at a gain of 2000). While injecting the H2O2 solution, the CL kinetic curve was recorded using a microplate chemiluminescence detector.
[0073] Example 2: Preparation of label-free CL immunosensor and testing of exosomes
[0074] In this Example 2, bfCL-Fe3O4@Au / Ag prepared in Example 1 was used to prepare a CL immunosensor, and exosomes were detected using the CL immunosensor.
[0075] First, cell culture and isolation of exosomes to be tested were performed according to the following steps: A549 cells were cultured in DMEM medium containing 10% FBS and 1% penicillin / streptomycin in an incubator at 5% CO2 and 37°C. When the cells covered about 30% of the bottom of the bottle, the cells were cultured in DMEM medium containing 10% exosome-free FBS and 1% penicillin / streptomycin for another 48 hours. The supernatant of the culture solution was collected and centrifuged at 4°C to obtain exosomes, and the centrifugation operation included: first centrifuging at 300g for 10 minutes, then centrifuging at 1000g for 10 minutes to remove cells, and then centrifuging at 10,000g for 30 minutes to remove cell debris. The supernatant was then filtered through a 0.22μm filter and then centrifuged at 100,000g for 70 minutes to obtain small exosome particles. The exosome pellets were washed with PBS and centrifuged again at 100,000 g for 70 minutes. The exosome pellets were finally dissolved in PBS and stored at -80°C for later use.
[0076] Exosomes were characterized and quantified by dropping 10 μL of the exosome suspension prepared from A549 cells as described above onto a copper grid, leaving it for 1 minute, and blotting the floating solution on the copper grid with filter paper. 2% uranyl acetate was dropped onto the copper grid and left for 1 minute. The solution was blotted with filter paper, dried in air, and TEM micrographs were taken at 120 kV using a transmission electron microscope. nFCM was used to record the particle size distribution and particle concentration of the exosomes prepared from A549 cells.
[0077] according to Figure 2 The label-free CL immunosensor for detecting exosomes was prepared as shown in the schematic diagram, and the label-free CL immunosensor was used to detect exosomes. The specific steps are as follows: First, prepare 1 mL of the aqueous suspension of bfCL-Fe3O4@Au / Ag prepared in Example 1 with a concentration of mg / mL, add 25 μL of the aqueous dispersion of CD63-Ab with a concentration of 1.2 mg / mL, and continue to react at 25°C in an oscillator for 1 hour. The resulting material was magnetically separated and washed with 0.01 M PBS buffer (pH 7.4). The sample was treated in a 1% BSA solution for 10 minutes to block the nonspecific binding sites in the sample, and bfCL-Fe3O4@Au / Ag combined with CD63-Ab and BSA was obtained, which will be referred to as bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA in the following text. The exosomes described above were diluted to different concentrations (3.1×10 3 to 3.1×10 8Particles / ml), 120 μL of each exosome sample was mixed with 120 μL of the bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA suspension prepared as described above, and gently shaken at 37°C for 10 minutes. The product was then washed with ultrapure water and dispersed in 480 μL of PBS buffer. The product obtained was a complex of exosomes and bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA, which is hereinafter referred to as bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA / exosome complex. Finally, 100 μL of the dispersed bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA / exosome complex suspension was added to each well of the microplate using a pipette, and then 100 μL of a 1 mM H2O2 solution in 0.01 M NaOH was injected into each well. After adding the above hydrogen peroxide solution, the CL kinetic curve of each well was immediately recorded using a microplate chemiluminescence detector.
[0078] The characterization results of the products and intermediates obtained in Examples 1-2 are as follows:
[0079] FIG. 3A to FIG. 3D TEM images of aminated Fe3O4 magnetic particles, Fe3O4@Au, Fe3O4@Au / Ag, and bfCL-Fe3O4@Au / Ag are shown, respectively. Figure 3A It shows that the diameter of the aminated Fe3O4 magnetic particles is about 150 nm; Figure 3B It shows that Au nanoparticles are uniformly arranged on the surface of aminated Fe3O4 magnetic particles to form a first Au shell layer, and the overall diameter of Fe3O4@Au is about 157nm; Figure 3C It shows that a Ag shell is formed on the outer surface of Fe3O4@Au, and the diameter of Fe3O4@Au / Ag is about 199nm; Figure 3D It shows that the combination of ABEI and Co 2+ Afterwards, the morphology of the particle surface did not change.
[0080] Figure 4 The mapping images of different elements of bfCL-Fe3O4@Au / Ag prepared in Example 1 are shown, which show that Fe, N, Au, Ag and Co are uniformly distributed on the surface, indicating that Au, Ag, Co 2+ All are evenly applied on the aminated Fe3O4 magnetic particles located in the core.
[0081] Figure 5The fluorescence spectra of ABEI as raw material in Example 1, the intermediate product Fe3O4@Au / Ag prepared in Example 1, and the final product bfCL-Fe3O4@Au / Ag prepared in Example 1 are shown, and the excitation wavelength is 270nm. The comparison shows that ABEI has been combined in bfCL-Fe3O4@Au / Ag prepared in Example 1.
[0082] Fig. 6A The full XPS spectra of the aminated Fe3O4 magnetic particles used as raw materials in Example 1, the intermediate products Fe3O4@Au and Fe3O4@Au / Ag prepared in Example 1, and the final product bfCL-Fe3O4@Au / Ag prepared in Example 1 are shown; Figures 6B to 6E The deconvoluted XPS spectra of Au 4f, Ag 3d, N 1s and Co 2p in the final product bfCL-Fe3O4@Au / Ag prepared in Example 1 are shown respectively. Fig. 6A It shows that the signals of Au, Ag and Co elements appear in sequence during the synthesis process of Example 1, which indicates that Au, Ag and Co are applied in sequence on the surface of the aminated Fe3O4 magnetic particles. 2+ .in addition Figure 6B It shows that Au exists in bfCL-Fe3O4@Au / Ag with a valence of 0. Figure 6C This indicates that Ag exists in bfCL-Fe3O4@Au / Ag with zero valence. Fig.6D Indicates Co 2+ It binds to the surface of the Ag shell via Co-N coordination. Fig. 6E This indicates that Co 2+ It coordinates with the Fe3O4@Au / Ag surface and combines with the amino group of ABEI to finally obtain bfCL-Fe3O4@Au / Ag.
[0083] Figure 7 The zeta potential of different samples is shown, where (a) represents the aminated Fe3O4 magnetic particles used as raw materials in Example 1, (b) represents the intermediate product Fe3O4@Au obtained in Example 1, (c) represents the intermediate product Fe3O4@Au / Ag obtained in Example 1, and (d) represents the final product bfCL-Fe3O4@Au / Ag obtained in Example 1. (a) is a Fe3O4 magnetic particle, and its zeta potential is +16.83mV, which becomes -11.14mV after applying gold. After further applying a silver shell, the zeta potential of Fe3O4@Au / Ag becomes -13.27mV, and after applying Co 2+After ABEI, the zeta potential of bfCL-Fe3O4@Au / Ag becomes +27.45mV. The above results show that bfCL-Fe3O4@Au / Ag was successfully synthesized in Example 1. In addition, ICP-AES experiments proved that Co 2+ is 0.013 mg / mL, and the bfCL-Fe3O4@Au / Ag and Co 2+ The mass ratio is 77:1.
[0084] Based on the above characterization results, it can be determined that bfCL-Fe3O4@Au / Ag was successfully synthesized in Example 1.
[0085] The magnetic properties of bfCL-Fe3O4@Au / Ag prepared in Example 1 were studied at room temperature. Figure 8 The saturation magnetization curve of bfCL-Fe3O4@Au / Ag is shown. Figure 8 The two inserted small figures show the photos of bfCL-Fe3O4@Au / Ag suspension before (left) and after (right) applying an external magnetic field. Figure 8 As shown in Figure 2, the saturation magnetization value of bfCL-Fe3O4@Au / Ag is 55.98emu / g, indicating that it has superparamagnetism. Figure 8 As can be seen from the inset picture, when a magnetic field is applied to one side of the glass vial containing the bfCL-Fe3O4@Au / Ag suspension, the bfCL-Fe3O4@Au / Ag nanoparticles will quickly and tightly gather on one side of the glass vial, so that they can be easily separated. The magnetic separation mentioned in the above Example 1 is carried out in this way. This proves that the bfCL-Fe3O4@Au / Ag synthesized in claim 1 of the present application has excellent potential for use as a biological experimental analysis platform.
[0086] Example 3: Analysis of dispersion stability of the product obtained in Example 1
[0087] In this embodiment, the aminated Fe3O4 magnetic particles used as raw materials in Example 1, the bfCL-Fe3O4@Au / Ag prepared in Example 1, and the ABEI and Co 2+ The dispersion stability of the particles obtained by dual functionalization of carboxylated Fe3O4 magnetic particles (dfCL-magnetic particles (MB)) and PEG-coated dfCL-magnetic particles (PEG / dfCL-magnetic particles (MB)) was characterized.
[0088] The synthesis of dfCL-MB was carried out by a typical 1-ethyl-(3-dimethylaminopropyl)carbodiimide / N-hydroxysuccinimide coupling reaction to immobilize ABEI on the carboxylated MB surface, and Co was bound to the MB surface through coordination reaction and electrostatic interaction. 2+ The PEG / dfCL-MB was prepared by directly connecting to the surface of ABEI / MB. The PEG / dfCL-MB was prepared by preparing a sulfonyl polyethylene glycol (PEG) coating layer on the surface of Fe3O4MB using the technology described in the document "Automatic label-free immunoassay with high sensitivity for rapid detection of SARS-CoV-2 nucleocapsid protein based on chemiluminescent magnetic beads" (Sensors and Actuators, B. Chemical, Lyu, Aihua et al., Vol. 349, December 2021), and then the PEG-coated Fe3O4MB was combined with Co ions and ABEI according to the steps described in Example 1.
[0089] In the prior art, after the magnetic particles are modified or functionalized, a common problem is that the modification or functionalization easily causes the magnetic particles to agglomerate, which significantly deteriorates the stability of the dispersion. In order to study the dispersion stability of the materials prepared in this application, the applicant analyzed the dispersibility of the aqueous dispersions of various materials including bfCL-Fe3O4@Au / Ag prepared in Example 1 of this application. The photos of the analysis process are shown in FIG. Fig. 9 The magnetic nanomaterials for dispersion stability characterization include the aminated Fe3O4 magnetic particles used as raw materials in Example 1, bfCL-Fe3O4@Au / Ag prepared in Example 1, and the magnetic nanomaterials prepared by ABEI and Co 2+ Particles obtained by dual functionalization of carboxylated Fe3O4 magnetic particles (dfCL-magnetic particles (MB)) and PEG-coated dfCL-magnetic particles (PEG / dfCL-magnetic particles (MB)). Fig. 9 As shown, the aminated Fe3O4MB, dfCL-MB and PEG / dfCL-MB used as control experiments all underwent significant sedimentation within 1 hour, while only the bfCL-Fe3O4@Au / Ag magnetic nanomaterial prepared in Example 1 was able to maintain good dispersion for up to 3 hours, indicating that the bfCL-Fe3O4@Au / Ag prepared in Example 1 has good dispersibility and is suitable for constructing immunosensors.
[0090] Example 4: CL performance analysis of the product obtained in Example 1
[0091] In this example, the product bfCL-Fe3O4@Au / Ag prepared in Example 1 and two control samples MB@ABEI-Au / Co 2+ (MAA / Co 2+ ) and dfCL-MB were characterized. In addition, the CL performance of ABEI used as a raw material in Example 1 was also characterized in this example. As mentioned above, dfCL-MB is a typical 1-ethyl-(3-dimethylaminopropyl) carbodiimide / N-hydroxysuccinimide coupling reaction to fix ABEI on the carboxylated MB surface, and Co 2+ directly attached to the surface of ABEI / MB; while MAA / Co 2+ The ABEI-AuNPs were formed by reducing HAuCl4 with ABEI on the surface of aminated Fe3O4 magnetic particles (MB), and Co 2+ Combined.
[0092] The CL properties of bfCL-Fe3O4@Au / Ag and the comparative samples prepared in Example 1 were tested using a microplate chemiluminescence detector. The measured CL properties are shown in FIG. 10A to FIG. 10D .like Fig. 10A As shown, bfCL-Fe3O4@Au / Ag exhibits a higher CL emission intensity than MB@ABEI-Au / Co as the control sample. 2+ (MAA / Co 2+ ) and dfCL-MB were 36 and 3.5 times higher, respectively. Fig. 10B It shows that the peak of the CL emission signal of bfCL-Fe3O4@Au / Ag is at a similar wavelength to the peak of the ABEI emission signal.
[0093] Fig. 10C The results show that the signal intensity emitted by the ABEI-H2O2 system alone is very weak. After the Fe3O4MB is mixed with ABEI, the CL intensity is reduced to one-sixth of the original value, which indicates that the combination of aminated Fe3O4MB and ABEI alone will cause a serious quenching effect. After the Au / Ag shell is applied to the aminated Fe3O4MB, the CL intensity of the mixture of Fe3O4@Au / Ag and ABEI is 8.6 times higher than that of the mixture of Fe3O4 and ABEI. 2+After forming a mixture with Fe3O4@Au / Ag and ABEI, its CL intensity is increased by 44.7 times compared with the mixture of Fe3O4@Au / Ag and ABEI. The above CL characterizations are all characterizations of physical mixtures, and the relative proportions of the components in the above mixtures correspond to the proportions of the components used in Example 1 of the present invention.
[0094] However, the inventors found that when the product bfCL-Fe3O4@Au / Ag nanocomposite material prepared in Example 1 was used, the CL intensity achieved was higher than that of the above-mentioned Fe3O4@Au / Ag, ABEI and Co 2+ The mixture further improved by 3.5 times. This shows that the composite prepared in Example 1 achieved a 3.5-fold improvement in CL intensity compared to a physical mixture of the components in the same amounts and ratios. Without wishing to be bound by a particular theory, the applicant speculates that this may be caused by the synergistic effect caused by the combination of the various components in bfCL-Fe3O4@Au / Ag.
[0095] In addition, the applicant also studied the changes in CL properties of the bfCL-Fe3O4@Au / Ag product prepared in Example 1 within 30 days. The results show that Fig. 10D The results showed that after 30 days, the relative standard deviation (RSD) of the CL signal intensity was 5.2%, indicating that the material prepared in Example 1 has excellent stability and is very suitable for constructing a biosensor with good stability.
[0096] Embodiment 5:
[0097] In this Example 5, the effects of changes in various process conditions (pH value and hydrogen peroxide concentration) on CL luminescence properties were studied.
[0098] First, CL luminescence properties were detected on a 96-well microplate according to the steps described in Example 1. 100 μL of the bfCL-Fe3O4@Au / Ag suspension prepared in Example 1 was added to each well. Then, at a gain of 2200, 100 μL of 1 mM H2O2 dissolved in aqueous NaOH solutions of different concentrations was injected into each well. When necessary, a dilute hydrochloric acid solution was used to adjust the materials in each well to different pH conditions. While injecting the H2O2 solution, a microplate chemiluminescence detector was used to record the CL kinetic curve. The highest peak intensity was recorded. The effect of pH on CL intensity was tested in this way, and the results are shown in Fig.11A .
[0099] In addition, CL luminescence property detection was performed on a 96-well microplate according to the steps described in Example 1. 100 μL of the bfCL-Fe3O4@Au / Ag suspension prepared in Example 1 was added to each well, and then 100 μL of a solution obtained by dissolving H2O2 of different concentrations in 0.01M NaOH aqueous solution was injected into each well at a gain of 2200. The pH value in each well was fixed at 12. While injecting the H2O2 solution, a microplate chemiluminescence detector was used to record the CL kinetic curve. The highest peak intensity was recorded. The effect of H2O2 concentration on CL intensity was tested in this way, and the results are shown in Fig. 11B .
[0100] Depend on Fig.11A and 11B From the results, we can see that the best experimental results can be obtained when the H2O2 concentration is 1mM and the pH value is 12.
[0101] Example 6
[0102] In this example, the effect of the thickness of the silver shell on the CL intensity was studied. Specifically, the steps of the example were repeated to synthesize bfCL-Fe3O4@Au / Ag, except that the amount of nitrate solution was changed to 0.9mL, 1.2mL, 1.5mL, 1.8mL and 2.1mL, respectively. The TEM images of the obtained bfCL-Fe3O4@Au / Ag products are shown in Fig. 12A , 12B , 12C, 12D and 12E. In addition, the CL properties of the products with different silver dosages were characterized according to the steps described in Example 1. The results are shown in Fig.12F .from Fig.12F It can be seen that when the amount of silver nitrate solution is 1.2 ml, the obtained bfCL-Fe3O4@Au / Ag product can achieve the most optimized CL properties, while when the amount of silver is higher or lower, the CL properties of the obtained bfCL-Fe3O4@Au / Ag product will further deteriorate.
[0103] Embodiment 7:
[0104] In this example, the effects of BSA solution treatment time and exosome incubation time on the CL properties of bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA / exosome complexes were studied.
[0105] Specifically, the steps described in Example 2 for synthesizing the bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA / exosome complex were repeated in this example, with the only difference being that the BSA solution treatment time was selected to be 10, 15, 20, 25, and 30 minutes (the BSA treatment time used in Example 2 was 10 minutes), or the exosome incubation time was changed to 3 minutes, 5 minutes, 8 minutes, 10 minutes, 15 minutes, and 25 minutes (the exosome incubation time used in Example 2 was 10 minutes). The CL intensities measured under the above different conditions are summarized and shown in Fig.13A and Fig. 13B ,in Fig.13A The relationship between BSA solution treatment time and CL properties is shown. Fig. 13B The relationship between exosome culture time and CL properties is shown. Fig.13A and 13B The results shown show that the best CL performance can be obtained when the BSA solution treatment time is 10 minutes and the exosome culture time is 10 minutes, so this optimal condition is adopted in the following examples.
[0106] Example 8
[0107] In this example, the experiment was carried out according to the same steps as in Example 2, with the only difference being that the concentration of exosomes was changed to detect the CL intensity of the bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA / exosome complex at different concentrations, and a graph was drawn based on the logarithmic values of intensity and concentration, as shown in FIG. Fig.14A As shown. Fig.14A It can be seen that when the exosome concentration is 3.1×10 3 -3.1×10 8 In the range of particles / mL, there is a very good linear relationship between the CL intensity (I) and the logarithmic value of the exosome concentration (C). The linear fitting equation obtained by calculating the data is I = 25599.56 + 1633.37log C (R 2 =0.9992, n=3). Using the technology of the present application, it can be confirmed that the detection limit (LOD) of exosomes is 2.1×10 3 Particles / ml, at this time the signal-to-noise ratio is 3 (S / N=3). In contrast, all technologies 1 developed so far in the prior art cannot achieve such a wide effective detection concentration range and such high sensitivity. In addition, the detection technology of the present application is a label-free technology, which does not require a complicated labeling process, and can achieve simplified working process and lower costs.
[0108] Example 9
[0109] In this example, the selectivity of the present technology for exosomes was studied by conducting experiments in the presence of interfering proteins.
[0110] In this example, hIgM, AFP and HER2 proteins were selected as interfering proteins. Specifically, in this example, the process of Example 2 was repeated, except that a concentration of 3.1×10 8 particles / ml of exosomes, and the above three proteins were added to them at the same time, with each protein at a concentration of 10 -9 g / mL. In addition, Example 2 was repeated three times, and the protein was replaced with the same concentration of hIgM, AFP or HER2 protein in each repetition. The CL intensity measured in each experiment 1 is summarized as follows: Fig. 14B As shown. ΔI represents the relative CL intensity calculated by I-I0, where I represents the CL intensity when exosomes are used and I0 represents the CL intensity when no exosomes are added. Fig. 14B It can be seen that significant ΔI can be achieved only for exosomes and mixtures (mixed proteins), while other interfering proteins alone show very poor ΔI. The results prove that the technology of the present application can achieve excellent selective detection of exosome target substances.
[0111] Example 10
[0112] This example characterizes the changes in CL properties of the bfCL-Fe3O4@Au / Ag / CD63-Ab / BSA / exosome complex synthesized in Example 2 during the 30-day detection process. The results are as follows: Fig.15 As shown. Fig.15 The results shown show that after continuous detection of exosomes for 30 days, the RSD is 5.4%, indicating that the label-free CL immunosensor prepared in Example 2 has excellent stability and reproducibility.
[0113] Example 11: Detection of exosomes in human serum samples
[0114] In this example, the clinical detection of exosomes in human serum samples using the samples of this application was tested. All serum samples used in this example were provided by the First Affiliated Hospital of USTC, and all samples were stored at -20°C. Before testing, the samples were diluted one hundred times with 0.01M PBS (pH = 7.4), and no other pretreatment was required before use. First, samples from four healthy persons were randomly collected, and the results are shown in Table 1. The CL immunosensor of this application showed good performance with a recovery rate of 91.6% to 102.9%, indicating that the samples synthesized in Examples 1 and 2 of this application are very suitable for clinical detection of CL immunosensors. Four serum samples obtained from lung cancer patients were also used for exosome detection. As shown in Table 1, the concentration of exosomes in the serum of cancer patients was determined to be 1.4×10 4 Particles / mL to 2.1×10 5 The results show that the label-free CL immunosensor developed in this application can detect the concentration of exosomes in serum samples of lung cancer patients with good accuracy.
[0115] Table 1. Quantitative detection of exosomes in human serum samples
[0116]
[0117] In addition, to further investigate the clinical utility of the technology developed in this application, exosomes were detected in serum samples of a series of healthy individuals and cancer patients, and the results are summarized as follows Fig. 14C Specifically, Fig. 14C As shown, the CL intensity of exosomes in the serum of 19 lung cancer patients, 10 breast cancer patients and 4 liver cancer patients was tested, and the CL intensity of exosomes in the serum of these cancer patients was significantly higher than that of exosomes in the serum of 21 healthy persons. It can be seen that the technology developed in this application can effectively distinguish healthy persons from cancer patients.
Claims
1. A chemiluminescent composition comprising: (i) a nanoparticle having a core-shell structure, the core-shell structure comprising at least one core and at least one shell, the core comprising Fe3O4, the shell comprising at least one noble metal selected from the group consisting of gold, silver, ruthenium, rhodium, palladium, osmium, iridium and platinum; (ii) transition metal ions; and (iii) a compound of the general formula (I), in, Ring A represents C6-C 14 Aromatic rings; R1 and R2 independently represent hydrogen, the terminal group is substituted by amino or is an unsubstituted straight chain or branched chain (C1-C 30 )alkyl, provided that the -NR1R2 moiety has at least one NH2 terminal group.
2. The chemiluminescent composition according to claim 1, characterized in that The core-shell structure includes a core portion, a first shell portion surrounding the core portion, and a second shell portion surrounding the first shell portion, the core portion contains Fe3O4, the first shell portion contains at least one precious metal selected from the following: gold, silver, ruthenium, rhodium, palladium, osmium, iridium and platinum, the second shell portion contains at least one precious metal selected from the following: gold, silver, ruthenium, rhodium, palladium, osmium, iridium and platinum, and the precious metal in the first shell portion is different from the precious metal in the second shell portion.
3. The chemiluminescent composition according to claim 1, characterized in that The core is a Fe3O4 nanoparticle whose surface is functionalized with amino-containing groups.
4. The chemiluminescent composition according to claim 2, characterized in that The first shell portion includes gold and the second shell portion includes silver.
5. The chemiluminescent composition according to claim 1, characterized in that The transition metal ion is selected from Co 2+ 、Ni 2+ , Fe 3+ , Fe 2+ Cr 3+ , Cu 2+ ; The molar ratio of the compound of general formula (I) to the transition metal ion is 1:10 to 10000:
1.
6. The chemiluminescent composition according to claim 1, characterized in that In the compound of the general formula (I), the A ring represents C6-C 10 aromatic ring, wherein R1 and R2 independently represent hydrogen, the terminal group is substituted by an amino group or is an unsubstituted straight chain or branched chain (C1-C 10 )alkyl, provided that the -NR1R2 moiety has at least one NH2 terminal group.
7. A method for preparing the chemiluminescent composition according to any one of claims 1 to 6, the method comprising the following steps: 1) applying one or more shells containing precious metals on the surface of Fe3O4 particles to form nanoparticles with a core-shell structure; 2) combining the nanoparticles having a core-shell structure with the transition metal ions and the compound of the general formula (I) to form the chemiluminescent composition.
8. A method for qualitative or quantitative analysis of an analyte, the method comprising the following steps: Step 1: mixing a sample containing an analyte with the composition according to any one of claims 1 to 6 to obtain an analyte system, and optionally adding an additive before, during or after the step 1, wherein the additive is selected from one or more of a pH adjuster, a pH buffer, an oxidant, a reductant, a stabilizer, a bactericide, a preservative, a chelating agent, and a complexing agent; Step 2: using a sensor to detect the light emitted by the above analyte system; The method does not involve labeling of the analyte.
9. The method according to claim 1, characterized in that Prior to step 1, the following step is further performed: allowing the composition according to any one of claims 1 to 6 to bind to a specific antibody or antigen, wherein the specific antibody or antigen is a specific antibody or antigen against the analyte.
10. The method according to claim 8, characterized in that The analyte is selected from: exosomes, novel coronavirus N protein, novel coronavirus S1, novel coronavirus RBD, cardiac troponin, copeptin, cardiac fatty acid binding protein, α-fetoprotein, prostate cancer markers, liver cancer markers, colorectal cancer markers, pancreatic cancer markers, gastric cancer markers, esophageal cancer markers, lung cancer markers, breast cancer markers, ovarian cancer markers, uterine cancer markers, hyperthyroidism markers, hepatitis markers, anemia markers, glucose metabolism markers, and bone metabolism markers.