Liquid injection method for improving wettability of electrolyte of lithium ion battery
Through three liquid injection methods, the lithium-ion battery electrolyte and pole pieces are fully infiltrated to ensure that it solves the problem of poor electrolyte wettability in high-energy-density batteries, improves battery performance and production efficiency, and reduces energy consumption.
Patent Information
- Application Number
- CN202410885475.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-01
AI Technical Summary
In high-energy-density lithium-ion batteries, it is difficult to fully infiltrate between the electrolyte and the pole pieces, resulting in poor performance and safety issues. Existing liquid injection methods have problems with high energy consumption, cost and efficiency limitations when improving wettability.
Adopt three injection methods: one injection to 80%, pump negative pressure, two injections to 85%, let it stand and form before high temperature, let it stand after high temperature, inject the last three times until it is fully charged, and shorten the time before forming at high temperature. Allow the rest time to ensure that the electrolyte and pole pieces are fully infiltrated.
It achieves perfect infiltration of electrolyte and pole pieces, improves cycle performance, significantly reduces energy consumption, improves production efficiency, and reduces the energy consumption of industrial production by shortening the standing time before forming to high temperature.
Smart Images

Figure CN118738786A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery injection, and in particular to a method for improving the wettability of lithium ion battery electrolyte. Background Art
[0002] As the global energy storage market continues to grow, the energy density of batteries is getting higher and higher, which leads to a higher compaction density of the electrodes. A larger compaction density will reduce the porosity of the positive and negative electrode plates, making it difficult for the electrolyte of the lithium-ion battery to fully penetrate the electrode plates, which in turn causes the battery performance to deteriorate.
[0003] Usually, the injection of lithium-ion batteries is divided into two steps, namely, the first injection, standing before high temperature, formation, standing after high temperature, and the second injection. The first injection volume is injected to 85% of the reserved volume, and the second injection volume is directly injected to the reserved volume. However, for batteries with high energy density, this injection method is difficult to achieve a good wetting effect between the electrode and the electrolyte. When disassembling the battery, it is found that a large amount of lithium precipitation is generated in the negative electrode, which limits the performance of the battery and even causes safety problems. Usually, increasing the standing time before high temperature formation can improve the wetting effect, but the high temperature energy consumption is large, which will limit the cost and efficiency of production. Summary of the invention
[0004] The object of the present invention is to provide a method for injecting electrolyte for improving the wettability of lithium ion battery electrolyte, so as to overcome the above-mentioned defects in the prior art.
[0005] A method for improving the wettability of lithium ion battery electrolyte injection, comprising the following steps:
[0006] Step 1. In an environment of 25°C, take a 314Ah battery cell after baking, inject 900g of electrolyte normally, and then let it stand for 1 hour;
[0007] Step 2: After standing still, draw negative pressure to allow the electrolyte and the electrode to fully infiltrate;
[0008] Step 3: After the negative pressure is pumped out, the battery cell is injected with electrolyte for the second time, and the electrolyte is injected to 960g;
[0009] Step 4: Then let it stand for 5 hours before high temperature and carry out the formation normally;
[0010] Step 5: After the formation is completed, let it stand at high temperature for 8 hours;
[0011] Step 6: After the battery cell is aged for 8 hours, it is cooled to room temperature and then filled three times with electrolyte until the holding amount is 1130g. The sealing pins are then welded and the battery cell is fully charged.
[0012] Preferably, in step 2, negative pressure is applied for 2 hours, and the pressure is maintained at ≤-80 kPa.
[0013] Preferably, the formation process in step 4 is as follows: first stand for 5 minutes, then charge at a constant current of 31.4A for 18 minutes, then stand for 5 minutes, then charge at a constant current of 51.4A for 139 minutes, and finally stand for 15 minutes.
[0014] Preferably, the temperature during high temperature standing in step 4 is 45°C.
[0015] Preferably, the full charging process in step 6 is as follows: first stand for 5 minutes, then charge to 3.65V with a constant current of 94.2A, then charge to 15.7A with a constant voltage of 3.65V, and finally stand for 5 minutes.
[0016] The present invention has the following advantages:
[0017] 1. The liquid injection method of the present application adopts three liquid injections: one injection to 80% of the reserved amount, vacuum pumping, a second injection to 85% of the reserved amount, standing before high temperature, formation, standing after high temperature, and three injections to the reserved amount, which can greatly improve the infiltration between the electrolyte and the electrode, shorten the standing time before high temperature formation, and reduce energy consumption.
[0018] 2. The fully charged interface of the battery cell obtained by the liquid injection method of the present invention presents a perfect golden color, which indicates that the negative pressure after one liquid injection can fully infiltrate the electrolyte and the electrode; while the battery cell obtained by the conventional liquid injection method has lithium precipitation on its fully charged interface. At the same time, the battery cell obtained by the present invention has better cycle performance. More importantly, this method can shorten the standing time before high temperature formation by several times, greatly reducing energy consumption in industrial production and improving efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic diagram of the negative electrode interface after full charge and disassembly after formation according to the present invention.
[0020] Figure 2 This is a 25°C@0.5P / 0.5P cycle performance diagram of the present invention. DETAILED DESCRIPTION
[0021] The specific implementation modes of the present invention are further explained in detail below by describing the embodiments with reference to the accompanying drawings, so as to help those skilled in the art to have a more complete, accurate and in-depth understanding of the concept and technical solution of the present invention.
[0022] Example 1
[0023] (1) In an environment of 25°C, take a 314Ah battery cell after baking, inject 900g of electrolyte normally, then let it stand for 1 hour. After the standing period, draw negative pressure for 2 hours and keep the pressure ≤-80kPa to allow the electrolyte and the electrode to fully penetrate.
[0024] (2) After the negative pressure is pumped out, the battery cell is injected with electrolyte to 960g, and then left to stand for 5 hours before high temperature, and the formation is carried out normally. The formation process is as follows: standing for 5 minutes → 31.4A constant current charging for 18 minutes → standing for 5 minutes → 51.4A constant current charging for 139 minutes → standing for 15 minutes;
[0025] After the formation is completed, the high temperature is allowed to stand for 8 hours, during which the temperature is 45°C.
[0026] (3) After the battery cell is aged for 8 hours, it is cooled to room temperature and then injected three times with electrolyte until the electrolyte reaches 1130 g, and then the sealing pins are welded;
[0027] Finally, fully charge it. The full charging process is as follows: let it stand for 5 minutes → charge at 94.2A constant current to 3.65V → charge at 3.65V constant voltage to 15.7A → let it stand for 5 minutes.
[0028] (4) Disassemble the above battery cells.
[0029] Comparative Example 1
[0030] (1) In an environment of 25°C, take another 314Ah battery cell after baking and inject 960g of electrolyte normally.
[0031] (2) After the above-mentioned battery cell was left standing at high temperature for 20 hours, it was formed normally. After the formation was completed, the formation process was as follows: standing for 5 minutes → 31.4A constant current charging for 10 minutes → standing for 5 minutes → 51.4A constant current charging for 139 minutes → standing for 15 minutes; standing for 8 hours after high temperature, wherein the temperature during high temperature standing was 45°C.
[0032] (3) After the battery cell is aged for 8 hours, it is cooled to room temperature and then injected with electrolyte to a retention volume of 1130 g, and then the sealing pins are welded;
[0033] Finally, fully charge it. The full charging process is as follows: let it stand for 5 minutes → charge at 94.2A constant current to 3.65V → charge at 3.65V constant voltage to 15.7A → let it stand for 5 minutes.
[0034] (4) Disassemble the above battery cells.
[0035] Experiments have shown that the battery cell obtained by the injection method of the present invention in Example 1 has a perfect golden yellow interface between the negative electrode plate, which indicates that the negative pressure after one injection can fully infiltrate the electrolyte and the electrode plate; while the battery cell obtained by the conventional injection method in Comparative Example 1 has lithium precipitation on its fully charged interface (such as the attached Figure 1 At the same time, the battery cell obtained by the present invention has a better cycle performance (as shown in the attached Figure 2 More importantly, the method can shorten the standing time before high temperature formation by several times, greatly reducing the energy consumption in industrial production and improving efficiency.
[0036] The present invention is described above by way of example in conjunction with the accompanying drawings. It is obvious that the specific implementation of the present invention is not limited to the above-mentioned method. As long as various non-substantial improvements are made using the concept and technical solution of the present invention, or the practical invention and technical solution are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A method for improving the wettability of lithium ion battery electrolyte, characterized in that: The following steps are involved: Step 1. In an environment of 25°C, take a 314Ah battery cell after baking, inject 900g of electrolyte normally, and then let it stand for 1 hour; Step 2: After standing still, draw negative pressure to allow the electrolyte and the electrode to fully infiltrate; Step 3: After the negative pressure is pumped out, the battery cell is injected with electrolyte for the second time, and the electrolyte is injected to 960g; Step 4: Then let it stand for 5 hours before high temperature and carry out the formation normally; Step 5: After the formation is completed, let it stand at high temperature for 8 hours; Step 6: After the battery cell is aged for 8 hours, it is cooled to room temperature and then filled three times with electrolyte until the holding amount is 1130g. The sealing pins are then welded and the battery cell is fully charged.
2. A method for improving the wettability of lithium ion battery electrolyte according to claim 1, characterized in that: In step 2, negative pressure is applied for 2 h and the pressure is maintained at ≤-80 kPa.
3. A method for improving the wettability of lithium ion battery electrolyte according to claim 1, characterized in that: The formation process in step 4 is as follows: first let it stand for 5 minutes, then charge it at a constant current of 31.4A for 18 minutes, then let it stand for another 5 minutes, then charge it at a constant current of 51.4A for 139 minutes, and finally let it stand for 15 minutes.
4. A method for improving the wettability of lithium ion battery electrolyte according to claim 1, characterized in that: The temperature during high temperature standing in step 4 is 45°C.
5. A method for improving the wettability of lithium ion battery electrolyte according to claim 1, characterized in that: The full charging process in step 6 is as follows: let it stand for 5 minutes, then charge to 3.65V with a constant current of 94.2A, then charge to 15.7A with a constant voltage of 3.65V, and finally let it stand for 5 minutes.
Citation Information
Cited By
Method for infiltrating alkali metal ion battery cell with electrolyte, formation method and battery cell
CN119833773A