Formation method of sodium battery, sodium battery and electric equipment
Through the process flow of static aging, normal temperature formation, secondary aging and charge and discharge cycles, the components and microstructure of the sodium battery SEI film are optimized, which solves the problem of poor stability of the sodium battery SEI film and significantly improves its cycle performance. and service life, meeting the needs of commercial applications.
Patent Information
- Application Number
- CN202410813406.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-01
AI Technical Summary
The SEI film formed by the existing sodium battery formation process has poor stability, which affects the cycle performance of the sodium battery and is difficult to meet the needs of commercial applications.
The process flow of static aging, normal temperature formation, secondary aging, charge and discharge cycles and three aging is adopted to optimize the components and microstructure of the SEI film. Through the synergistic effect of temperature and time, the stability and stability of the SEI film are improved. Ion conductivity properties.
It significantly improves the normal temperature cycle performance and cycle life of sodium batteries, expands their commercial application potential, and enhances market competitiveness.
Smart Images

Figure CN118738573A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of sodium ion batteries, and in particular to a formation method of a sodium battery, a sodium battery and an electrical device. Background Art
[0002] Sodium-ion batteries are batteries with similar energy storage mechanisms to lithium-ion batteries, and their manufacturing costs are low, making them more likely to meet the low-cost demand for large-scale energy storage devices. Both lithium and sodium batteries need to undergo a formation treatment before leaving the factory to form a solid electrolyte interface (SEI) on the surface of the battery's negative electrode material, which is convenient for improving the battery's cycle stability.
[0003] However, the current formation of sodium batteries is usually carried out with reference to the formation process of lithium batteries. However, due to the differences in composition, solubility in electrolyte, etc. between the SEI film of sodium batteries and the SEI film of lithium batteries, the stability of the SEI film of sodium batteries formed with reference to the formation process of sodium batteries is poor, which is not conducive to improving the cycle performance of sodium batteries. Summary of the invention
[0004] In view of this, the present application provides a formation method particularly suitable for sodium batteries to obtain a finished sodium battery with excellent cycle stability.
[0005] In a first aspect, the present application provides a sodium battery formation method, comprising the following steps:
[0006] (1) The assembled sodium battery is subjected to static aging, then subjected to room temperature formation at a temperature of 20-40° C., and then subjected to secondary aging at a temperature of 45-60° C.;
[0007] (2) subjecting the sodium battery after the secondary aging to charge and discharge cycles at 20-40° C., and then subjecting the battery to a third aging at a temperature of 35-65° C. for 12 hours to 30 days.
[0008] Through the above-mentioned novel formation method, the components and microstructure of the inner and outer layers of the SEI film of the obtained sodium battery can be optimized at the same time. Under their synergistic effect, the room temperature cycle performance of the sodium battery is greatly improved, which is beneficial to expand the commercial application of sodium batteries.
[0009] In a second aspect, the present application provides a sodium battery obtained by the formation method of the first aspect.
[0010] The cycle performance of the sodium battery obtained by the above-mentioned formation method can be greatly improved, especially the cycle performance at room temperature is excellent and the cycle life is long, which is conducive to its commercial application.
[0011] In a third aspect, the present application provides an electrical device, which includes the sodium battery described in the second aspect of the present application.
[0012] The electrical equipment is powered by the sodium battery after formation. Based on the good cycle performance of the sodium battery, the market competitiveness of the electrical equipment is outstanding. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a process flow chart of the sodium battery formation method provided in this application.
[0014] Figure 2 The electrochemical impedance spectroscopy (EIS) test results of the sodium battery of Comparative Example 1 and the sodium battery of Example 5 that were not aged three times are summarized.
[0015] Figure 3 The characterization results of the SEI films of the sodium battery of Comparative Example 1 which was not aged three times and the sodium battery of Example 5 are summarized and compared. DETAILED DESCRIPTION
[0016] In order to solve the problem that the formation process used in existing sodium batteries is not conducive to maintaining the stability of the formed SEI film and is not conducive to improving the battery cycle performance, the present application provides a formation method that can improve the room temperature cycle performance of sodium batteries.
[0017] Specifically, the process flow chart of the sodium battery formation method provided in this application is as follows: Figure 1 The formation method may include the following steps:
[0018] (1) The assembled sodium battery is subjected to static aging, then subjected to room temperature formation at a temperature of 20-40° C., and then subjected to secondary aging at a temperature of 45-60° C.;
[0019] (2) subjecting the sodium battery after the secondary aging to charge and discharge cycles at 20-40° C., and then subjecting the battery to a third aging at a temperature of 35-65° C. for 12 hours to 30 days.
[0020] The applicant has conducted in-depth research on the physicochemical properties of the SEI film of the sodium battery and explored a formation process that matches it well. Specifically, the assembled sodium battery filled with electrolyte is first subjected to static aging, room temperature formation, and secondary aging at 45-60°C in sequence, so that the initial SEI film can be constructed and the more soluble part of its outer layer can be dissolved; then the sodium battery after the secondary formation is charged and discharged for 1-3 cycles, so that the SEI film can become relatively stable, and then three agings at a specific temperature and a specific time can be performed, so that some unstable organic sodium salts in the outer layer of the SEI film can be dissolved and reconstructed to an appropriate extent, reducing the thickness of the overall SEI film to reduce its transmission impedance, thereby facilitating the improvement of the ion conduction performance of the SEI film; in addition, the organic lithium salt in the SEI film is decomposed into inorganic lithium salts, especially as the unstable organic lithium salts in the inner layer of the SEI film decompose, the inorganic lithium salts with relatively stable chemical and physical properties will be more evenly and densely distributed, effectively isolating the reaction between the negative electrode material and the electrolyte, thereby stabilizing the interface between the negative electrode material and the electrolyte. Therefore, after the sodium battery is treated by the above-mentioned formation method, its room temperature cycle performance can be greatly improved, which is conducive to its commercial application.
[0021] Wherein, in step (1), the assembled sodium battery is a sealed sodium battery filled with electrolyte. Specifically, the assembled sodium battery includes a battery housing, a battery cell and an electrolyte contained in the battery housing, wherein the battery cell includes a positive electrode sheet, a negative electrode sheet and a separator located between the positive electrode sheet and the negative electrode sheet. Wherein, the assembly process of the sodium battery includes: stacking the positive electrode sheet, the separator and the negative electrode sheet in sequence to form a bare battery cell, loading the bare battery cell into a battery housing (such as an aluminum shell / steel shell / aluminum-plastic film), injecting the electrolyte into the battery housing after vacuum baking, and finally sealing the battery housing.
[0022] In step (1), the purpose of static aging is to allow the electrolyte in the newly assembled sodium battery to infiltrate its battery cell to facilitate subsequent formation. In the embodiment of the present application, the temperature of the static aging is 20-45°C, and the time is 24h-72h. Exemplarily, the temperature of the static aging can be specifically 23°C, 25°C, 28°C, 30°C, 32°C, 35°C, 38°C, 40°C, or 42°C. The time for static aging can be specifically 28h, 30h, 36h, 40h, 42h, 48h, 54h, 60h, 66h, or 70h, etc.
[0023] The purpose of formation is to cause an irreversible reaction between the negative electrode material and the solvent, additives and other molecules in the electrolyte at the negative electrode interface to form a passivation film layer covering the surface of the negative electrode, namely the aforementioned SEI film. Among them, in order to improve the formation efficiency, in most cases, the formation of lithium batteries is carried out at high temperature (≥45°C). The main components of the SEI film of sodium batteries include inorganic sodium salts and sodium-containing organic matter. The inorganic sodium salts are closer to the negative electrode material layer. The solubility of the SEI film of sodium batteries in the electrolyte is much greater than the solubility of the SEI film of lithium-ion batteries in the same composition electrolyte. In order to avoid excessive dissolution of the SEI film formed by formation in the electrolyte solvent and avoid re-formation, the formation of the sodium battery is controlled at room temperature (20-40°C). The temperature of normal temperature formation can be, for example, 22°C, 25°C, 28°C, 30°C, 32°C, 35°C, or 38°C.
[0024] In the embodiments of the present application, the normal temperature formation may adopt a step-by-step graded formation, that is, the normal temperature formation may include more than two charging stages. Wherein, after the normal temperature formation is completed, the sodium battery reaches 100% SOC. In some embodiments of the present application, the normal temperature formation includes two-step charging, wherein the first step of charging is charging at a rate of 0.01C-0.2C for 120-180min, and the second step of charging is charging at a rate of 0.2C-0.5C at constant current and constant voltage to 100% SOC. Controlling the charging rate of the first step to be relatively small can ensure that the density of the formed SEI film mainly composed of inorganic sodium salts is relatively high, so that it can play a role in reducing the side reactions between the negative electrode active materials and the electrolyte. The charging rate of the second step is greater than that of the first step, which can reduce the charging time and facilitate the formation of a loose structure SEI film mainly composed of organic sodium salts, which is conducive to the infiltration of the electrolyte and the active Na + Desolvation and shuttling are achieved in this part of the SEI film. In some embodiments, after the first step of charging is completed, the second step of charging can be performed after a period of rest.
[0025] In the implementation manner of the present application, the cut-off voltage of the first step of charging is greater than 1.9V, and / or the SOC at the end of the first step of charging is 2%-25%. This ensures that the cut-off voltage (or end voltage) of the first step of charging is greater than the decomposition voltage of common film-forming additives in the electrolyte, so that the film-forming additives preferentially participate in film formation and reduce the irreversible consumption of solvents in the electrolyte. In some embodiments, the cut-off voltage of the first step of charging is greater than 2.0V, and can further be in the range of 2.1V-2.5V. The SOC at the end of the first step of charging can be 5%, 8%, 10%, 12%, 15%, 20%, etc.
[0026] In step (1), after the normal temperature chemical formation is completed, secondary aging is performed at a relatively high temperature (45-60° C.) (this step may also be referred to as “high temperature aging”), so that the particularly unstable or overly loose parts of the SEI film formed by the normal temperature chemical formation can be dissolved. At the same time, the secondary aging is not performed under power-on conditions, so that the SEI film will not be excessively dissolved and produce more gas.
[0027] Specifically, the secondary aging temperature can be 45°C, 46°C, 47°C, 48°C, 49°C, 50°C, 52°C, 53°C, 55°C, 56°C, 58°C or 59°C. In some embodiments, the secondary aging temperature is 45°C-55°C. In the embodiment of the present application, in step (1), the secondary aging time can be 20h-72h. Specifically, the secondary aging time can be 22h, 24h, 26h, 28h, 30h, 36h, 40h, 42h, 45h, 48h, 54h, 60h, 66h, or 70h.
[0028] In step (2), the charge and discharge cycle is carried out at room temperature at 20-40°C, so that the thickness of the SEI film in different regions becomes uniform, and there will be no local excessive thickness, and the outer layer of the SEI film that is too loose is removed, so that the formed SEI film is more stable. In addition, the charge and discharge cycle is carried out at room temperature rather than at a high temperature greater than 40°C, which can avoid the SEI film from being dissolved too much and needing to rebuild the SEI film, and avoid the generation of too much gas in this process and the need for an additional "exhaust" process after this process. Among them, the above-mentioned charge and discharge cycle can be specifically carried out at a temperature of 20°C, 23°C, 25°C, 28°C, 30°C, 32°C, 35°C, 38°C, 40°C, etc. The above-mentioned charge and discharge cycle can be carried out for 1-3 cycles. Carrying out a fewer number of charge and discharge cycles at room temperature can avoid a significant decrease in the capacity of the sodium battery.
[0029] In addition, since the sodium battery is charged and then aged for the second time, the sodium battery after the second ageing is discharged first and then charged during the charge and discharge cycle. In this application, the sodium battery reaches 100% SOC after the charge cycle.
[0030] In some embodiments of the present application, in step (2), the charge and discharge cycle is performed at a rate of 0.5C-1.0C. The charge and discharge rate can be 0.55C, 0.6C, 0.65C, 0.7C, 0.75C, 0.8C, or 0.9C, etc. In some embodiments, the charging process of the charge and discharge cycle includes charging to 100% SOC at a constant current and constant voltage of 0.5C-1.0C; the discharging process of the charge and discharge cycle includes constant current discharge at a rate of 0.5C-1.0C. Specifically, during discharge, the battery is first charged at a constant current of 0.5C-1.0C to a charge cutoff voltage, and then charged to 100% SOC at a constant voltage of the charge cutoff voltage.
[0031] In some embodiments of the present application, the charge cut-off voltage of the charge-discharge cycle is 3.9-4.1V, and the discharge cut-off voltage is 1.5-2.0V. Exemplarily, the charge cut-off voltage of the charge-discharge cycle can be specifically 3.9V, 3.95V, 4.0V, 4.05V, 4.1V, etc. The discharge cut-off voltage of the charge-discharge cycle can be, for example, 1.5V, 1.6V, 1.7V, 1.8V, 1.9V, 2.0V, etc.
[0032] In step (2) of the present application, as described above in the present application, adding the above-mentioned three agings at 25-65°C for 12 hours to 20 days in the formation process of the sodium battery can reduce the thickness of the SEI film of the sodium battery, optimize the components and microstructure of the inner and outer layers of the SEI film, and improve the room temperature cycle performance of the sodium battery. In addition, the three agings are not carried out at a temperature greater than 65°C (for example, above 70°C), which can avoid the drastic dissolution and reconstruction of the formed sodium battery SEI film in the process, and the sodium embedded in the negative electrode or adsorbed on the surface of the negative electrode material reacts with the electrolyte to a large extent to produce a large amount of gas, which in turn causes the battery's vent valve to be flushed open, resulting in a battery short circuit, etc.
[0033] Exemplarily, the temperature of the three agings can be 30°C, 35°C, 38°C, 40°C, 42°C, 45°C, 48°C, 50°C, 55°C, 58°C, 60°C, 62°C, 65°C, etc. The duration of the three agings can be 18 hours, 24 hours (i.e., 1 day), 36 hours, 48 hours (i.e., 2 days), 60 hours, 72 hours (i.e., 3 days), 96 hours (i.e., 4 days), 5 days, 5.5 days, 6 days, 6.5 days, 7 days, 8 days, 9 days, 10 days, 11 days, 12 days, 13 days, 14 days, 15 days, 16 days, 17 days, 18 days, 19 days, 20 days, 22 days, 25 days, 26 days, 28 days, 29 days, etc. In some embodiments of the present application, the temperature of the three agings is 35-60°C. The duration of the three agings is 24 hours-10 days. A suitably high aging temperature is conducive to accelerating the optimization of the components and structure of the inner and outer layers of the SEI membrane of the sodium battery. A suitably long aging time can ensure that the components and structure of the inner and outer layers of the SEI membrane of the sodium battery are optimized while also taking into account production efficiency.
[0034] In the present application, the aforementioned negative electrode sheet, positive electrode sheet, and separator are all conventional choices in the battery field. Generally, the positive electrode sheet includes a positive electrode current collector and a positive electrode material layer disposed on the positive electrode current collector; the positive electrode material layer includes a positive electrode active material, a binder, and an optional conductive agent. Similarly, the negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on the negative electrode current collector, and the negative electrode material layer may include a negative electrode active material, a binder, and an optional conductive agent. Among them, the positive electrode current collector and the negative electrode current collector can be independently selected from metal foil, carbon-coated metal foil, or porous metal plate, etc. The metal foil can be a metal single substance foil, or a metal alloy foil. In sodium batteries, it is common to use aluminum foil for the positive electrode current collector and the negative electrode current collector. The cost of aluminum foil is relatively low.
[0035] For sodium batteries, the negative electrode active material may include, but is not limited to, one or more of hard carbon, soft carbon, mesophase carbon microspheres, graphene and carbon nanotubes. The positive electrode active material may include, but is not limited to, one or more of layered sodium-based oxides, polyanionic sodium-based cathode materials, Prussian blue, Prussian white, etc. Exemplarily, the structural formula of the layered sodium-based oxide may be L x Na y M z Cu α Fe β Mn γ O 2+δ-0.5η X η, wherein L is an alkali metal doping substitution element, M is a transition metal doping substitution element, X is an oxygen doping substitution element, 0≤x<0.35, 0.65≤y≤1, 0<α≤0.3, 0<β≤0.5, 0<γ≤0.5, -0.03≤δ≤0.03, 0≤η≤0.1, z+α+β+γ=1, and mx+y+nz+2α+3β+4γ=2(2+δ). The structural formula of an exemplary polyanionic sodium positive electrode material may be A a M b (PO4) c O x X 3-x , wherein A is one or more of H, Li, Na, K and NH4, M is one or more of Ti, Cr, Mn, Fe, Co, Ni, V, Cu and Zn, X is one or more of F, Cl and Br, 0<a≤4, 0<b≤2, 1≤c≤3, 0≤x≤2. The exemplary structural formula of Prussian blue and Prussian white can be expressed as A x M[M′(CN)6] y ·zH2O, wherein A is one or more of alkali metal ions and alkaline earth metal ions, M and M' are transition metal elements, 0 <x≤2,0.8≤y<1,0<z≤20。
[0036] Adding a binder to the positive electrode material layer and the negative electrode material layer can help them to adhere firmly to the current collector; adding a conductive agent to the positive electrode material layer and the negative electrode material layer can improve their conductivity. The present application does not specifically limit the types of binders and conductive agents, and can be selected according to actual needs. Exemplarily, the binder may include polyvinylidene fluoride (PVDF), polyacrylic acid (PAA), lithium polyacrylate, sodium polyacrylate, polyacrylate (such as polymethyl methacrylate, polymethyl acrylate, polyethyl acrylate, etc.), polyacrylonitrile (PAN), styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), sodium carboxymethyl cellulose (CMC-Na), lithium carboxymethyl cellulose, sodium alginate, etc., but not limited thereto. The conductive agent may include one or more of conductive carbon black (such as acetylene black, Ketjen black, Super P, etc.), carbon nanotubes, carbon nanodots, carbon nanofibers, graphene, etc., but not limited thereto.
[0037] The positive electrode material layer is obtained by coating a positive electrode slurry of corresponding composition on the positive electrode current collector and then baking. The solvent in the positive electrode slurry may include but is not limited to one or more of N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), N,N-dimethylformamide (DMF), ethanol, etc. Similarly, the solvent in the negative electrode slurry used to form the negative electrode material layer may include but is not limited to one or more of water, NMP, THF, DMF, and ethanol.
[0038] The diaphragm may include but is not limited to one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, polyvinylidene fluoride, etc., and may be a single-layer film or a multi-layer film. The electrolyte may include an organic solvent, a sodium salt and optional electrolyte additives. Among them, the electrolyte additives include but are not limited to one or more of film-forming additives, anti-overcharge additives, flame retardants, etc., which can be added according to actual needs. The organic solvent may include but is not limited to one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC) and ether solvents (such as ethylene glycol monomethyl ether series); the sodium salt may be one or more of NaPF6, NaClO4, NaBCl4, NaSO3CF3 and Na(CH3)C6H4SO3.
[0039] The present application also provides a sodium battery obtained by the above-mentioned formation method. The cycle performance of the sodium battery obtained by the above-mentioned formation method can be well improved, especially the cycle performance at room temperature is excellent and the cycle life is long, which is conducive to its commercial application. For example, the sodium battery can be used in electrical equipment to supply power for it; it can also be used in energy storage systems.
[0040] The embodiment of the present application also provides an electric device, which includes a sodium battery obtained by the above-mentioned formation method of the present application. The electric device uses the sodium battery to power itself, and based on the good cycle performance of the sodium battery, the electric device has a long service life and outstanding market competitiveness.
[0041] In the implementation manner of the present application, the electrical equipment includes but is not limited to one or more of 3C products (such as mobile phones, laptops, tablet computers, wearable devices, etc.), or electric transportation vehicles (such as electric cars, electric motorcycles, electric bicycles, etc.).
[0042] The embodiments of the present application are further described below in conjunction with multiple embodiments.
[0043] Before introducing the sodium battery formation method provided by the present application, the preparation method of the sodium battery to be formed is first introduced.
[0044] 1) Preparation of positive electrode sheet: The positive electrode active material (specifically NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, abbreviated as NFM), a conductive agent (specifically single-walled carbon nanotubes (SWCNT)), and a binder (specifically PVDF) are mixed in a solvent N-methylpyrrolidone (NMP) in a weight ratio of 95:2.5:2.5 to prepare a positive electrode slurry; the positive electrode slurry is coated on both sides of an aluminum foil, and the positive electrode sheet is obtained after baking and rolling.
[0045] 2) Preparation of negative electrode sheet: hard carbon as negative electrode active material is mixed with conductive agent (specifically Super P and CNT), binder SBR and binder CMC in water at a mass ratio of 92:3:2:3 to prepare negative electrode slurry; the negative electrode slurry is coated on both sides of aluminum foil, and the negative electrode sheet is obtained after drying and rolling.
[0046] 3) Preparation of electrolyte: at 25°C, ethylene carbonate (EC), propylene carbonate (PC) and diethyl carbonate (DEC) are mixed at a volume ratio of 1:1:1 to obtain a mixed organic solvent; then a certain amount of film-forming additive - fluoroethylene carbonate (FEC) is added to the mixed organic solvent, and after mixing, a certain amount of sodium hexafluorophosphate (NaPF6) as an electrolyte sodium salt is added and mixed to obtain the desired electrolyte.
[0047] 4) Assembly of sodium battery: Under an ambient dew point of less than -20°C, the positive electrode sheet, separator and negative electrode sheet are stacked in order and wound into a bare battery cell, which is then placed in an aluminum shell. After welding, the bare battery cell is transferred to a vacuum environment for baking, and then the electrolyte is injected into the aluminum-plastic film in a glove box filled with nitrogen (nitrogen dew point ≤ -50°C), and then the battery shell is sealed to obtain a sodium battery.
[0048] Example 1
[0049] A sodium battery formation method comprising:
[0050] (1) The assembled sodium battery is aged at 25°C for 72 hours to allow the electrolyte to fully infiltrate the battery cell; then, it is formed at room temperature at 25°C, specifically including: first charging at 0.05C for 180 minutes, with an end voltage of 2.4V, and then charging at 0.2C constant current and constant voltage to 100% SOC; then, the sodium battery is aged for a second time at 45°C for 48 hours;
[0051] (2) The sodium battery after the secondary aging was subjected to three charge and discharge cycles at 25°C and 0.7C, wherein the charge cut-off voltage was 3.9V, the discharge cut-off voltage was 1.5V, and the sodium battery reached 100% SOC after the charge cycle; finally, the sodium battery was aged three times at 35°C for 72 hours to obtain a finished sodium battery that can be used for electrochemical performance testing.
[0052] Example 2
[0053] A sodium battery formation method, which differs from Example 1 only in that the three agings are performed at 45° C. for 72 hours.
[0054] Example 3
[0055] A sodium battery formation method, which differs from Example 1 only in that the three agings are carried out at 60° C. for 72 hours.
[0056] Example 4
[0057] A sodium battery formation method, which differs from Example 1 only in that the three agings are carried out at 60° C. for 6 days.
[0058] Example 5
[0059] A sodium battery formation method, which differs from Example 1 only in that the three agings are carried out at 60° C. for 28 days.
[0060] Comparative Example 1
[0061] A sodium battery formation method, which differs from Example 1 only in that the three-stage aging is not performed.
[0062] Comparative Example 2
[0063] A sodium battery formation method, which differs from Example 1 only in that the three agings are performed at 70° C. for 12 hours.
[0064] Comparative Example 3
[0065] A sodium battery formation method, which differs from Example 1 only in that the normal temperature charge and discharge cycle of step (2) is not performed and the three-stage aging is not performed.
[0066] The finished sodium battery products obtained by the formation methods described in the above embodiments and comparative examples were tested for their room temperature cycle performance and rated capacity, and the results are summarized in the following Table 1.
[0067] Among them, the test method for room temperature cycle performance includes: at 25±3℃, charging and discharging tests are carried out on each sodium battery product in a cycle of 1.0C charging / 2.0C discharging: the charging process is constant current and constant voltage charging, the charging cut-off voltage is 3.9V, and the cut-off current is 0.025C; the discharging process is constant current discharge, and the discharge cut-off voltage is 1.5V.
[0068] The test method for the rated capacity of the battery includes: at 25±3°C, first discharging each battery to 1.5V at 0.2C, then charging to 3.9V at 0.2C constant current and constant voltage, with a cut-off current of 0.025C, and then discharging to 1.5V at 0.2C, and recording the discharge capacity (as the rated capacity of the battery).
[0069] Table 1
[0070]
[0071] From the comparison of Examples 1-5 and Comparative Example 1 in Table 1, it can be seen that adding a third aging process to the sodium battery after primary aging, room temperature formation, secondary aging, and room temperature charge and discharge cycle can help improve the room temperature cycle performance of the sodium battery without reducing the rated capacity of the sodium battery, and can even improve the capacity to a certain extent. This is because the three-stage aging can effectively optimize / reconstruct the original unstable and thick SEI film of the sodium battery (see Figure 3 ).
[0072] Figure 2-Figure 3 The EIS and SEI film characterization results of the sodium battery of Comparative Example 1 which was not aged three times and the sodium battery of Example 5 which was aged three times were summarized and compared. Figure 2 This is a comparison chart of the EIS of the sodium battery of comparative example 1 and the sodium battery of example 5 at full charge state (3.9V). Figure 3 In the figure, (a) and (d) are scanning electron microscope photographs (SEM) of the cross-section of each SEI film, (b) and (e) are scanning transmission electron microscope (STEM) photographs of each SEI film, (c) is the energy spectrum line scan of the area indicated by the arrow in (b), and (f) is the energy spectrum line scan of the area indicated by the arrow in (e).
[0073] Figure 2 Each EIS curve is mainly composed of a semicircle in the high-frequency region and a slant line in the low-frequency region. The larger the diameter of the semicircle in the high-frequency region, the greater the charge transfer impedance of the battery. Figure 2 It can be seen that after three agings, the cell transmission impedance of the sodium battery in Example 5 is significantly reduced. Figure 3 It can be seen that the overall formation process of the sodium battery in Comparative Example 1 does not use three agings, and the thickness of the formed SEI film is relatively thick ( Figure 3 In (a), the thickness of the SEI film of the battery of Example 5, which was aged three times, is thinner ( Figure 3 In (d), the thickness of the regions is marked as 9nm, 15nm, and 21nm. Figure 3 It can be seen from (a), (b) and (c) that in Comparative Example 1, it can be observed that the thickness of the battery SEI film is relatively large (60-80nm thick), resulting in a relatively large impedance when the charge passes through the SEI film; the inorganic sodium salt (such as Na2O, NaF and other components) is mainly distributed in the inner layer of the SEI film (near the hard carbon negative electrode material side), and the distribution is not dense enough, and the hard carbon surface cannot be effectively protected during the long cycle process, resulting in more side reactions, a large loss of active substances, and too fast consumption of electrolyte, and serious gas production; while the thickness of the battery SEI film of Example 5, which adopts three-time aging, is significantly reduced (about 10-20nm thick), and the charge is easier to transmit through the SEI film; and the organic sodium salt is converted into inorganic sodium salt during the three-time aging process, making the inorganic sodium salt in the inner layer of the SEI film denser (see Figure 3 (d), (e) and (f)), thereby achieving effective coating of the negative electrode hard carbon surface in a long cycle, effectively reducing side reactions during the cycle, reducing the consumption of electrolyte and the loss of active substances, and thus improving the battery cycle life.
[0074] In addition, from the comparison of Examples 1-3 in Table 1, it can be seen that when the three aging times remain unchanged, increasing the temperature of the three agings within an appropriate temperature range is more conducive to improving the room temperature cycle performance of the sodium battery. This may be because within a certain temperature range, the unstable components in the SEI film can be decomposed more quickly with the increase of the three formation temperatures. As the components in the SEI film change, the reconstructed SEI film is more stable in long cycles. From the comparison of Examples 3-5, it can be seen that when the temperature of the three agings is 60°C and the three aging times are selected for 72h, the room temperature cycle improvement effect on the sodium battery is the most significant, and the aging time is short, taking into account production efficiency.
[0075] From the comparison between Comparative Example 2 and other embodiments, it can be learned that when the temperature of the tertiary aging is too high (for example, 70° C.), even if the time of the tertiary aging is controlled to be short, the SEI film of the sodium battery will be drastically dissolved and reconstructed due to the high temperature. During this period, the sodium embedded or adsorbed in the negative electrode will undergo a violent side reaction with the electrolyte to produce a large amount of gas, causing the battery's vent valve to be flushed open, and then the battery will short-circuit and be scrapped. Finally, the capacity retention rate of the battery in Comparative Example 2 after 1000 cycles was not measured.
[0076] The above-mentioned embodiments only express several exemplary implementations of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application.
Claims
1. A sodium battery formation method, It is characterized in that The following steps are involved: (1) The assembled sodium battery is subjected to static aging, then subjected to room temperature formation at a temperature of 20-40° C., and then subjected to secondary aging at a temperature of 45-60° C.; (2) subjecting the sodium battery after the secondary aging to charge and discharge cycles at 20-40° C., and then subjecting the battery to a third aging at a temperature of 35-65° C. for 12 hours to 30 days.
2. The chemical formation method according to claim 1, It is characterized in that The temperature of the three aging processes is 35-60° C. and the duration is 24 hours to 10 days.
3. The chemical formation method according to claim 1, It is characterized in that The room temperature formation includes two-step charging, wherein the first step of charging is charging at a rate of 0.01C-0.2C for 120-180min, and the second step of charging is charging at a rate of 0.2C-0.5C at constant current and constant voltage to 100% SOC.
4. The chemical formation method according to claim 3, It is characterized in that The cut-off voltage of the first step of charging is greater than 1.9V.
5. The formation method according to any one of claims 1 to 4, It is characterized in that The charging process of the charge-discharge cycle includes: charging to 100% SOC at a constant current and voltage of 0.5C-1.0C; and the discharging process of the charge-discharge cycle includes discharging at a constant current of 0.5C-1.0C.
6. The formation method according to any one of claims 1 to 5, It is characterized in that The charge cut-off voltage of the charge-discharge cycle is 3.9-4.1V, and the discharge cut-off voltage is 1.5-2.0V.
7. The formation method according to any one of claims 1 to 6, It is characterized in that In step (2), the charge and discharge cycle is performed for 1 to 3 cycles.
8. The formation method according to any one of claims 1 to 7, It is characterized in that In step (1), the temperature of the static aging is 20-45° C., and the duration is 24 h to 72 h.
9. The formation method according to any one of claims 1 to 8, It is characterized in that The secondary aging is carried out for 20 hours to 72 hours.
10. A sodium battery obtained by the formation method according to any one of claims 1 to 9.
11. An electrical device, It is characterized in that Comprising the sodium battery as claimed in claim 10.