Hard carbon negative electrode material, preparation method thereof and sodium ion battery

Through oxidative cross-linking of starch, cellulose, and resin and low-temperature and high-temperature carbonization, hard carbon anode materials with rich closed-pore structures are prepared, which solves the problem of low capacity of hard carbon materials in sodium-ion batteries and improves the performance of sodium-ion batteries. Energy density and electrochemical performance.

CN118754100AActive Publication Date: 2024-10-11四川佰思格新材料科技有限公司

Patent Information

Application Number
CN202410991271.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-11
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing hard carbon materials have low capacity when used in sodium-ion batteries, which limits their application in sodium-ion batteries.

Method used

Starch, cellulose, and resin are used as raw materials, oxidative cross-linking treatment is performed with oxidizing acids, and low- and high-temperature carbonization is performed in an inert atmosphere to prepare hard carbon anode materials with rich closed-pore structures.

Benefits of technology

It improves the energy density and electrochemical performance of sodium-ion batteries, and improves the kinetics and low-temperature performance of the full battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754100A_ABST
    Figure CN118754100A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of battery materials, in particular to a hard carbon negative electrode material, a preparation method thereof and a sodium ion battery, and the preparation method comprises the following steps: mixing starch, cellulose and resin to obtain a mixed raw material; adding oxidizing acid into the mixed raw material, and carrying out oxidation crosslinking treatment at 50-200 DEG C to obtain an oxidation-crosslinking material; washing the oxidized-crosslinked material to obtain a washed material; granulating the washed material to obtain a spherical precursor; performing low-temperature carbonization on the spherical precursor in an inert atmosphere to obtain a precursor subjected to low-temperature pretreatment; and carbonizing the precursor subjected to low-temperature pretreatment at 1200-1600 DEG C in an inert atmosphere to obtain the hard carbon negative electrode material. The starch, the cellulose and the resin are used as mixed raw materials, and the pre-treatment processes of oxidation cross-linking and low-temperature carbonization are combined, so that the prepared hard carbon negative electrode material is rich in closed pore structure and mostly located on the surface, and the capacity can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a hard carbon negative electrode material and a preparation method thereof, and a sodium ion battery. Background Art

[0002] Because sodium-ion batteries rely on low-cost and abundant sodium resources, they have become recognized as the most competitive alternative to lithium-ion batteries in recent years.

[0003] The development of sodium-ion batteries depends largely on the performance of electrode materials, among which the negative electrode material is the key factor affecting the performance of sodium-ion batteries. The graphite negative electrode material commonly used in lithium-ion batteries has a very low sodium storage capacity and is not suitable for sodium-ion batteries. Hard carbon materials have become sodium-ion battery negative electrode materials with commercial prospects due to their advantages such as structural stability and a lower sodium insertion voltage platform. However, when existing hard carbon materials are used in sodium-ion batteries, they still face the problem of low capacity, which limits their application in sodium-ion batteries. Summary of the invention

[0004] In order to solve the problem of low capacity of hard carbon materials in the prior art when used in sodium ion batteries, the present invention provides a method for preparing a hard carbon negative electrode material. The preparation method uses starch, cellulose, and resin as raw materials, and performs oxidative cross-linking treatment with an oxidizing acid and then carbonizes the material, so that the prepared hard carbon negative electrode material has a rich closed-pore structure, which helps to improve the capacity, thereby solving the problem of low capacity of hard carbon materials in the prior art when used in sodium ion batteries.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] A method for preparing a hard carbon negative electrode material comprises the following steps:

[0007] S1: Mixing starch, cellulose and resin to obtain a mixed raw material;

[0008] S2: adding an oxidizing acid to the mixed raw material, and performing an oxidative crosslinking treatment at 50-200° C. to obtain an oxidized-crosslinked material;

[0009] S3: washing the oxidation-crosslinked material to obtain a washed material;

[0010] S4: granulating the washed material to obtain a spherical precursor;

[0011] S5: performing low-temperature carbonization on the spherical precursor under an inert atmosphere to obtain a low-temperature pretreated precursor;

[0012] S6: In an inert atmosphere, carbonizing the low-temperature pretreated precursor at 1200-1600° C. to obtain a hard carbon negative electrode material.

[0013] Optionally, the resin is selected from at least one of epoxy resin, phenolic resin, polycarbonate, polyurethane, polyvinyl chloride, ABS, furan resin, furfural resin, bismaleimide resin, and polyimide resin.

[0014] Optionally, in step S1, the mass ratio of the starch, the cellulose and the resin is (1-5): (2-6): (3-6).

[0015] Optionally, the oxidizing acid is selected from at least one of sulfuric acid, nitric acid, permanganic acid, perchloric acid, chloric acid, and hypochlorous acid.

[0016] Optionally, in step S2, the mass ratio of the mixed raw material to the oxidizing acid is (1-10):1.

[0017] Optionally, the particle size D50 of the spherical precursor in step S4 is 5-10 μm.

[0018] Optionally, step S5 includes: under an inert atmosphere, heating the spherical precursor to 200° C. for 1 hour, heating to 400° C. for 2 hours, and heating to 550-600° C. for 2 hours to obtain a low-temperature pretreated precursor.

[0019] Optionally, in step S6, the temperature is increased to 1200-1600° C. at a heating rate of 0.5-5° C. / min.

[0020] Another object of the present invention is to provide a hard carbon negative electrode material, which is prepared by the preparation method of the hard carbon negative electrode material as described above.

[0021] Another object of the present invention is to provide a sodium ion battery comprising the hard carbon negative electrode material as described above.

[0022] The beneficial effects of the present invention are:

[0023] The preparation method of the hard carbon negative electrode material provided by the present invention uses starch, cellulose and resin as mixed raw materials, and combines the pretreatment process of oxidative cross-linking and low-temperature carbonization, as well as a spherical precursor structure, so that the prepared hard carbon negative electrode material has a rich closed-pore structure, and most of it is located on the surface, which effectively improves the energy density and electrochemical performance of the sodium ion battery, and is beneficial to improving the full battery dynamics and low-temperature performance while increasing the capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0025] Figure 1It is a rate discharge performance diagram of the hard carbon negative electrode materials prepared in various embodiments and comparative examples of the present invention. DETAILED DESCRIPTION

[0026] The present invention is now further described in detail. The embodiments described below are exemplary and intended to be used to explain the present invention, but cannot be understood as limiting the present invention. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0027] In order to solve the problem of low capacity of hard carbon materials when used in sodium ion batteries in the prior art, the present invention provides a method for preparing a hard carbon negative electrode material, which comprises the following steps:

[0028] S1: Mixing starch, cellulose and resin to obtain a mixed raw material;

[0029] S2: adding an oxidizing acid to the mixed raw material, and performing an oxidative crosslinking treatment at 50-200° C. to obtain an oxidized-crosslinked material;

[0030] By using a mixture of starch, cellulose and resin as a mixed raw material, a rich pore structure is generated during the carbonization of starch, which is conducive to the storage of sodium ions; cellulose is a linear polymer of repeating units (glucose), which has the function of improving structural stability and first effect; the resin has a softening effect, and when mixed with starch and cellulose, it can improve the toughness of hard carbon and prevent the hard carbon particles from breaking during high-rate discharge; through the oxidation cross-linking treatment process, the surface of the material has a richer micropore and ultramicropore structure, and after high-temperature carbonization, such micropores and ultramicropores shrink and close to form a closed-pore structure, providing a place for the diffusion, storage and deintercalation of sodium ions;

[0031] S3: washing the oxidized-crosslinked material to obtain a washed material; preferably neutralizing it with at least one of sodium carbonate, sodium bicarbonate, sodium citrate, calcium carbonate, ammonium bicarbonate, sodium hydroxide, and potassium hydroxide, and then washing it with water multiple times until it is neutral to remove residual impurity ions in the material to obtain a washed material;

[0032] S4: Granulate the washed material to obtain a spherical precursor; preferably, the washed material is granulated into a spherical precursor with a D50 of 5-10 μm by spray granulation, solvent volatilization, solvent replacement, or chemical cross-linking-polymerization; the spherical structure is beneficial to reducing the micropore exposure rate, promoting the cross-linking of the mesoporous structure to transform into closed pores, and is beneficial to improving the compaction density of the pole piece in the preparation of the full battery pole piece, thereby improving the energy density and dynamic performance of the full battery;

[0033] S5: The spherical precursor is subjected to low-temperature carbonization under an inert atmosphere to obtain a low-temperature pretreated precursor; the volatiles in the material are fully volatilized through the low-temperature carbonization process, and the ultra-micropores and channels created by the volatiles provide more abundant paths for subsequent ion transfer, which can improve the kinetics of the hard carbon product;

[0034] S6: In an inert atmosphere, carbonize the low-temperature pretreated precursor at 1200-1600° C. to obtain a hard carbon negative electrode material; preferably, in this step, the temperature is increased to 1200-1600° C. at a heating rate of 0.5-5° C. / min, and the carbonization time is 1-5 h.

[0035] The preparation method of the hard carbon negative electrode material provided by the present invention uses starch, cellulose and resin as mixed raw materials, and combines the pretreatment process of oxidative cross-linking and low-temperature carbonization, as well as a spherical precursor structure, so that the prepared hard carbon negative electrode material has a rich closed-pore structure, and most of it is located on the surface, which effectively improves the energy density and electrochemical performance of the sodium ion battery, is beneficial to improve the capacity while improving the dynamics and low-temperature performance of the whole battery, and is suitable for low-temperature usage scenarios.

[0036] In order to ensure the electrochemical properties of the hard carbon negative electrode material, the resin of the present invention is preferably selected from at least one of epoxy resin, phenolic resin, polycarbonate, polyurethane, polyvinyl chloride, ABS, furan resin, furfural resin, bismaleimide resin, and polyimide resin; based on the excellent wear resistance, tensile resistance and flexibility of polyurethane resin, the resin of the present invention is further preferably polyurethane resin, so as to maintain the integrity of the particles during the rolling process of the battery pole piece; the starch is preferably selected from at least one of potato starch, corn starch, wheat starch, bean starch, cornstarch, kudzu starch, lotus root starch, water chestnut starch, cross-linked starch, and esterified starch; the cellulose is preferably selected from at least one of natural cellulose and artificial cellulose, and the cellulose is further preferably flax cellulose.

[0037] Furthermore, in the preferred embodiment of the present invention, the mass ratio of starch, cellulose and resin in step S1 is (1-5): (2-6): (3-6).

[0038] To ensure the smooth progress of the oxidative crosslinking process, the present invention preferably uses an oxidizing acid selected from at least one of sulfuric acid, nitric acid, permanganic acid, perchloric acid, chloric acid, and hypochlorous acid; and further preferably, the mass ratio of the mixed raw material to the oxidizing acid in step S2 is (1-10):1, and further preferably is 3:1.

[0039] To ensure the kinetics of the hard carbon negative electrode material, the preferred step S5 of the present invention includes: in an inert atmosphere, heating the spherical precursor to 200°C for 1 hour, heating to 400°C for 2 hours, and heating to 550-600°C for 2 hours to obtain a low-temperature pretreated precursor.

[0040] Another object of the present invention is to provide a hard carbon negative electrode material, which is prepared by the method for preparing the hard carbon negative electrode material as described above.

[0041] The hard carbon negative electrode material provided by the present invention has a rich closed-pore structure, and the closed-pore structure is mostly located on the surface, which effectively improves the energy density and electrochemical performance of the sodium ion battery, and is beneficial to improving the full battery dynamics and low-temperature performance while increasing the capacity.

[0042] Another object of the present invention is to provide a sodium ion battery, which comprises the hard carbon negative electrode material as described above.

[0043] The sodium ion battery provided by the present invention adopts a hard carbon negative electrode material with rich closed-pore structure, and the closed-pore structure is mostly located on the surface, which effectively improves the energy density and electrochemical performance of the sodium ion battery, and is beneficial to improving the full battery dynamics and low-temperature performance while increasing the capacity.

[0044] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below.

[0045] Example 1

[0046] This embodiment provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0047] S1: mixing wheat starch, flax cellulose and polyurethane resin in a mass ratio of 1:6:3 to obtain a mixed raw material;

[0048] S2: adding oxidizing acid sulfuric acid (mass fraction of 15%) to the mixed raw material, the mass ratio of the mixed raw material to sulfuric acid is 3:1, mixing evenly, heating to 120° C., keeping the temperature for 6 hours, and performing oxidation cross-linking treatment to obtain an oxidation-cross-linked material;

[0049] S3: washing the oxidized-crosslinked material with a sodium carbonate aqueous solution and water in sequence until it becomes neutral, removing residual impurity ions in the material, and obtaining a washed material;

[0050] S4: granulating the washed material by spray granulation to obtain a spherical precursor with a D50 of 7 μm;

[0051] S5: In a nitrogen atmosphere, the spherical precursor is heated to 200° C. and kept for 1 h, then to 400° C. and kept for 2 h, and then to 550° C. and kept for 2 h, to obtain a low-temperature pretreated precursor;

[0052] S6: In a nitrogen atmosphere, the temperature is raised to 1400°C at a heating rate of 3°C / min to carbonize the low-temperature pretreated precursor for 3 hours to obtain a hard carbon negative electrode material.

[0053] Example 2

[0054] This embodiment provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0055] S1: mixing wheat starch, flax cellulose and polyurethane resin in a mass ratio of 5:2:3 to obtain a mixed raw material;

[0056] S2: adding oxidizing acid sulfuric acid (mass fraction of 15%) to the mixed raw material, the mass ratio of the mixed raw material to sulfuric acid is 3:1, mixing evenly, heating to 50° C., keeping the temperature for 6 hours, and performing oxidation cross-linking treatment to obtain an oxidation-cross-linked material;

[0057] S3: washing the oxidized-crosslinked material with a sodium carbonate aqueous solution and water in sequence until it becomes neutral, removing residual impurity ions in the material, and obtaining a washed material;

[0058] S4: granulating the washed material by spray granulation to obtain a spherical precursor with a D50 of 7 μm;

[0059] S5: In a nitrogen atmosphere, the spherical precursor is heated to 200° C. and kept for 1 h, then to 400° C. and kept for 2 h, and then to 600° C. and kept for 2 h, to obtain a low-temperature pretreated precursor;

[0060] S6: In a nitrogen atmosphere, the temperature is raised to 1200°C at a heating rate of 0.5°C / min to carbonize the low-temperature pretreated precursor for 5 hours to obtain a hard carbon negative electrode material.

[0061] Example 3

[0062] This embodiment provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0063] S1: mixing wheat starch, flax cellulose and polyurethane resin in a mass ratio of 1:3:6 to obtain a mixed raw material;

[0064] S2: adding oxidizing acid sulfuric acid (mass fraction of 15%) to the mixed raw material, the mass ratio of the mixed raw material to sulfuric acid is 3:1, mixing evenly, heating to 200° C., keeping the temperature for 6 hours, performing oxidation cross-linking treatment, and obtaining an oxidation-cross-linked material;

[0065] S3: washing the oxidized-crosslinked material with a sodium carbonate aqueous solution and water in sequence until it becomes neutral, removing residual impurity ions in the material, and obtaining a washed material;

[0066] S4: granulating the washed material by spray granulation to obtain a spherical precursor with a D50 of 7 μm;

[0067] S5: In a nitrogen atmosphere, the spherical precursor is heated to 200° C. and kept for 1 h, then to 400° C. and kept for 2 h, and then to 600° C. and kept for 2 h, to obtain a low-temperature pretreated precursor;

[0068] S6: In a nitrogen atmosphere, the temperature is raised to 1600°C at a heating rate of 5°C / min, and the low-temperature pretreated precursor is carbonized for 1 hour to obtain a hard carbon negative electrode material.

[0069] Comparative Example 1

[0070] This comparative example provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0071] S1: mixing wheat starch and polyurethane resin in a mass ratio of 1:3 to obtain a mixed raw material;

[0072] S2: adding oxidizing acid sulfuric acid (mass fraction of 15%) to the mixed raw material, the mass ratio of the mixed raw material to sulfuric acid is 3:1, mixing evenly, heating to 120° C., keeping the temperature for 6 hours, and performing oxidation cross-linking treatment to obtain an oxidation-cross-linked material;

[0073] S3: washing the oxidized-crosslinked material with a sodium carbonate aqueous solution and water in sequence until it becomes neutral, removing residual impurity ions in the material, and obtaining a washed material;

[0074] S4: granulating the washed material by spray granulation to obtain a spherical precursor with a D50 of 7 μm;

[0075] S5: In a nitrogen atmosphere, the spherical precursor is heated to 200° C. and kept for 1 h, then to 400° C. and kept for 2 h, and then to 550° C. and kept for 2 h, to obtain a low-temperature pretreated precursor;

[0076] S6: In a nitrogen atmosphere, the temperature is raised to 1400°C at a heating rate of 3°C / min to carbonize the low-temperature pretreated precursor for 3 hours to obtain a hard carbon negative electrode material.

[0077] Comparative Example 2

[0078] This comparative example provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0079] S1: mixing flax cellulose and polyurethane resin in a mass ratio of 2:1 to obtain a mixed raw material;

[0080] S2: adding oxidizing acid sulfuric acid (mass fraction of 15%) to the mixed raw material, the mass ratio of the mixed raw material to sulfuric acid is 3:1, mixing evenly, heating to 120° C., keeping the temperature for 6 hours, and performing oxidation cross-linking treatment to obtain an oxidation-cross-linked material;

[0081] S3: washing the oxidized-crosslinked material with a sodium carbonate aqueous solution and water in sequence until it becomes neutral, removing residual impurity ions in the material, and obtaining a washed material;

[0082] S4: granulating the washed material by spray granulation to obtain a spherical precursor with a D50 of 7 μm;

[0083] S5: In a nitrogen atmosphere, the spherical precursor is heated to 200° C. and kept for 1 h, then to 400° C. and kept for 2 h, and then to 550° C. and kept for 2 h, to obtain a low-temperature pretreated precursor;

[0084] S6: In a nitrogen atmosphere, the temperature is raised to 1400°C at a heating rate of 3°C / min to carbonize the low-temperature pretreated precursor for 3 hours to obtain a hard carbon negative electrode material.

[0085] Comparative Example 3

[0086] This comparative example provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0087] S1: mixing wheat starch and flax cellulose in a mass ratio of 1:6 to obtain a mixed raw material;

[0088] S2: adding oxidizing acid sulfuric acid (mass fraction of 15%) to the mixed raw material, the mass ratio of the mixed raw material to sulfuric acid is 3:1, mixing evenly, heating to 120° C., keeping the temperature for 6 hours, and performing oxidation cross-linking treatment to obtain an oxidation-cross-linked material;

[0089] S3: washing the oxidized-crosslinked material with a sodium carbonate aqueous solution and water in sequence until it becomes neutral, removing residual impurity ions in the material, and obtaining a washed material;

[0090] S4: granulating the washed material by spray granulation to obtain a spherical precursor with a D50 of 7 μm;

[0091] S5: In a nitrogen atmosphere, the spherical precursor is heated to 200° C. and kept for 1 h, then to 400° C. and kept for 2 h, and then to 550° C. and kept for 2 h, to obtain a low-temperature pretreated precursor;

[0092] S6: In a nitrogen atmosphere, the temperature is raised to 1400°C at a heating rate of 3°C / min to carbonize the low-temperature pretreated precursor for 3 hours to obtain a hard carbon negative electrode material.

[0093] Comparative Example 4

[0094] S1: mixing wheat starch, flax cellulose and polypropylene resin in a mass ratio of 1:6:3 to obtain a mixed raw material;

[0095] S2: adding oxidizing acid sulfuric acid (mass fraction of 15%) to the mixed raw material, the mass ratio of the mixed raw material to sulfuric acid is 3:1, mixing evenly, heating to 120° C., keeping the temperature for 6 hours, and performing oxidation cross-linking treatment to obtain an oxidation-cross-linked material;

[0096] S3: washing the oxidized-crosslinked material with a sodium carbonate aqueous solution and water in sequence until it becomes neutral, removing residual impurity ions in the material, and obtaining a washed material;

[0097] S4: granulating the washed material by spray granulation to obtain a spherical precursor with a D50 of 7 μm;

[0098] S5: In a nitrogen atmosphere, the spherical precursor is heated to 200° C. and kept for 1 h, then to 400° C. and kept for 2 h, and then to 550° C. and kept for 2 h, to obtain a low-temperature pretreated precursor;

[0099] S6: In a nitrogen atmosphere, the temperature is raised to 1400°C at a heating rate of 3°C / min to carbonize the low-temperature pretreated precursor for 3 hours to obtain a hard carbon negative electrode material.

[0100] Comparative Example 5

[0101] This comparative example provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0102] S1: mixing wheat starch, flax cellulose and polyurethane resin in a mass ratio of 1:6:3 to obtain a mixed raw material;

[0103] S2: Granulate the mixed raw materials by spray granulation to obtain a spherical precursor with a D50 of 7 μm;

[0104] S3: In a nitrogen atmosphere, the spherical precursor is heated to 200°C for 1 hour, then to 400°C for 2 hours, and then to 550°C for 2 hours to obtain a low-temperature pretreated precursor;

[0105] S4: In a nitrogen atmosphere, the temperature is raised to 1400°C at a heating rate of 3°C / min to carbonize the low-temperature pretreated precursor for 3 hours to obtain a hard carbon negative electrode material.

[0106] Comparative Example 6

[0107] This comparative example provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0108] S1: mixing wheat starch, flax cellulose and polyurethane resin in a mass ratio of 1:6:3 to obtain a mixed raw material;

[0109] S2: adding oxidizing acid sulfuric acid (mass fraction of 15%) to the mixed raw material, the mass ratio of the mixed raw material to sulfuric acid is 3:1, mixing evenly, heating to 120° C., keeping the temperature for 6 hours, and performing oxidation cross-linking treatment to obtain an oxidation-cross-linked material;

[0110] S3: washing the oxidized-crosslinked material with a sodium carbonate aqueous solution and water in sequence until it becomes neutral, removing residual impurity ions in the material, and obtaining a washed material;

[0111] S4: granulating the washed material by spray granulation to obtain a spherical precursor with a D50 of 7 μm;

[0112] S5: In a nitrogen atmosphere, the spherical precursor is heated to 400°C and kept at this temperature for 5 hours to obtain a low-temperature pretreated precursor;

[0113] S6: In a nitrogen atmosphere, the temperature is raised to 1400°C at a heating rate of 3°C / min to carbonize the low-temperature pretreated precursor for 3 hours to obtain a hard carbon negative electrode material.

[0114] The performance of the negative electrode materials prepared in the above embodiments and comparative examples was evaluated by button cells. The electrode slurry was prepared in the following ratio: active material: conductive agent SP: binder CMC: dispersant SBR = 92:3.0:1.5:3.5. Appropriate amounts of ethanol and water were added to prepare the slurry. The coating thickness was 200 μm. The electrode sheets were made into pole pieces after drying and tableting. Metal sodium was used as the counter electrode, 1 mol / L NaPF6 DEC / EC (1:1) solution was used as the electrolyte, and glass fiber filter paper membrane GF / C was used as the diaphragm. The 2032 button cells were assembled. The battery was tested at 0.1A g -1 The charge and discharge performance was tested at a current density of 10000, and the test results are shown in Table 1. At -10℃, the 5C rate discharge performance was verified, and the test results are shown in Table 1. Figure 1 shown.

[0115] The test results are shown in Table 1:

[0116] Table 1

[0117]

[0118]

[0119] The difference between Comparative Example 1 and Example 1 is that cellulose is not added to the mixed raw material, and the first efficiency of the prepared hard carbon negative electrode material is reduced due to the lack of structural stabilization of linear molecules;

[0120] The difference between Comparative Example 2 and Example 1 is that no starch is added to the mixed raw materials. Since the pore structure is underdeveloped during the carbonization process of the material, the specific capacity of the prepared hard carbon negative electrode material is greatly reduced;

[0121] The difference between Comparative Example 3 and Example 1 is that no resin is added to the mixed raw material, and because the toughness of the material is reduced, the particles are easily broken when working at a high rate, and the low-temperature dynamic performance of the prepared hard carbon negative electrode material is poor;

[0122] The difference between Comparative Example 4 and Example 1 is that the resin in the mixed raw material is replaced. Since polypropylene contains only two elements, C and H, and no isocyanate and polyol functional groups, the prepared hard carbon negative electrode material has low toughness and poor structural stability during high-rate discharge.

[0123] The difference between Comparative Example 5 and Example 1 is that the mixed raw material is not subjected to oxidative crosslinking treatment. Since there are fewer micropores and ultramicropores on the surface of the material, there are insufficient places for sodium ion diffusion, storage and deintercalation, and the specific capacity and first efficiency of the prepared hard carbon negative electrode material are relatively low;

[0124] The difference between Comparative Example 6 and Example 1 is that the spherical precursor is not carbonized at low temperature by gradually increasing the temperature. Since the volatile matter in the material is not completely evaporated, the micropores and pore structures required for sodium ion transfer are not rich enough, and the kinetic performance of the prepared hard carbon negative electrode material is poor.

[0125] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a hard carbon negative electrode material, characterized in that: The steps include: S1: Mixing starch, cellulose and resin to obtain a mixed raw material; S2: adding an oxidizing acid to the mixed raw material, and performing an oxidative crosslinking treatment at 50-200° C. to obtain an oxidized-crosslinked material; S3: washing the oxidation-crosslinked material to obtain a washed material; S4: granulating the washed material to obtain a spherical precursor; S5: performing low-temperature carbonization on the spherical precursor under an inert atmosphere to obtain a low-temperature pretreated precursor; S6: In an inert atmosphere, carbonizing the low-temperature pretreated precursor at 1200-1600° C. to obtain a hard carbon negative electrode material.

2. The method for preparing a hard carbon negative electrode material according to claim 1, characterized in that: The resin is selected from at least one of epoxy resin, phenolic resin, polycarbonate, polyurethane, polyvinyl chloride, ABS, furan resin, furfural resin, bismaleimide resin and polyimide resin.

3. The method for preparing a hard carbon negative electrode material according to claim 2, characterized in that: The mass ratio of the starch, the cellulose and the resin in step S1 is (1-5): (2-6): (3-6).

4. The method for preparing a hard carbon negative electrode material according to claim 1, characterized in that: The oxidizing acid is selected from at least one of sulfuric acid, nitric acid, permanganic acid, perchloric acid, chloric acid, and hypochlorous acid.

5. The method for preparing a hard carbon negative electrode material according to claim 4, characterized in that: The mass ratio of the mixed raw material to the oxidizing acid in step S2 is (1-10):

1.

6. The method for preparing a hard carbon negative electrode material according to claim 1, characterized in that: The particle size D50 of the spherical precursor in step S4 is 5-10 μm.

7. The method for preparing a hard carbon negative electrode material according to claim 1, characterized in that: Step S5 includes: in an inert atmosphere, heating the spherical precursor to 200° C. and keeping it for 1 hour, heating it to 400° C. and keeping it for 2 hours, and heating it to 550-600° C. and keeping it for 2 hours, to obtain a low-temperature pretreated precursor.

8. The method for preparing a hard carbon negative electrode material according to claim 1, characterized in that: In step S6, the temperature is increased to 1200-1600° C. at a heating rate of 0.5-5° C. / min.

9. A hard carbon negative electrode material, characterized in that: The hard carbon negative electrode material is prepared by the preparation method of any one of claims 1 to 8.

10. A sodium ion battery, characterized in that: Comprising the hard carbon negative electrode material as claimed in claim 9.

Citation Information

Patent Citations

  • Nitrogen and phosphorus co-doped sodium ion battery hard carbon negative electrode material and preparation method thereof

    CN116534839A

  • Sodium-ion battery anode material and preparation method thereof

    CN116666581A

  • Porous hard carbon negative electrode material, preparation method thereof and sodium ion battery

    CN117228670A

  • Soft carbon coated phosphorus / sodium co-doped hard carbon sodium ion battery negative electrode material and preparation method thereof

    CN118315549A

  • Pyrolytic amorphous carbon material, preparation method and use thereof

    WO2016074479A1

Cited By

  • Resin-based sodium ion battery hard carbon material and preparation method thereof

    CN119612494A

  • Preparation method of carbohydrate-based sodium ion battery hard carbon negative electrode material

    CN119706805A

  • Preparation method of hard carbon negative electrode material for sodium ion battery

    CN119706805B

  • Biomass-based hard carbon negative electrode material, preparation method thereof and sodium ion battery

    CN119873791A