Soft package lithium ion battery containing synchronous lithium plating reference electrode and preparation method of soft package lithium ion battery
By introducing an additional second positive electrode and an electrochemical lithium plating structure into the lithium-ion battery, the problem of long lithium plating time for the copper foil reference electrode during the preparation process of the lithium-ion battery, which affects lithium ion transmission and active lithium loss, is solved. Provides more efficient lithium plating and stable reference electrode.
Patent Information
- Application Number
- CN202410787650.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-18
AI Technical Summary
In the existing three-electrode system, copper foil is used as a reference electrode in the preparation process of lithium-ion batteries. There are problems such as long lithium plating time, affecting lithium ion transmission, irreversible loss of active lithium and stability of the reference electrode.
Using the design of a soft-pack lithium-ion battery, by introducing an additional second positive electrode and an electrochemical lithium plating structure, the reference electrode current collector is placed between the second positive electrodes, and the blank area is used for simultaneous lithium plating, shortening the lithium plating time and Improve lithium plating efficiency and avoid active lithium loss and reference electrode failure.
It reduces the lithium plating time by half, improves the lithium plating efficiency, reduces the loss of active lithium and stabilizes the reference electrode, and avoids the influence of the reference electrode on the charge and discharge process.
Smart Images

Figure CN118748274A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to a soft-package lithium ion battery containing a synchronous lithium-plating reference electrode and a preparation method thereof. Background Art
[0002] In 1913, Lewis, Keyes and others conducted electrochemical research on lithium metal and designed a classic three-electrode experiment. They accurately calculated the electrode potential of lithium, which opened the way for the electrochemical application of lithium metal and became the cornerstone of the development of lithium-ion batteries. In a two-electrode system, the counter electrode has a dual role and also plays the role of a reference electrode. However, in conventional tests, the counter electrode is often polarized due to the passage of current, resulting in a potential shift. At this time, the electrode potential fed back is the relative electrode potential. As a typical representative of a two-electrode system, the full-battery voltage change during the charge and discharge process of lithium-ion batteries is the change in the relative electrode potential of the positive and negative electrodes. It is impossible to accurately decouple the potential signals from the positive and negative electrodes, making it impossible to accurately interpret the electrochemical behavior of lithium-ion batteries during the charge and discharge process, making lithium-ion batteries a black box. By introducing a three-electrode system, the electrochemical behavior of the positive and negative electrodes can be accurately decoupled, and the reference electrode becomes a "key" to open the black box.
[0003] During the fast charging process, the slow kinetics of lithium insertion into the graphite negative electrode leads to severe polarization on the graphite negative electrode side, which reduces the negative electrode potential to 0 V (vs. Li / Li + ), while the graphite lithium insertion potential is about 0.1V (vs.Li / Li + ) Due to the existence of polarization, it is very easy to reach the lithium deposition potential threshold of 0V (vs.Li / Li + ), lithium metal is deposited on the surface of the graphite negative electrode. In the three-electrode system, the reference electrode is a stable electrode with known potential, high compatibility with the electrolyte, and no pollution. It can be used as a potential reference to effectively decouple the electrochemical information of the positive and negative electrodes. The three-electrode method monitors the negative electrode's potential to lithium (vs. Li / Li) during the battery charge and discharge process. + ), and then synchronously measure the occurrence of lithium deposition. Therefore, the three-electrode system has also become an in-situ non-destructive detection method for fast charging and lithium deposition, which plays an important role in effectively detecting the lithium deposition boundary of the fast charging process and optimizing the fast charging strategy. Commonly used reference electrodes in the three-electrode system of lithium-ion batteries include lithium sheets, in-situ lithium plating of copper wires, and alloy materials formed by lithium and metals.
[0004] Chinese patent CN 113889599A provides a method for preparing a perforated copper foil as a reference electrode for the lithium supplement part, by opening multiple rows of circular through holes of the same size and arranged at equal intervals on the copper foil, forming a copper foil with a special structure as a reference electrode, placed between the positive and negative electrode sheets and separated by a diaphragm, and firstly using a constant current to charge and plate lithium on the outer surface of the copper foil close to the positive electrode sheet for 5 hours, and then performing the same lithium plating operation on the outer surface close to the negative electrode sheet. Although this method can ensure effective lithium plating and uniform lithium plating thickness, the through holes can also facilitate the transmission of lithium ions during charging and discharging to a certain extent. However, the area without through holes will still hinder the transmission of lithium ions during charging and discharging, and this problem will not be completely avoided, and the single-sided lithium plating time is as long as 5 hours, and the lithium plating time of the entire reference electrode is relatively long. At the same time, the lithium plating process will consume the active lithium of the positive and negative electrodes, resulting in irreversible loss of lithium on the positive and negative electrodes.
[0005] Chinese patent CN 115132962A provides a method for preparing a reference electrode with a composite structure formed by superimposing copper foil and lithium foil, and a three-layer composite structure containing lithium foil layers on both sides of the copper foil surface is obtained by applying a fixed pressure on both sides of the copper foil to roll the lithium foil. This design fixes the lithium foil on the copper foil by rolling, ensuring sufficient lithium on the reference electrode, but the direct use of lithium foil for preparation has stricter environmental requirements. The preparation process needs to prevent the oxidation of lithium foil. At the same time, the lithium foil and the copper foil are combined by physical means. If they cannot be effectively bonded and the post-process operation of the battery cell preparation will bring the risk of lithium foil falling off, causing the reference electrode to fail. Compared with electrochemical deposition lithium plating, this scheme cannot be plated with lithium twice. Once there is a problem with the combination of lithium foil and copper foil, it will cause the potential to be unstable and the risk of failure of the entire three-electrode system will increase.
[0006] Therefore, the following problems need to be solved when using copper foil as the reference electrode of the three-electrode system: 1. It should not affect the transmission of lithium ions during the charge and discharge process; 2. The efficiency of electrochemical deposition of positive and negative lithium plating needs to be further improved; 3. The irreversible loss of active lithium from the positive and negative electrodes should be avoided as much as possible during the electrochemical deposition of lithium plating. 4. The bond between lithium and the metal copper matrix should be tight to avoid failure of the reference electrode and ensure that the reference electrode can be reused. Summary of the invention
[0007] Based on the shortcomings of the existing preparation technology, in order to solve the problems existing in the previous three-electrode preparation process, the present invention is inspired by the structure of the soft-pack lithium-ion battery cell and provides a soft-pack lithium-ion battery containing a synchronous lithium-plating reference electrode and a preparation method thereof. The preparation method of this invention can realize the rapid preparation of the soft-pack lithium-ion battery reference electrode, and can effectively shorten the electrochemical lithium plating time by half under the same lithium plating experimental conditions, thereby improving the efficiency of electrochemical lithium plating.
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] In a first aspect, a soft-pack lithium-ion battery containing a simultaneous lithium-plating reference electrode, wherein the interior of the soft-pack lithium-ion battery includes a laminated battery core and an electrochemical lithium-plating structure arranged on the outer side of the laminated battery core, wherein the laminated battery core includes a plurality of first positive electrodes and negative electrodes alternately laminated; the electrochemical lithium-plating structure includes two second positive electrodes and a reference electrode current collector located between the two second positive electrodes, wherein blank areas for lithium plating are provided on both surfaces of the reference electrode current collector opposite to the two second positive electrodes, wherein the blank areas can be respectively used as lithium sources with their corresponding second positive electrodes, and lithium layers are simultaneously deposited by electrochemical lithium plating to obtain reference electrodes with lithium plated on both back-to-back surfaces; the first positive electrode, negative electrode, second positive electrode and reference electrode are separated from each other by a diaphragm, or at least one side of each other is coated with a diaphragm to separate them from each other.
[0010] Further, the first positive electrode and the second positive electrode are completely identical except for the size;
[0011] And / or, the length and width of the diaphragm are both 0.2-1.5 mm greater than the length and width of the pole pieces it separates and / or covers.
[0012] Furthermore, the maximum cross-sectional area of the first positive electrode is greater than the maximum cross-sectional area of the second positive electrode, and the maximum cross-sectional area of the second positive electrode is greater than the maximum cross-sectional area of the reference electrode;
[0013] And / or, the diaphragm includes a first diaphragm, a second diaphragm and a third diaphragm, the first diaphragm is used to separate / cover the first positive electrode and / or negative electrode; the second diaphragm is used to separate / cover the second positive electrode; the third diaphragm is used to separate / cover the reference electrode.
[0014] Further, the reference electrode current collector comprises copper foil and / or copper wire;
[0015] And / or, a reference electrode lug is provided on the reference electrode;
[0016] And / or, a first positive electrode tab is provided on the first positive electrode;
[0017] And / or, a negative electrode tab is provided on the negative electrode;
[0018] And / or, a second positive electrode tab is provided on the second positive electrode.
[0019] Further, the reference electrode current collector comprises copper foil and copper wire;
[0020] And / or, the copper wire is an enameled copper wire, and its wire diameter is 40 μm to 60 μm;
[0021] And / or, the copper foil has a thickness of 5 μm to 10 μm;
[0022] and / or, a portion of the reference electrode current collector other than the blank area is covered with an adhesive tape;
[0023] And / or, the first positive electrode tab is parallel to the negative electrode tab, the reference electrode tab is parallel to the second positive electrode tab, and the second positive electrode tab is perpendicular to the first positive electrode tab.
[0024] Furthermore, the blank area is located on the surface of one end of the copper foil away from the copper wire, and the area of the blank area occupies 1 / 5 to 1 / 2 of the entire surface area of the copper foil;
[0025] And / or, the tape material is one of PET, MOPP and PI;
[0026] And / or, the reference electrode tab is made of nickel-plated copper;
[0027] And / or, the material of the second positive electrode tab is aluminum.
[0028] In a second aspect, a method for preparing the soft-pack lithium-ion battery comprises the following steps:
[0029] S1, alternately stacking a plurality of first positive electrodes, separators and negative electrodes to form a stacked battery cell;
[0030] S2, placing the blank area of the reference electrode current collector between the two second positive electrodes, and separating the three by a diaphragm to form an electrochemical lithium plating structure;
[0031] S3, placing the electrochemical lithium plating structure on one side of the laminated battery core, leading out the reference electrode current collector and the second positive electrode tab before packaging to enable electrochemical lithium plating connection, and obtaining an intermediate product after packaging;
[0032] S4, baking, liquid injection, standing, chemical formation, and volume separation of the intermediate product; then electrochemically plating lithium on the reference electrode current collector to obtain a reference electrode and a soft-pack lithium-ion battery.
[0033] Further, in step S1, after lamination, a first positive electrode tab is provided on the first positive electrode, and a negative electrode tab is provided on the negative electrode, and both the first positive electrode tab and the negative electrode tab are led out from the top of the laminated battery cell;
[0034] And / or, in step S2, the reference electrode current collector includes a copper foil with a blank area and a copper wire welded on the copper foil, and the second positive electrode is obtained by cutting and shrinking two other first positive electrodes, and the two second positive electrodes are welded with second positive electrode tabs; in step S3, the electrochemical lithium plating structure is arranged on one side of the laminated battery core, and then the copper wire and the second positive electrode tab are led out from the side of the laminated battery core;
[0035] And / or, in step S4, the working current I=Ai selected during the electrochemical lithium plating, wherein the current density is i, i=7.0-10.0 μA / mm 2 The area of the blank area is A, A = 0.4 ~ 1.2cm 2 ;
[0036] And / or, in step S4, the time of the electrochemical lithium plating is 1 to 4 hours.
[0037] Furthermore, in step S2, the copper wire is an enameled copper wire, the enameled copper wire is partially depainted with a strong acid solution, and is cleaned, impurities removed, and dried for standby use; the copper foil is cut to a suitable size, cleaned to remove the surface oxide layer, and then dried for standby use; finally, the standby copper wire and the copper foil are welded together, and a blank area is reserved on the top surface of the copper foil away from the copper wire for subsequent lithium plating, and the remaining area to the welding area is coated with tape;
[0038] And / or, before the electrochemical lithium plating, a reference electrode tab is arranged on the copper wire.
[0039] Furthermore, the electrochemical lithium plating structure, and / or the reference electrode tab, and / or the first positive electrode tab, and / or the negative electrode tab, and / or the second positive electrode tab are all fixed by tab glue or tape.
[0040] Compared with the prior art, the present invention has at least the following beneficial effects:
[0041] The soft-pack lithium-ion battery of the present invention has a multi-electrode system. Specifically, on the basis of a laminated battery cell, two second positive electrodes are additionally introduced to construct an electrochemical lithium plating structure system of the second positive electrode, a diaphragm, a reference electrode current collector, a diaphragm, and a second positive electrode, and the system is placed at the outermost layer of the battery cell. The system composed of the two second positive electrodes and the reference electrode current collector is used as an auxiliary lithium plating structure to achieve efficient lithium plating of a current collector such as copper foil or copper wire. The soft-package lithium-ion battery containing a synchronous lithium-plated reference electrode constructed by the present invention solves some problems caused by the preparation of a current collector such as copper foil as a reference electrode for a three-electrode system. The work of the present invention has the following outstanding advantages: First, from the perspective of the traditional three-electrode system structure, most of them place copper foil, copper wire, etc. between the positive and negative electrodes inside the battery cell and use a diaphragm for isolation. Since the copper wire or copper foil needs to have a layer of lithium deposited on the surface (lithium plating) to serve as a reference electrode with stable potential, it is necessary to charge before deposition to embed a certain amount of lithium in the negative electrode, so as to ensure that there is sufficient lithium source for reverse lithium plating. At the same time, the lithium plating process requires forward lithium plating between the positive electrode and the copper foil first. After the forward lithium plating is completed, reverse lithium plating is required between the negative electrode and the copper foil for the same time. The entire lithium plating process takes a long time. In the present invention, by introducing two additional positive electrode sheets and placing a current collector such as copper foil between the two positive electrode sheets, lithium plating can be achieved on different sides of the copper foil at the same time, and the electrochemical lithium plating time can be shortened by half while ensuring the same lithium layer thickness. Second, in the traditional placement method, the larger area of the copper foil will affect the transmission of lithium ions during the charging and discharging process. In particular, during the fast-charging high-rate (high-current) test, the copper foil will hinder the lithium ion transmission rate between the positive and negative electrodes, thereby affecting the fast-charging high-rate lithium plating test results. In this invention, the reference electrode is placed outside the battery body to avoid the influence of the reference electrode on the charging and discharging process. Third, by introducing an additional positive electrode sheet, the entire auxiliary lithium plating structure is placed outside the main battery cell. During the lithium plating process, the lithium source comes from the introduced positive electrode sheet, which avoids the loss of active lithium in the main battery cell. The lithium plating process of copper foil or copper wire will cause the capacity of the battery cell to decrease, affecting the capacity. This solution effectively avoids this shortcoming and greatly avoids the influence of the reference electrode on the battery cell body. Fourthly, since the lithium layer on the copper foil is deposited in situ by later electrochemical deposition, compared with other lithium foils and copper foils that are combined by physical methods such as rolling, the present invention is more stable in structure. At the same time, in the event that the lithium layer falls off, the reference electrode can be restored to stability through secondary electrochemical deposition, thereby ensuring the stability and reuse of the reference electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0043] Figure 1 This is a structural diagram of the appearance of the soft-pack lithium-ion battery of the present invention;
[0044] Figure 2 This is a diagram showing the internal structure of the soft-pack lithium-ion battery of the present invention;
[0045] Figure 3 This is an enlarged view of the local structure of the reference electrode of the present invention;
[0046] Figure 4 This is a lithium plating curve diagram of the reference electrode of the present invention;
[0047] Figure 5 This is a stability test diagram of the reference electrode of the present invention after lithium plating;
[0048] Figure 6 This is a test diagram of the negative electrode potential during the charging process of the soft-pack lithium-ion battery of the present invention.
[0049] Icon: 1-first diaphragm; 2-first positive electrode; 3-negative electrode; 4-second positive electrode; 5-reference electrode; 6-first positive electrode tab; 7-negative electrode tab; 8-second positive electrode tab; 9-tab glue; 10-reference electrode tab; 11-third diaphragm; 12-second diaphragm; 13-tape; 14-copper wire; 15-copper foil. DETAILED DESCRIPTION
[0050] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.
[0051] In the description of the present invention, the terms "back to back", "vertical", "upper", "lower", "parallel", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and do not require that the present invention must be constructed and operated in a specific orientation. Therefore, they should not be understood as limitations on the present invention. The terms "connected", "connected", and "set" used in the present invention should be understood in a broad sense. For example, it can be a fixed connection or a detachable connection; it can be a direct connection or an indirect connection through an intermediate component; it can be a wired electrical connection, a radio connection, or a wireless communication signal connection. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.
[0052] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0053] According to a first aspect of the present invention, a soft-pack lithium-ion battery containing a synchronous lithium-plated reference electrode, the interior of the soft-pack lithium-ion battery includes a laminated battery core and an electrochemical lithium-plating structure arranged on the outer side of the laminated battery core, the laminated battery core includes a plurality of first positive electrodes and negative electrodes of alternating laminates; the electrochemical lithium-plating structure includes two second positive electrodes and a reference electrode current collector located between the two second positive electrodes, blank areas for lithium plating are provided on both surfaces of the reference electrode current collector relative to the two second positive electrodes, the blank areas can be used as lithium sources with their corresponding second positive electrodes respectively, and lithium layers are deposited synchronously through electrochemical lithium plating to obtain reference electrodes with lithium plated on both back-to-back surfaces; the first positive electrode, negative electrode, second positive electrode and reference electrode are separated from each other by a diaphragm, or at least one side of each other is coated with a diaphragm to separate them from each other.
[0054] The present invention designs a multi-electrode structure based on the simultaneous positive and negative lithium plating of a reference electrode on the basis of a laminated core soft-pack lithium ion battery, specifically by introducing two additional positive electrode sheets on the side of the laminated core, that is, in the space between the outermost negative electrode of the laminated core and the shell or between the outermost positive electrode of the laminated core and the shell, and placing a reference electrode current collector such as a copper substrate (copper foil, copper wire, etc.) between the two positive electrode sheets, so that different surfaces of the copper substrate can be simultaneously plated with lithium to form a reference electrode, achieving the purpose of in-situ simultaneous lithium plating, and the electrochemical lithium plating time can be shortened by half under the premise of ensuring the same lithium layer thickness, thereby improving the efficiency of electrochemical deposition lithium plating. Moreover, lithium is in-situ loaded on the copper substrate by electrochemical deposition, ensuring the close combination of lithium and the copper substrate. At the same time, the copper substrate, especially the copper foil, is placed on the outside of the laminated battery cell, that is, the space between the laminated battery cell and the shell such as the aluminum-plastic film. Under the premise of ensuring the lithium plating of the copper foil, the problem of hindering the lithium ion transmission between the positive and negative electrodes during the charging and discharging process caused by the excessive specific surface area of the copper foil is solved, and the influence of the introduction of the copper foil on the electrochemical performance of the battery cell is reduced. The introduction of the additional positive electrode provides a sufficient lithium source for lithium plating, which can reduce the irreversible loss of active lithium caused by electrochemical lithium plating. Furthermore, when the copper substrate is made of copper foil, its lithium plating area is much larger than that of copper wire, so its lithium plating amount is also easily much higher than that of copper wire, and the service life of the reference electrode after lithium plating can be greatly improved.
[0055] In the present invention, the diaphragm is used to block the pole pieces to avoid short circuit caused by contact between the pole pieces, so there is no special limitation on its size, as long as it can completely separate and / or cover (separate / cover) the pole pieces. Usually, the length and width of the diaphragm are 0.2-1.5mm larger than the length and width of the pole pieces it separates and / or covers. Considering an optional implementation of the soft-pack lithium-ion battery of the present invention, the first positive electrode and the second positive electrode are exactly the same except for the size (completely the same means that the positive electrode material, surface density, current collector thickness, etc. on the second positive electrode sheet are exactly the same as the positive electrode sheet (first positive electrode sheet) in the original battery system (laminated cell), and the maximum cross-sectional area of the first positive electrode sheet is larger than the maximum cross-sectional area of the second positive electrode sheet. Furthermore, the second positive electrode sheet is obtained by cutting the first positive electrode sheet. Specifically, after cutting, the length L1 of the second positive electrode sheet is 3.0cm~4.0cm, and the width W1 is 3.5cm~4.5cm, so The length L3 of the diaphragm covering one or both sides thereof is 3.2cm to 4.2cm, and the width W3 of the diaphragm is 3.7cm to 4.7cm. In this way, it is possible to realize the additional provision of lithium source for lithium plating, and it is possible to not change the packaging production of the original battery, which is convenient for the sealing packaging of the entire battery). Therefore, as a further optional embodiment of the soft-pack lithium-ion battery of the present invention, the diaphragm includes a first diaphragm, a second diaphragm and a third diaphragm, the first diaphragm is used to separate / cover the first positive electrode and / or negative electrode; the second diaphragm is used to separate / cover the second positive electrode; the third diaphragm is used to separate / cover the reference electrode. Furthermore, since the maximum cross-sectional area of the first positive electrode is greater than the maximum cross-sectional area of the second positive electrode, and the maximum cross-sectional area of the second positive electrode is greater than the maximum cross-sectional area of the reference electrode, the maximum cross-sectional area of the first diaphragm is greater than the maximum cross-sectional area of the second diaphragm, and the maximum cross-sectional area of the second diaphragm is not less than the maximum cross-sectional area of the third diaphragm. Furthermore, the maximum cross-sectional area of the second diaphragm is greater than the maximum cross-sectional area of the third diaphragm, so that the third diaphragm can both shield the copper substrate, especially the copper foil, and facilitate the insertion operation to separate the copper substrate and the positive electrode sheet.In the present invention, the separation and / or coating of the electrodes by the diaphragm can be specifically as follows: the structural arrangement from one side to the other side of the battery housing can be the second diaphragm, the second positive electrode, the second diaphragm, the reference electrode, the third diaphragm, the second positive electrode, the first diaphragm, the negative electrode, the first diaphragm, the first positive electrode, the first diaphragm, the negative electrode, the first diaphragm, the first positive electrode, ..., the first diaphragm; it can also be the second diaphragm, the second positive electrode, the second diaphragm, the reference electrode, the third diaphragm, the second positive electrode, the first diaphragm, the first positive electrode, the first diaphragm, the negative ... first positive electrode, the first diaphragm, the first positive electrode, the first diaphragm, the first positive electrode, the A diaphragm, a first positive electrode, a first diaphragm, a negative electrode, ..., a first diaphragm; it can also be the first diaphragm, a negative electrode, the first diaphragm, the first positive electrode, the first diaphragm, the negative electrode, ... the first positive electrode, the first diaphragm, the second positive electrode, the second diaphragm, a reference electrode, the third diaphragm, the second positive electrode, the second diaphragm; it can also be the first diaphragm, the first positive electrode, the first diaphragm, the negative electrode, the first diaphragm, the first positive electrode, the first diaphragm..., the negative electrode, the first diaphragm, the second positive electrode, the second diaphragm, the reference electrode, the third diaphragm, the second positive electrode, the second diaphragm.
[0056] As an optional embodiment of the soft-pack lithium-ion battery of the present invention, the reference electrode current collector includes copper foil and / or copper wire. Further, the reference electrode current collector includes copper foil and copper wire, and the connection method of the copper foil and the copper wire is not particularly limited. The two can be mutually conductive. Specifically, ultrasonic welding and other existing technologies can be used to weld them. Further, the copper wire is an enameled copper wire with a wire diameter of 40μm to 60μm; and / or, the thickness of the copper foil is 5μm to 10μm, and after cutting, its length L4 is 2.5 to 3.5cm, and the width W4 is 0.5 to 1.0cm, and a blank area is reserved on it for lithium plating. Further, the blank area is on the surface of one end of the copper foil away from the copper wire, and the area of the blank area accounts for 1 / 5 to 1 / 2 of the entire surface area of the copper foil. Specifically, the length L5 of the blank area is 0.8 to 1.2m, and the width W4 is 0.5 to 1.0cm. Furthermore, the size of the third diaphragm is set according to the size of the copper foil and the blank area, and its length L2 is set to 3.8 cm to 4.0 cm, and the diaphragm width W2 is set to 1.5 cm to 2.0 cm.
[0057] As an optional embodiment of the soft-pack lithium-ion battery of the present invention, the reference electrode current collector is partially covered with a tape except for the blank area. Furthermore, the tape is made of one of PET, MOPP and PI.
[0058] As an optional embodiment of the soft-pack lithium-ion battery of the present invention, a reference electrode tab is provided on the reference electrode; and / or a first positive electrode tab is provided on the first positive electrode; and / or a negative electrode tab is provided on the negative electrode;
[0059] And / or, a second positive electrode tab is disposed on the second positive electrode. Further, the first positive electrode tab is parallel to the negative electrode tab, the reference electrode tab is parallel to the second positive electrode tab, and the second positive electrode tab is perpendicular to the first positive electrode tab; that is, the first positive electrode tab and the negative electrode tab are disposed on the first side of the soft-pack lithium-ion battery, the reference electrode tab and the second positive electrode tab are disposed on the second side of the soft-pack lithium-ion battery, and the first side is perpendicular to the second side;
[0060] And / or, the reference electrode tab is made of nickel-plated copper; and / or, the second positive electrode tab is made of aluminum.
[0061] According to a second aspect of the present invention, a method for preparing the soft-pack lithium-ion battery comprises the following steps:
[0062] S1, alternately stacking a plurality of first positive electrodes, separators and negative electrodes to form a stacked battery cell;
[0063] S2, placing the blank area of the reference electrode current collector between the two second positive electrodes, and separating the three by a diaphragm to form an electrochemical lithium plating structure;
[0064] S3, placing the electrochemical lithium plating structure on one side of the laminated battery core, leading out the reference electrode current collector and the second positive electrode tab before packaging to enable electrochemical lithium plating connection, and obtaining an intermediate product after packaging;
[0065] S4, baking, liquid injection, standing, chemical formation, and volume separation of the intermediate product; then electrochemically plating lithium on the reference electrode current collector to obtain a reference electrode and a soft-pack lithium-ion battery.
[0066] As an optional implementation of the preparation method of the present invention, in step S1, after lamination, a first positive electrode tab is provided on the first positive electrode, and a negative electrode tab is provided on the negative electrode, and both the first positive electrode tab and the negative electrode tab are led out from the top of the laminated battery cell;
[0067] And / or, in step S2, the reference electrode current collector includes a copper foil with a blank area and a copper wire welded to the copper foil, and the second positive electrode is obtained by cutting and shrinking two other first positive electrodes, and the two second positive electrodes are welded with second positive electrode tabs; further, ultrasonic welding is selected as the welding method between the second positive electrode and the second positive electrode tab; in step S3, the electrochemical lithium plating structure is arranged on one side of the laminated battery core, and then the copper wire and the second positive electrode tab are led out from the side of the laminated battery core;
[0068] And / or, in step S4, the working current I=Ai selected during the electrochemical lithium plating, wherein the current density is i, i=7.0-10.0 μA / mm 2The area of the blank area is A, A = 0.4 ~ 1.2cm 2 ;
[0069] And / or, in step S4, the time of the electrochemical lithium plating is 1 to 4 hours.
[0070] As an optional implementation of the preparation method of the present invention, in step S2, the copper wire is an enameled copper wire, the enameled copper wire is partially depainted with a strong acid solution, and is cleaned, impurities removed, and dried for standby use; the copper foil is cut to a suitable size, cleaned to remove the surface oxide layer, and then dried for standby use; finally, the standby copper wire and the copper foil are welded together, and a blank area is reserved on the top surface of the copper foil away from the copper wire for subsequent lithium plating, and the remaining area to the welding area is coated with tape; further, concentrated sulfuric acid is selected as the strong acid solution, dilute hydrochloric acid and ultrapure water are selected for cleaning impurities and oxide layers, and the drying temperature is selected at 30 to 50°C;
[0071] And / or, before the electrochemical lithium plating, a reference electrode tab is arranged on the copper wire, and further, the reference electrode tab is soldered by electric soldering iron.
[0072] As an optional embodiment of the preparation method of the present invention, the electrochemical lithium plating structure, and / or the reference electrode tab, and / or the first positive electrode tab, and / or the negative electrode tab, and / or the second positive electrode tab are all fixed by tab glue or tape.
[0073] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.
[0074] Example 1
[0075] A soft-pack lithium-ion battery containing a simultaneously plated lithium reference electrode, such as Figure 1 , 2As shown, the interior of the soft-pack lithium-ion battery includes a laminated battery core and an electrochemical lithium plating structure arranged on the outer side of the laminated battery core, the laminated battery core includes a plurality of alternately laminated first positive electrodes 2 and negative electrodes 3, a first positive electrode tab 6 is arranged on the first positive electrode 2, and a negative electrode tab 7 is arranged on the negative electrode 3, and the first positive electrode tab 6 is parallel to the negative electrode tab 7; the electrochemical lithium plating structure includes two second positive electrodes 4 and a reference electrode current collector located between the two second positive electrodes 4, and blank areas for lithium plating are provided on both surfaces of the reference electrode current collector relative to the two second positive electrodes 4, and the blank areas can be respectively used as the second positive electrodes 4 corresponding to the first positive electrode 4. A lithium source is subjected to electrochemical lithium plating and a lithium layer is deposited simultaneously to obtain two reference electrodes 5 with lithium plated on their back surfaces. A reference electrode ear 10 made of nickel-plated copper is arranged on the reference electrode 5, and the reference electrode ear 10 is parallel to the second positive electrode ear 8. A second positive electrode ear 8 made of aluminum is arranged on the second positive electrode 4, and the second positive electrode ear 8 is perpendicular to the first positive electrode ear 6. The first positive electrode 2, the negative electrode 3, the second positive electrode 4 and the reference electrode 5 are separated from each other by a diaphragm, or at least one side of each other is coated with a diaphragm to separate each other, and the length and width of the diaphragm are both larger than the length and width of the electrode separated and / or coated by it by 0.2-1.5mm.
[0076] Specifically, Figure 2 As shown, the second positive electrode 4 is completely identical to the first positive electrode 2 except for the size, and the maximum cross-sectional area of the second positive electrode 4 is smaller than the maximum cross-sectional area of the first positive electrode 2. The pole piece length L1 of the second positive electrode 4 is 3.0 cm to 4.0 cm, and the width W1 is 3.5 cm to 4.5 cm;
[0077] For example Figure 2 As shown, the maximum cross-sectional area of the reference electrode 5 is smaller than the maximum cross-sectional area of the second positive electrode 4, the reference electrode current collector comprises a copper foil 15 and a copper wire 14, the copper wire 14 is an enameled copper wire, and its wire diameter is 40 μm to 60 μm; the copper foil 15 is 5 μm to 10 μm thick, the length L4 is 2.5 to 3.5 cm, and the width W4 is 0.5 to 1.0 cm; the blank area is on the surface of one end of the copper foil 15 away from the copper wire 14, and the length L5 of the blank area is 0.8 to 1.2 m, and the width W4 is 0.5 to 1.0 cm; the portion of the reference electrode current collector other than the blank area is covered with a tape 13, and the material of the tape 13 is one of PET, MOPP and PI;
[0078] For example Figure 2 As shown, the diaphragm includes a first diaphragm 1, a second diaphragm 12 and a third diaphragm 11. The first diaphragm 1 is used to separate / cover the first positive electrode 2 and / or the negative electrode 3; the second diaphragm 12 is used to separate / cover the second positive electrode 4; the third diaphragm 11 is used to separate / cover the reference electrode 5, and the length L2 of the third diaphragm is 3.8 cm to 4.0 cm, and the diaphragm width W2 is 1.5 cm to 2.0 cm.
[0079] The method for preparing the soft-pack lithium-ion battery of this embodiment comprises the following steps:
[0080] S1, stacking a plurality of first positive electrodes 2, first separators 1 and negative electrodes 3 alternately in the order of first separator 1, negative electrode 3, first separator 1, first positive electrode 2, first separator 1, negative electrode 3... to form a laminated battery cell; and after stacking, a first positive electrode tab 6 is arranged on the first positive electrode 2, and a negative electrode tab 7 is arranged on the negative electrode 3, and the first positive electrode tab 6 and the negative electrode tab 7 are both led out from the top of the laminated battery cell;
[0081] S2, partially depaint the enameled copper wire with a strong acid solution, and then clean, remove impurities, and dry it for use; at the same time, cut the copper foil 15 to a suitable size, clean it to remove the surface oxide layer, and then dry it for use; finally, ultrasonically weld the spare copper wire 14 and the copper foil 15 together, and reserve a blank area on the top of the copper foil 15 for subsequent lithium plating, and use the tape 13 to wrap the remaining area to the welding area to obtain a reference electrode current collector; wherein, concentrated sulfuric acid is selected as the strong acid solution, dilute hydrochloric acid and ultrapure water are selected to clean impurities and oxide layers, and the drying temperature is selected at 30-50°C;
[0082] The second positive electrode 4 is obtained by cutting and shrinking two pieces of the first positive electrode 2, and is separated by the second separator 12 to form a laminated structure of the second separator 12, the second positive electrode 4, the second separator 12, and the second positive electrode 4; at the same time, the second positive electrode tab 8 is welded to the two second positive electrodes 4 by ultrasonic welding;
[0083] The blank area of the reference electrode current collector is placed between the two second positive electrodes 4, separated by the second separator 12 on one side and the third separator 11 on the other side, to form an electrochemical lithium plating structure;
[0084] S3, the electrochemical lithium plating structure is fixed on one side of the laminated battery core by side sealing with the tab glue 9, the laminated battery core and the electrochemical lithium plating structure are top-side sealed with the aluminum-plastic film after shell punching, and the copper wire 14 and the second positive electrode tab 8 are led out from the side to enable electrochemical lithium plating, and after packaging, the reference electrode tab 10 is soldered to the copper wire 14 by electric soldering to obtain an intermediate product;
[0085] S4, fix the reference electrode tab 10 by the tape 13, and fix the second positive electrode tab 8 by the tab glue 9, then bake the intermediate product, inject liquid, stand, form, divide the volume, and electrochemically plate lithium on the reference electrode current collector, select the working current I = Ai, where the current density is i = 7.0 ~ 10.0μA / mm 2 , the area of the blank area is A = 0.4 ~ 1.2 cm 2 After electrochemical lithium plating for 1 to 4 hours, a reference electrode 5 is obtained, and a soft-pack lithium-ion battery is obtained at the same time.
[0086] Figure 3 The reference electrode is simultaneously plated with lithium using a current of 0.28 mA to 1.2 mA. The lithium plating curve remains stable within the lithium plating time after 0.5 h, indicating that positive and negative simultaneous lithium plating can be achieved on the copper foil 15 by electrochemical deposition.
[0087] Figure 4 After lithium plating, the battery was left to stand for more than 12 hours, and then the open circuit voltage between the negative electrode and the reference electrode was monitored in real time. It was found that the voltage value changed little, only within 1mV, and stabilized at 0.1711V after 19 hours, indicating that the potential of the entire reference electrode can be stable, and the potential changes little over time, which can meet the use conditions of the reference electrode.
[0088] Figure 5 By using the reference electrode to monitor the negative electrode potential in real time during the charging process, the potential change information of the negative electrode during the charging process is obtained. Table 1 shows the negative electrode-reference potential information under different SOC states and different charging rates during the charging process, which realizes the dynamic monitoring of the negative electrode potential and effectively decouples the negative electrode potential information from the full battery voltage information for analysis. The specific Table 1 is as follows:
[0089] Table 1 Potential under different SOC states
[0090] SOC(%) Magnification (C) Full battery voltage (V) Negative electrode-reference potential (mV) 10% 1C 3.29 174.5 50% 1C 3.40 72.5 80% 1C 3.45 38.0 90% 1C 3.49 18.0 96% 0.5C 3.46 31.0 100% 0.2C 3.65 67.0
[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A soft-pack lithium-ion battery containing a synchronous lithium-plating reference electrode, characterized in that: The soft-pack lithium-ion battery comprises a laminated core and an electrochemical lithium plating structure arranged on the outer side of the laminated core. The laminated core comprises a plurality of alternately laminated first positive electrodes (2) and negative electrodes (3); the electrochemical lithium plating structure comprises two second positive electrodes (4) and a reference electrode current collector located between the two second positive electrodes (4); blank areas for lithium plating are provided on both surfaces of the reference electrode current collector opposite to the two second positive electrodes (4); the blank areas can use the corresponding second positive electrodes (4) as lithium sources, and a lithium layer is deposited synchronously through electrochemical lithium plating to obtain a reference electrode (5) with lithium plated on both back-to-back surfaces; the first positive electrode (2), the negative electrode (3), the second positive electrode (4) and the reference electrode (5) are separated from each other by a diaphragm, or at least one side of each other is coated with a diaphragm to separate each other.
2. The soft-pack lithium-ion battery according to claim 1, characterized in that: The first positive electrode (2) and the second positive electrode (4) are completely identical except for the size; And / or, the length and width of the diaphragm are both 0.2-1.5 mm greater than the length and width of the pole pieces it separates and / or covers.
3. The soft-pack lithium-ion battery according to claim 2, characterized in that: The maximum cross-sectional area of the first positive electrode (2) is greater than the maximum cross-sectional area of the second positive electrode (4), and the maximum cross-sectional area of the second positive electrode (4) is greater than the maximum cross-sectional area of the reference electrode (5); And / or, the diaphragm comprises a first diaphragm (1), a second diaphragm (12) and a third diaphragm (11), wherein the first diaphragm (1) is used to separate / cover the first positive electrode (2) and / or negative electrode (3); the second diaphragm (12) is used to separate / cover the second positive electrode (4); and the third diaphragm (11) is used to separate / cover the reference electrode (5).
4. The soft-pack lithium-ion battery according to claim 1, characterized in that: The reference electrode current collector comprises copper foil (15) and / or copper wire (14); And / or, a reference electrode tab (10) is provided on the reference electrode (5); And / or, a first positive electrode tab (6) is provided on the first positive electrode (2); And / or, a negative electrode tab (7) is provided on the negative electrode (3); And / or, a second positive electrode tab (8) is provided on the second positive electrode (4).
5. The soft-pack lithium-ion battery according to claim 1 or 4, characterized in that: The reference electrode current collector comprises a copper foil (15) and a copper wire (14); And / or, the copper wire (14) is an enameled copper wire, and its wire diameter is 40 μm to 60 μm; And / or, the copper foil (15) has a thickness of 5 μm to 10 μm; and / or, a portion of the reference electrode current collector other than the blank area is covered by an adhesive tape (13); And / or, the first positive electrode tab (6) is parallel to the negative electrode tab (7), the reference electrode tab (10) is parallel to the second positive electrode tab (8), and the second positive electrode tab (8) is perpendicular to the first positive electrode tab (6).
6. The soft-pack lithium-ion battery according to claim 5, characterized in that: The blank area is located on the surface of one end of the copper foil (15) away from the copper wire (14), and the area of the blank area occupies 1 / 5 to 1 / 2 of the entire surface area of the copper foil (15); And / or, the adhesive tape (13) is made of one of PET, MOPP and PI; And / or, the reference electrode tab (10) is made of nickel-plated copper; And / or, the material of the second positive electrode tab (8) is aluminum.
7. A method for preparing a soft-pack lithium-ion battery as claimed in any one of claims 1 to 6, characterized in that: The following steps are involved: S1, alternately stacking a plurality of first positive electrodes (2), separators and negative electrodes (3) to form a stacked battery cell; S2, placing the blank area of the reference electrode current collector between the two second positive electrodes (4), and separating the three by a diaphragm to form an electrochemical lithium plating structure; S3, arranging the electrochemical lithium plating structure on one side of the laminated battery core, leading out the reference electrode current collector and the second positive electrode (4) tab before packaging to enable electrochemical lithium plating connection, and obtaining an intermediate product after packaging; S4, baking, liquid injection, standing, chemical formation, and volume separation of the intermediate product; then electrochemically plating lithium on the reference electrode current collector to obtain a reference electrode (5), and at the same time obtain a soft-pack lithium-ion battery.
8. The preparation method according to claim 7, characterized in that: In step S1, after lamination, a first positive electrode tab (6) is provided on the first positive electrode (2), and a negative electrode tab (7) is provided on the negative electrode (3), and both the first positive electrode tab (6) and the negative electrode tab (7) are led out from the top of the laminated battery cell; And / or, in step S2, the reference electrode current collector comprises a copper foil (15) provided with a blank area and a copper wire (14) welded to the copper foil (15), and the second positive electrode (4) is obtained by cutting and shrinking two other first positive electrodes (2), and the two second positive electrodes (4) are welded with second positive electrode tabs (8); in step S3, the electrochemical lithium plating structure is arranged on one side of the laminated battery core, and then the copper wire (14) and the second positive electrode tab (8) are both led out from the side of the laminated battery core; And / or, in step S4, the working current I=Ai selected during the electrochemical lithium plating, wherein the current density is i, i=7.0-10.0 μA / mm 2 The area of the blank area is A, A = 0.4 ~ 1.2cm 2 ; And / or, in step S4, the time of the electrochemical lithium plating is 1 to 4 hours.
9. The preparation method according to claim 8, characterized in that: In step S2, the copper wire (14) is an enameled copper wire, which is partially depainted with a strong acid solution, cleaned, decontaminated, and dried for later use; the copper foil (15) is cut to a suitable size, cleaned to remove the surface oxide layer, and then dried for later use; finally, the spare copper wire (14) and the copper foil (15) are welded together, and a blank area is reserved on the top surface of the copper foil (15) away from the copper wire for subsequent lithium plating, and the remaining area to the welding area is coated with an adhesive tape (13); And / or, before the electrochemical lithium plating, a reference electrode tab (10) is arranged on the copper wire (14).
10. The preparation method according to claim 8 or 9, characterized in that: The electrochemical lithium plating structure, and / or the reference electrode tab (10), and / or the first positive electrode tab (6), and / or the negative electrode tab (7), and / or the second positive electrode tab (8) are all fixed by tab glue (9) or tape (13).
Citation Information
Patent Citations
Three-electrode lithium ion battery and preparation method thereof
CN113036251A
Reference electrode of lithium ion battery, three-electrode battery and preparation method of three-electrode battery
CN114335920A
Three-electrode cell structure, three-electrode battery and cathode potential monitoring method
CN116207357A
Three-electrode structure of lithium ion battery
CN203039037U
Three-electrode lithium ion battery for testing
CN214043743U