Manganese iron phosphate precursor with core-shell structure as well as preparation method and application of manganese iron phosphate precursor

Through the preparation method of core-shell structure iron manganese phosphate precursor, the problems of low electronic conductivity and lithium ion diffusion rate of lithium iron manganese phosphate cathode material are solved, and good electrochemical performance and cycle stability are achieved.

CN118754074APending Publication Date: 2024-10-11HUNAN YUNENG NEW ENERGY BATTERY MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411108884.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Lithium iron manganese phosphate cathode material exhibits poor electrochemical performance due to its crystal structure resulting in low electronic conductivity and lithium ion diffusion rate.

Method used

The preparation method of iron manganese phosphate precursor with core-shell structure is adopted. By controlling the growth and particle size of the precursor, the contact area between the material and the electrolyte is increased, and the lithium ion diffusion rate is enhanced. The method includes dissolving soluble manganese salts, iron salts and phosphates in water, adjusting the pH value to form a structure in which manganese phosphate is the core and iron phosphate is the shell, and is mixed and calcined with a phosphorus source, a lithium source and a carbon source to prepare a positive electrode material.

Benefits of technology

It significantly improves the lithium ion diffusion rate and cycle stability, reduces the dissolution of manganese elements, alleviates material structural distortion, and improves the stability and electrochemical performance of the charge and discharge platform.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754074A_ABST
    Figure CN118754074A_ABST
Patent Text Reader

Abstract

The invention provides an iron manganese phosphate precursor with a core-shell structure and a preparation method and application thereof, and the preparation method comprises the following steps: respectively dissolving a soluble manganese salt, a soluble iron salt and a soluble phosphate in water to obtain a soluble manganese salt solution, a soluble iron salt solution and a soluble phosphate solution; taking a soluble phosphate solution as a base solution, and reacting to obtain a first solution containing manganese phosphate as a core; soluble ferric salt and alkali liquor are added into the obtained first solution, a second solution is formed through reaction, aging, washing and drying are carried out, the iron manganese phosphate precursor of the core-shell structure is obtained, the preparation method of the iron manganese phosphate precursor of the core-shell structure is simple, non-toxic, free of pollution and beneficial to large-scale industrial production, and by controlling growth of the precursor, the core-shell structure can be prepared into the iron manganese phosphate precursor of the core-shell structure. And the particle size is reduced to increase the contact area between the material and an electrolyte so as to improve the diffusion rate of lithium ions, so that the material has good electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of new energy technology, and in particular to a core-shell structured manganese iron phosphate precursor and a preparation method and application thereof. Background Art

[0002] With the rapid development of science and technology and the pursuit of environmental protection and efficient energy, new energy storage technology has become a hot topic in the field of scientific research. Among them, the new cathode material between lithium manganese phosphate and lithium iron phosphate - lithium iron manganese phosphate cathode material has gradually attracted people's attention due to its unique performance and potential.

[0003] Compared with lithium iron phosphate, the introduction of manganese can increase the charge and discharge potential of the positive electrode material to 4.1V, thereby greatly improving the energy density of the positive electrode material. Compared with lithium manganese phosphate, the introduction of iron can significantly reduce the 3+ around However, due to the crystal structure of lithium iron manganese phosphate, it has low electronic conductivity and lithium ion diffusion rate. These huge disadvantages make the material exhibit poor electrochemical performance. Summary of the invention

[0004] The technical problem to be solved by the present application is to overcome the deficiencies and defects mentioned in the above background technology, provide a core-shell structured manganese iron phosphate precursor and its preparation method and a lithium manganese iron phosphate positive electrode material prepared using the core-shell structured manganese iron phosphate precursor, control the growth of the precursor, reduce the particle size to increase the contact area between the material and the electrolyte to increase the lithium ion diffusion rate, so that the material has good electrochemical properties.

[0005] In order to solve the above technical problems, the technical solution proposed in this application is:

[0006] In a first aspect, the present application provides a method for preparing a core-shell structured manganese iron phosphate precursor, comprising the following steps:

[0007] (1) dissolving a soluble manganese salt, a soluble iron salt and a soluble phosphate in water to obtain a soluble manganese salt solution, a soluble iron salt solution and a soluble phosphate solution respectively;

[0008] (2) using the soluble phosphate solution obtained in step (1) as a base solution, heating and stirring, adding an alkali solution and the soluble manganese salt solution obtained in step (1), and obtaining a first solution after reaction, wherein the alkali solution is used to adjust the pH value of the first solution to maintain a preset pH value;

[0009] (3) adding the alkali solution and the soluble iron salt solution obtained in step (1) to the first solution to react and form a second solution, wherein the alkali solution is also used to adjust the pH value of the second solution to maintain it at the preset pH value;

[0010] (4) Aging, washing, and drying the second solution obtained in step (3) to obtain a core-shell structured manganese iron phosphate precursor.

[0011] In one embodiment, the soluble manganese salt in step (1) is one or more of manganese sulfate, manganese acetate, manganese nitrate, manganese chloride or manganese citrate; the soluble iron salt is one or more of ferrous sulfate, ferric chloride, ferrous chloride or ferrous citrate; the soluble phosphate is one or more of phosphoric acid, diammonium hydrogen phosphate or diammonium phosphate.

[0012] In one embodiment, in step (1), the molar ratio of the soluble manganese salt to the soluble iron salt is x:(1-x), wherein 0.3≤x≤0.7, and the molar ratio of the soluble phosphate is 5% to 40% in excess of the total amount of the soluble manganese salt and the soluble iron salt.

[0013] In one embodiment, in step (2), the temperature of the heating and stirring is 40° C. to 80° C., and the stirring speed is 300 rpm to 600 rpm.

[0014] In one embodiment, the alkaline solution in step (2) and step (3) is one or more of ammonia water and sodium hydroxide solution, and the preset pH value is 3 to 7.

[0015] In one embodiment, the aging time in step (4) is 3 h to 12 h; the solvent used for washing is one or more of distilled water, anhydrous ethanol or acetone; the drying temperature is 60° C. to 120° C.; and the drying time is 2 h to 8 h.

[0016] In the second aspect, the present application also provides a core-shell manganese ferrophosphate precursor obtained by the preparation method of the core-shell manganese ferrophosphate precursor as described in the first aspect, wherein the precursor particles of the manganese ferrophosphate precursor have manganese phosphate as the core and iron phosphate as the shell.

[0017] In the third aspect, the present application also provides an application of a core-shell structured manganese iron phosphate precursor obtained by the preparation method described in the first aspect or a core-shell structured manganese iron phosphate precursor as described in the second aspect, for preparing a lithium iron phosphate manganese positive electrode of a lithium ion battery, comprising the following steps: mixing the core-shell structured manganese iron phosphate precursor with a phosphorus source, a lithium source, and a carbon source, and calcining to obtain a lithium iron manganese phosphate positive electrode material; preparing a lithium iron manganese phosphate positive electrode of a lithium ion battery based on the lithium iron manganese phosphate positive electrode material.

[0018] In one embodiment, the phosphorus source is one or more of phosphoric acid, diammonium hydrogen phosphate or ammonium dihydrogen phosphate; the lithium source is one or more of lithium carbonate, lithium hydroxide or lithium acetate, and the carbon source is one or more of glucose, sucrose or citric acid; the calcination parameters are: temperature 300°C to 900°C, calcination time 3h to 12h, and calcination atmosphere is a mixed atmosphere of any one of nitrogen, argon, helium and hydrogen.

[0019] In a fourth aspect, the present application further provides a lithium-ion battery, comprising a lithium iron manganese phosphate positive electrode prepared by the application as described in the third aspect.

[0020] Compared with the prior art, the beneficial effects of this application are:

[0021] 1. The present application provides a method for preparing a core-shell structured manganese iron phosphate precursor that is simple, non-toxic and pollution-free, and is conducive to large-scale industrial production. The growth of the precursor is controlled by aging time, thereby reducing the particle size to increase the contact area between the material and the electrolyte to increase the lithium ion diffusion rate, thereby making the material have good electrochemical properties.

[0022] 2. The positive electrode material prepared in this application using the core-shell structure of manganese phosphate as the core and iron phosphate as the shell as the raw material has good electrochemical properties, increased lithium ion diffusion rate, basically no attenuation of the charge and discharge platform, and high cycle stability.

[0023] 3. The existing lithium iron manganese phosphate cathode material has the problem of manganese dissolution, which will cause the material structure to be distorted and affect the material's cycle stability. The manganese element is designed to be in the core and wrapped by the iron element, which reduces the reaction between manganese and the electrolyte, inhibits the dissolution of manganese, alleviates the Ginger effect of manganese, and improves the stability of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0025] Figure 1 A schematic flow chart of a method for preparing a core-shell structured manganese iron phosphate precursor provided in the present application.

[0026] Figure 2 This is the XRD diagram of the lithium iron manganese phosphate positive electrode material prepared in Example 1.

[0027] Figure 3This is a SEM image of the lithium iron manganese phosphate positive electrode material prepared in Example 1.

[0028] Figure 4 This is a charge and discharge curve diagram of the lithium iron manganese phosphate positive electrode material prepared in Example 1. DETAILED DESCRIPTION

[0029] To facilitate the understanding of the present application, the present application will be described in more comprehensive and detailed manner below in conjunction with the accompanying drawings and preferred embodiments of the specification, but the protection scope of the present application is not limited to the following specific embodiments.

[0030] Unless otherwise defined, all professional terms used below have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of this application.

[0031] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0032] The first aspect of the present application provides a method for preparing a core-shell structured manganese iron phosphate precursor, comprising the following steps:

[0033] (1) dissolving a soluble manganese salt, a soluble iron salt and a soluble phosphate in water to obtain a soluble manganese salt solution, a soluble iron salt solution and a soluble phosphate solution respectively;

[0034] (2) using the soluble phosphate solution obtained in step (1) as a base solution, heating and stirring, adding an alkali solution and the soluble manganese salt solution obtained in step (1), and obtaining a first solution after reaction, wherein the alkali solution is used to adjust the pH value of the first solution to maintain a preset pH value;

[0035] (3) adding alkaline solution and the soluble iron salt solution obtained in step (1) to the first solution to react and form a second solution, wherein the alkaline solution is also used to adjust the pH value of the second solution to maintain it at the preset pH value;

[0036] (4) Aging, washing, and drying the second solution obtained in step (3) to obtain a core-shell structured manganese iron phosphate precursor.

[0037] Compared with the prior art, the beneficial effects of this application are:

[0038] 1. The present application provides a method for preparing a core-shell structured manganese iron phosphate precursor, which is simple, non-toxic and pollution-free, and is conducive to large-scale industrial production. By controlling the growth of the precursor and reducing the particle size, the contact area between the material and the electrolyte is increased, thereby increasing the diffusion rate of lithium ions and improving the electrochemical performance of the manganese iron phosphate precursor.

[0039] 2. The positive electrode material prepared by the core-shell structure of manganese phosphate as the core and iron phosphate as the shell using the iron phosphate manganese precursor as the raw material has good electrochemical properties, increases the diffusion rate of lithium ions, makes the charge and discharge platform attenuation of the lithium ion battery very small, and improves the stability of the charge and discharge cycle.

[0040] In one embodiment, the soluble manganese salt in step (1) is one or more of manganese sulfate, manganese acetate, manganese nitrate, manganese chloride and manganese citrate; the soluble iron salt is one or more of ferrous sulfate, ferric chloride, ferrous chloride and ferrous citrate; and the soluble phosphate is one or more of phosphoric acid, diammonium hydrogen phosphate and diammonium phosphate.

[0041] In one embodiment, the concentration of the soluble phosphate solution is 0.025 g / mL to 0.028 g / mL; the concentration of the soluble manganese salt solution is 0.039 g / mL to 0.059 g / mL; the concentration of the soluble iron salt solution is 0.043 g / mL to 0.064 g / mL; within the concentration range of this embodiment, the generation rate of the core-shell manganese phosphate iron precursor with manganese phosphate as the core and iron phosphate as the shell can be increased.

[0042] In one embodiment, in step (1), the molar ratio of the soluble manganese salt to the soluble iron salt is x:(1-x), wherein 0.3≤x≤0.7, and the molar ratio of the soluble phosphate is 5% to 40% in excess of the total amount of the soluble manganese salt and the soluble iron salt; since a core-shell structure precursor needs to be formed, the molar ratio of the soluble manganese salt to the soluble iron salt needs to be controlled within the scope of this embodiment; a molar ratio greater than or less than that of this embodiment will reduce the performance of the core-shell structured iron manganese phosphate precursor; since the phosphate reacts with the manganese salt and the iron salt at the same time, the amount of the phosphate is greater than the total amount of the manganese salt and the iron salt.

[0043] In one embodiment, in step (2), the temperature for heating and stirring is 40°C to 80°C, and the stirring speed is 300rpm to 600rpm; the appropriate temperature range and stirring speed can accelerate the reaction, shorten the time for preparing the core-shell structured manganese iron phosphate precursor, and reduce the production cost.

[0044] In one embodiment, the alkali solution in step (2) and step (3) is one or more of ammonia water and sodium hydroxide solution, and the preset pH value is 3 to 7; the solution acidity of the entire preparation process is controlled to improve the reaction efficiency of phosphate with manganese salt and iron salt.

[0045] In one embodiment, the aging time in step (4) is 3 h to 12 h; the solvent used for washing is one or more of distilled water, anhydrous ethanol or acetone; the drying temperature is 60° C. to 120° C.; the drying time is 2 h to 8 h; the process parameters of this embodiment can effectively control the quality stability of the core-shell structured manganese iron phosphate precursor, thereby improving the stability of the lithium-ion battery.

[0046] The second aspect of the present application also provides a core-shell manganese ferrophosphate precursor obtained by the preparation method of the core-shell manganese ferrophosphate precursor as described in the first aspect, wherein the precursor particles of the manganese ferrophosphate precursor have manganese phosphate as the core and iron phosphate as the shell.

[0047] The third aspect of the present application also provides an application of a core-shell structured manganese iron phosphate precursor obtained by the preparation method described in the first aspect or a core-shell structured manganese iron phosphate precursor as described in the second aspect, for preparing a lithium iron manganese phosphate positive electrode for a lithium ion battery, comprising the following steps: mixing the core-shell structured manganese iron phosphate precursor with a phosphorus source, a lithium source, and a carbon source, and calcining to obtain a lithium ion lithium iron manganese phosphate positive electrode material; preparing a lithium iron manganese phosphate positive electrode for a lithium ion battery based on the lithium iron manganese phosphate positive electrode material.

[0048] In one embodiment, the phosphorus source is one or more of phosphoric acid, diammonium hydrogen phosphate or ammonium dihydrogen phosphate, the lithium source is one or more of lithium carbonate, lithium hydroxide or lithium acetate, and the carbon source is one or more of glucose, sucrose or citric acid; the calcination parameters are: temperature 300°C to 900°C, calcination time 3h to 12h, and calcination atmosphere is a mixed atmosphere of any one of nitrogen, argon, helium and hydrogen; multiple choices of phosphorus source, lithium source and carbon source are conducive to expanding the source and reducing production costs; controlling the calcination parameters improves the quality stability of the lithium iron manganese phosphate positive electrode.

[0049] The fourth aspect of the present application also provides a lithium-ion battery, including a lithium iron manganese phosphate positive electrode prepared by the application as described in the third aspect; the lithium-ion battery prepared using the lithium iron manganese phosphate positive electrode can increase the diffusion rate of lithium ions, improve the stability of the charge and discharge cycle, and improve the performance of the lithium-ion battery.

[0050] In order to make the above implementation details and operations of the present application clearly understood by those skilled in the art, and to significantly demonstrate the good electrochemical performance of the lithium iron manganese phosphate positive electrode material for lithium-ion batteries prepared from the iron manganese phosphate precursor of the present application, the above technical scheme is illustrated by means of multiple embodiments below.

[0051] Embodiment 1:

[0052] A method for preparing a core-shell structured manganese iron phosphate precursor comprises the following steps:

[0053] (1) Weigh 1.3866 g of diammonium hydrogen phosphate and dissolve it in 50 mL of distilled water to prepare a soluble phosphate solution, weigh 1.4706 g of manganese acetate tetrahydrate and dissolve it in 30 mL of distilled water to prepare a soluble manganese salt solution, and weigh 1.6218 g of ferric chloride hexahydrate and dissolve it in 30 mL of distilled water to prepare a soluble iron salt solution;

[0054] (2) using a soluble phosphate solution as a base liquid, heating it to 60° C., adding a soluble manganese salt solution and an ammonia solution to the base liquid, stirring evenly, and allowing the manganese phosphate core particles to grow, thereby obtaining a first solution;

[0055] (3) adding a soluble iron salt solution and an ammonia solution to the first solution and stirring the mixture evenly to allow the shell iron phosphate particles to grow to form a second solution;

[0056] (4) The second solution was aged for 3 hours, washed with distilled water for 6 times, and dried in an oven at 80° C. for 5 hours to obtain a core-shell structured iron-manganese phosphate precursor with manganese phosphate as the core and iron phosphate as the shell of the present application.

[0057] The reaction pH was controlled at 5 throughout the process, and the stirring speed was 600 rpm.

[0058] An application of a core-shell structured manganese iron phosphate precursor for preparing a lithium manganese iron phosphate positive electrode for a lithium ion battery comprises the following steps:

[0059] Weigh 0.4610g lithium carbonate and 0.6002g glucose in a 100mL zirconia ball mill, add 10mL anhydrous ethanol and mix for 30min, then add 1.7224g iron manganese phosphate precursor and 0.2852g ammonium dihydrogen phosphate and mix for 1h, take out and dry in an oven at 80°C for 2h, heat to 350°C at a rate of 5°C / min, calcine under argon / hydrogen (95 / 5) gas protection for 3 hours, then heat to 650°C at a rate of 5°C / min, calcine under argon / hydrogen (95 / 5) gas protection for 5 hours, and then heat to 650°C at a rate of 5°C / min, calcine under argon / hydrogen (95 / 5) gas protection for 5 hours. The obtained powder is the lithium iron manganese phosphate positive electrode material of the lithium ion battery, and then the lithium iron manganese phosphate positive electrode of the lithium ion battery is prepared based on the lithium iron manganese phosphate positive electrode material.

[0060] Among them, the XRD of lithium iron manganese phosphate positive electrode material is as follows Figure 1 As shown in the figure, the diffraction peaks of the lithium iron manganese phosphate positive electrode material at all angles match the standard card, and the diffraction peaks are sharp, indicating that the material is well crystallized and is a pure phase. Figure 2 As shown in Figure 1, it shows that the particle size of the lithium iron manganese phosphate positive electrode material is at the nanometer level. Due to the small particle size, the contact area between the lithium iron manganese phosphate positive electrode material and the electrolyte is increased, thereby increasing the diffusion rate of lithium ions and improving the electrochemical performance of the iron manganese phosphate precursor. The charge and discharge curves at a current of 0.1C are shown in Figure 1. Figure 3 As shown, its discharge capacity reaches This is close to the theoretical value, indicating that the lithium manganese iron phosphate positive electrode material of this embodiment has good electrochemical performance.

[0061] Embodiment 2:

[0062] A method for preparing a core-shell structured manganese iron phosphate precursor comprises the following steps:

[0063] (1) Weigh 1.3892 g of diammonium hydrogen phosphate and dissolve it in 50 mL of distilled water to prepare a soluble phosphate solution; weigh 1.1764 g of manganese acetate tetrahydrate and dissolve it in 30 mL of distilled water to prepare a soluble manganese salt solution; weigh 1.9462 g of ferric chloride hexahydrate and dissolve it in 30 mL of distilled water to prepare a soluble iron salt solution;

[0064] (2) using a soluble phosphate solution as a base liquid, heating it to 80° C., adding a soluble manganese salt solution and an ammonia solution to the base liquid for reaction, stirring evenly, and allowing the manganese phosphate core particles to grow, thereby obtaining a first solution;

[0065] (3) adding a soluble iron salt solution and an ammonia solution to the first solution and stirring the solution uniformly to allow the shell iron phosphate particles to grow to form a second solution;

[0066] (4) The second solution was aged for 5 hours, washed with distilled water for 6 times, and dried in an oven at 80° C. for 5 hours to obtain the core-shell structured iron-manganese phosphate precursor with manganese phosphate as the core and iron phosphate as the shell of the present application. The reaction pH was controlled to be 4.5 throughout the process, and the stirring speed was 600 rpm.

[0067] An application of a core-shell structured manganese iron phosphate precursor for preparing a lithium manganese iron phosphate positive electrode for a lithium ion battery comprises the following steps:

[0068] Weigh 0.4610g lithium carbonate and 0.6002g sucrose in a 100mL zirconia ball mill, add 10mL anhydrous ethanol and mix for 30min, then add 1.7224g iron manganese phosphate precursor and 0.2852g ammonium dihydrogen phosphate and mix for 1h, take out and dry in an 80°C oven for 2h, heat to 350°C at a rate of 3°C / min, calcine for 3 hours under argon / hydrogen (95 / 5) gas protection, then heat to 700°C at a rate of 3°C / min, calcine for 3 hours under argon / hydrogen (95 / 5) gas protection, and then heat to 700°C at a rate of 3°C / min, calcine for 3 hours under argon / hydrogen (95 / 5) gas protection, and the obtained powder is the lithium iron manganese phosphate positive electrode material of the lithium ion battery, and then the lithium iron manganese phosphate positive electrode of the lithium ion battery is prepared based on the lithium iron manganese phosphate positive electrode material.

[0069] Embodiment 3:

[0070] A method for preparing a core-shell structured manganese iron phosphate precursor comprises the following steps:

[0071] (1) Weigh 1.2742 g of diammonium hydrogen phosphate and dissolve it in 50 mL of distilled water to prepare a soluble phosphate solution, weigh 1.7646 g of manganese acetate tetrahydrate and dissolve it in 30 mL of distilled water to prepare a soluble manganese salt solution, and weigh 1.2974 g of ferric chloride hexahydrate and dissolve it in 30 mL of distilled water to prepare a soluble iron salt solution;

[0072] (2) using a soluble phosphate solution as a base liquid, heating it to 80° C., adding a soluble manganese salt solution and an ammonia solution to the base liquid for reaction, stirring evenly, and allowing the manganese phosphate core particles to grow, thereby obtaining a first solution;

[0073] (3) then adding a soluble iron salt solution and an ammonia solution to the first solution and stirring evenly to allow the shell iron phosphate particles to grow to form a second solution;

[0074] (4) The second solution was aged for 8 hours, washed with distilled water for 6 times, and dried in an oven at 80° C. for 5 hours to obtain the core-shell structured iron-manganese phosphate precursor with manganese phosphate as the core and iron phosphate as the shell of the present application. The reaction pH was controlled to be 5.5 throughout the process, and the stirring speed was 600 rpm.

[0075] An application of a core-shell structured manganese iron phosphate precursor for preparing a lithium manganese iron phosphate positive electrode for a lithium ion battery comprises the following steps:

[0076] Weigh 0.4610g lithium carbonate and 0.6002g sucrose in a 100mL zirconia ball mill, add 10mL anhydrous ethanol and mix for 30min, then add 1.7224g iron manganese phosphate precursor and 0.2852g ammonium dihydrogen phosphate and mix for 1h, take out and dry in an oven at 80°C for 2h, heat to 650°C at a rate of 3°C / min, and calcine for 6 hours under argon / hydrogen (95 / 5) gas protection. The obtained powder is the lithium iron manganese phosphate positive electrode material of the lithium ion battery, and the lithium iron manganese phosphate positive electrode of the lithium ion battery is prepared based on the lithium iron manganese phosphate positive electrode material.

[0077] Comparative Example 1:

[0078] A method for preparing a manganese iron phosphate precursor comprises the following steps:

[0079] Weigh 1.3866g of diammonium hydrogen phosphate and dissolve it in 50mL of distilled water to obtain a soluble phosphate solution, weigh 1.4706g of tetrahydrate manganese acetate and dissolve it in 30mL of distilled water to obtain a soluble manganese salt solution, weigh 1.6218g of ferric chloride hexahydrate and dissolve it in 30mL of distilled water to obtain a soluble iron salt solution, use the soluble phosphate solution as the base liquid, heat it to 60°C, react, add the soluble manganese salt solution, the soluble iron salt solution and the ammonia solution to the base liquid together, so that the salt solution drips at the same time, stir evenly, age for 3h, wash with distilled water 6 times, and dry in an oven at 80°C for 5h to obtain an iron manganese phosphate precursor without a special structure. The reaction pH is controlled to be 5 throughout the process, and the stirring speed is 600rpm.

[0080] A preparation of a positive electrode comprises the following steps:

[0081] Weigh 0.4610g lithium carbonate and 0.6002g glucose in a 100mL zirconia ball mill, add 10mL anhydrous ethanol and mix for 30min, then add 1.7224g iron manganese phosphate precursor and 0.2852g ammonium dihydrogen phosphate and mix for 1h, take out and dry in an oven at 80℃ for 2h, heat to 350℃ at a rate of 5℃ / min, calcine under argon / hydrogen (95 / 5) gas protection for 3 hours, then heat to 650℃ at a rate of 5℃ / min, calcine under argon / hydrogen (95 / 5) gas protection for 5 hours, and then heat to 650℃ at a rate of 5℃ / min, calcine under argon / hydrogen (95 / 5) gas protection for 5 hours. The obtained powder is the lithium iron manganese phosphate positive electrode material, and the lithium iron manganese phosphate positive electrode of the lithium ion battery is prepared based on the lithium iron manganese phosphate positive electrode material.

[0082] Comparative Example 2:

[0083] A method for preparing a manganese iron phosphate precursor comprises the following steps:

[0084] Weigh 1.3866g diammonium hydrogen phosphate and dissolve it in 50mL distilled water to obtain a soluble phosphate solution, weigh 1.4706g manganese acetate tetrahydrate and dissolve it in 30mL distilled water to obtain a soluble manganese salt solution, weigh 1.6218g ferric chloride hexahydrate and dissolve it in 30mL distilled water to obtain a soluble iron salt solution, use the soluble phosphate solution as the base liquid, heat it to 60°C, react, add the soluble manganese salt solution, the soluble iron salt solution and the ammonia solution to the base liquid together, add the soluble manganese salt solution dropwise from fast to slow, and add the soluble iron salt solution dropwise from slow to fast, so that the salt solution drips at the same time, stir evenly, age for 3h, wash with distilled water 6 times, and dry in an oven at 80°C for 5h to obtain a special structure of iron-manganese phosphate precursor with a gradient distribution of iron and manganese. The reaction pH is controlled to be 5 throughout the process, and the stirring speed is 600rpm.

[0085] A preparation of a positive electrode comprises the following steps:

[0086] Weigh 0.4610g lithium carbonate and 0.6002g glucose in a 100mL zirconia ball mill, add 10mL anhydrous ethanol and mix for 30min, then add 1.7224g iron manganese phosphate precursor and 0.2852g ammonium dihydrogen phosphate and mix for 1h, take out and dry in an oven at 80℃ for 2h, heat to 350℃ at a rate of 5℃ / min, calcine under argon / hydrogen (95 / 5) gas protection for 3 hours, then heat to 650℃ at a rate of 5℃ / min, calcine under argon / hydrogen (95 / 5) gas protection for 5 hours, and then heat to 650℃ at a rate of 5℃ / min, calcine under argon / hydrogen (95 / 5) gas protection for 5 hours. The obtained powder is the lithium iron manganese phosphate positive electrode material, and the lithium iron manganese phosphate positive electrode of the lithium ion battery is prepared based on the lithium iron manganese phosphate positive electrode material.

[0087] 1. Performance testing:

[0088] Weigh the active material positive electrode material, binder PVDF, and conductive agent SP in a mass ratio of 7:2:1, grind and disperse, mix evenly, and keep the slurry with good fluidity. Apply the slurry on a flat aluminum foil and dry it. Put the dried electrode into a vacuum drying oven at 80°C and let it stand. Finally, use a manual cutting machine to cut it into a circular electrode with a diameter of 10 mm.

[0089] The button-type simulated battery is assembled in a glove box with a good atmosphere. The lithium battery consists of the following parts: a battery case of model C2025, a working electrode, a negative electrode metal lithium, a diaphragm, a nickel mesh of appropriate size (for support), and an electrolyte of 1M LiPF6 (EC / DMC / EMC = 1 / 1 / 1 by volume). The assembly order of the battery is: positive electrode case-positive electrode-two drops of electrolyte-diaphragm-one drop of electrolyte-metal lithium-nickel mesh-negative electrode case. After assembly, a sealing machine is used to seal the battery. The samples were sealed under pressure and then left to stand at room temperature. Battery test system, all electrochemical performance tests were carried out at room temperature. The battery performance test results are shown in Table 1.

[0090] Table 1 Performance test results of each embodiment and each comparative example

[0091] project 1C1000 cycle capacity retention rate Example 1 95.7% Example 2 94.9% Example 3 92.8% Comparative Example 1 80.3% Comparative Example 2 85.3%

[0092] As can be seen from Table 1, after 1000 cycles of testing at 1C current, the capacity retention rate of the embodiment of the present application is much higher than that of the comparative example, which reflects that the composite material prepared using the core-shell structured manganese iron phosphate precursor has good electrochemical properties, indicating that the manganese iron phosphate regulation strategy of the present application has a certain improvement effect on the electrochemical properties of the positive electrode material, and can greatly improve its cycle stability.

[0093] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A method for preparing a core-shell structured manganese iron phosphate precursor, characterized in that: The steps include: (1) dissolving a soluble manganese salt, a soluble iron salt and a soluble phosphate in water to obtain a soluble manganese salt solution, a soluble iron salt solution and a soluble phosphate solution respectively; (2) using the soluble phosphate solution obtained in step (1) as a base solution, heating and stirring, adding an alkali solution and the soluble manganese salt solution obtained in step (1), and obtaining a first solution after reaction, wherein the alkali solution is used to adjust the pH value of the first solution to maintain a preset pH value; (3) adding the alkali solution and the soluble iron salt solution obtained in step (1) to the first solution to react and form a second solution, wherein the alkali solution is also used to adjust the pH value of the second solution to maintain it at the preset pH value; (4) Aging, washing, and drying the second solution obtained in step (3) to obtain a core-shell structured manganese iron phosphate precursor.

2. The preparation method according to claim 1, characterized in that: In step (1), the soluble manganese salt is one or more of manganese sulfate, manganese acetate, manganese nitrate, manganese chloride or manganese citrate; the soluble iron salt is one or more of ferrous sulfate, ferric chloride, ferrous chloride or ferrous citrate; and the soluble phosphate is one or more of phosphoric acid, diammonium hydrogen phosphate or diammonium phosphate.

3. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of the soluble manganese salt to the soluble iron salt is x:(1-x), wherein 0.3≤x≤0.7, and the molar ratio of the soluble phosphate is 5%-40% in excess of the total amount of the soluble manganese salt and the soluble iron salt.

4. The preparation method according to claim 1, characterized in that: The temperature for heating and stirring in step (2) is 40° C. to 80° C., and the stirring speed is 300 rpm to 600 rpm.

5. The preparation method according to claim 1, characterized in that: The alkaline solution in step (2) and step (3) is one or more of ammonia water and sodium hydroxide solution, and the preset pH value is 3 to 7.

6. The preparation method according to claim 1, characterized in that: In step (4), the aging time is 3 h to 12 h; the solvent used for washing is one or more of distilled water, anhydrous ethanol or acetone; the drying temperature is 60° C. to 120° C.; and the drying time is 2 h to 8 h.

7. A core-shell structured manganese ferrophosphate precursor obtained by the method for preparing a core-shell structured manganese ferrophosphate precursor according to any one of claims 1 to 6, characterized in that: The precursor particles of the iron manganese phosphate precursor have manganese phosphate as the core and iron phosphate as the shell.

8. A use of a core-shell structured manganese ferrophosphate precursor obtained by the preparation method according to any one of claims 1 to 6 or a core-shell structured manganese ferrophosphate precursor according to claim 7, characterized in that: The method for preparing a lithium iron manganese phosphate positive electrode for a lithium ion battery comprises the following steps: The core-shell structured manganese iron phosphate precursor is mixed with a phosphorus source, a lithium source and a carbon source, and calcined to obtain a manganese iron phosphate lithium positive electrode material; and a manganese iron phosphate lithium positive electrode of a lithium ion battery is prepared based on the manganese iron phosphate lithium positive electrode material.

9. The use according to claim 8, characterized in that: The phosphorus source is one or more of phosphoric acid, diammonium hydrogen phosphate and diammonium dihydrogen phosphate; The lithium source is one or more of lithium carbonate, lithium hydroxide or lithium acetate; The carbon source is one or more of glucose, sucrose or citric acid; The calcination parameters are: temperature of 300° C. to 900° C., calcination time of 3 h to 12 h, and calcination atmosphere of a mixture of any one of nitrogen, argon, and helium and hydrogen.

10. A lithium ion battery, characterized in that: It comprises a lithium manganese iron phosphate positive electrode prepared by the application as described in claim 8 or 9.

Citation Information

Patent Citations

  • Lithium ferric manganese phosphate positive electrode material with iron and manganese elements in full-concentration gradient distribution and preparation method of lithium ferric manganese phosphate positive electrode material

    CN114725340A

  • Ferric manganese phosphate precursor, lithium iron manganese phosphate positive electrode material and preparation method and application of ferric manganese phosphate precursor and lithium iron manganese phosphate positive electrode material

    CN117440928A

  • Method for producing transition metal arsenates and / or phosphates having an olivine structure

    WO2018024979A1