Glass packaging material for lithium thionyl chloride battery and preparation method of glass packaging material

By using special glass material combinations and preparation processes, the problem of insufficient thionyl chloride resistance of glass packaging materials for lithium thionyl chloride batteries is solved, high-strength and air-tight packaging of lithium thionyl chloride batteries is achieved, and short circuits of the batteries due to corrosion are avoided. phenomenon.

CN118754446APending Publication Date: 2024-10-11LIAONING GLASS CERAMIC TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410921371.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The glass packaging material of lithium thionyl chloride batteries is not resistant to thionyl chloride, which causes corrosion reactions and makes the battery short-circuited and unusable.

Method used

Using a combination of special glass materials, including SiO2, B2O3, Al2O3, ZnO, K2O, Na2O, CaO, SrO, BaO, MgO, TiO2/ZrO2, La2O3/BeO, through melting, water quenching, ball milling, sieving and microcrystallization Processing to prepare alkali boron zinc aluminosilicate system crystallized glass powder for packaging of lithium thionyl chloride battery cover pack.

Benefits of technology

The material maintains high strength and airtightness within the temperature range of use, preventing corrosion reactions, ensuring that the battery will not be short-circuited due to corrosion of the glass material, and extending the service life of the battery.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a glass packaging material for a lithium thionyl chloride battery, which is prepared from the following components in percentage by mass: 20 to 55 percent of SiO2, 15 to 40 percent of B2O3, 5 to 20 percent of Al2O3, 5 to 15 percent of ZnO, 1 to 5 percent of K2O, 1 to 5 percent of Na2O, 2 to 10 percent of CaO, 2 to 10 percent of SrO, 2 to 10 percent of BaO, 2 to 10 percent of MgO, 6 to 10 percent of TiO2 / ZrO2 and 0.005 to 0.5 percent of La2O3 / BeO, the mass ratio of TiO2 to ZrO2 in TiO2 / ZrO2 is 7 to 3, and the mass ratio of La2O3 to BeO in La2O3 / BeO is 2 to 1. After the material provided by the invention is packaged with a cover group and the battery is packaged, the glass material of the cover group is non-corrosive, the condition that the battery cannot work due to short circuit caused by the corrosion of the packaging glass material can be avoided, and meanwhile, the battery can still have relatively high strength and relatively high air tightness in an allowable temperature range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electronic materials, and in particular to a glass packaging material for a lithium thionyl chloride battery and a preparation method thereof. Background Art

[0002] Lithium thionyl chloride battery is the battery with the highest specific energy among the current chemical power sources. It has high operating voltage, stable working platform, and the advantages of long-term energy storage. It is widely used in military electronic devices, gun sights, smart water meters and other military and civilian related fields. The packaging condition of the metal-glass encapsulated insulator cover assembly, a key component of lithium thionyl chloride battery, plays a vital role in its performance and safety and reliability in application.

[0003] At present, most of the glass packaging materials used in the production of lithium-thionyl chloride battery pack covers rely on imports. The packaging materials provided by many domestic enterprises, scientific research institutions, and universities cannot meet the requirements of use under working conditions. The common technical problem is that the packaging materials are not resistant to thionyl chloride, mainly because thionyl chloride can easily generate mixed acid when it meets water, and it is also very corrosive and can easily corrode stainless steel or general metals. Most of the glass materials used for packaging will also come into contact with it and react, causing the lithium-thionyl chloride battery to short-circuit and cannot be used.

[0004] Therefore, how to solve the problem of thionyl chloride intolerance of existing packaging glass materials is an urgent problem to be solved. Summary of the invention

[0005] In view of this, the present invention discloses a glass packaging material for lithium thionyl chloride batteries and a preparation method thereof, so as to provide a special glass material that can achieve good packaging with a thionyl chloride battery cover assembly.

[0006] In one aspect, the present invention provides a glass packaging material for lithium thionyl chloride batteries, which comprises SiO 2 20-55%, B 2 O 3 15-40%, Al 2 O 3 5-20%, ZnO 5-15%, K 2 O 1-5%, Na 2 O 1-5%, CaO 2-10%, SrO 2-10%, BaO 2-10%, MgO 2-10%, TiO 2 / ZrO 2 6-10%, La 2 O 3 / BeO0.005-0.5%, and TiO 2 / ZrO 2 Medium TiO2 The mass ratio with ZrO 2 is 7:3, and the mass ratio of La 2 O 3 / BeO to BeO is 2:1 in La 2 O 3 .

[0007] Preferably, by mass percentage, it includes SiO 2 20 - 55%, B 2 O 3 15 - 40%, Al 2 O 3 5 - 20%, ZnO 5 - 15%, K 2 O 1 - 5%, Na 2 O 1 - 5%, CaO 2 - 10%, SrO 2 - 10%, BaO 2 - 10%, MgO is 2 - 10%, TiO 2 / ZrO 2 6 - 10%, La 2 O 3 / BeO 0.005 - 0.5%, Y 2 O 3 0 - 2%, V 2 O 5 0 - 2%, CuO 0 - 2%, CeO 2 0 - 2%, Pr 6 O 11 0 - 2% or Li 2 O 0 - 2%, and in TiO 2 / ZrO 2 the mass ratio of TiO 2 to ZrO 2 is 7:3, and the mass ratio of La 2 O 3 / BeO to BeO is 2:1 in La 2 O 3 .

[0008] On the other hand, the present invention also provides a preparation method of the glass encapsulation material for the lithium thionyl chloride battery, including:

[0009] Step 1: Weigh each component of the raw materials by mass percentage and mix them evenly, and then melt the evenly mixed raw materials to obtain glass liquid;

[0010] Step 2: Pour out the melted glass liquid, and successively carry out water quenching, drying, ball milling, and sieving to obtain alkali borosilicate zinc aluminosilicate system glass powder;

[0011] Step 3: Perform microcrystallization treatment on the glass powder, allow the sample to cool in the furnace, and obtain alkali-boron-zinc-aluminum-silicate system microcrystalline glass powder.

[0012] Preferably, the method for melting the glass raw materials in step 1 comprises: placing the uniformly mixed raw materials into a platinum crucible, and keeping the temperature at 160-360°C for 0.5-2 hours at a heating rate of 2°C / min; continuing to heat to 1400-1600°C at a heating rate of 2-5°C / min, covering the crucible to prevent volatilization of boric acid, and keeping the temperature for 1-2 hours.

[0013] Preferably, step 3: microcrystallization treatment of alkali-boron-zinc-aluminum-silicate system glass powder comprises: heating the above-mentioned glass powder to 340-550°C at a speed of 4-8°C / min, and keeping it warm for 2-2.5 hours, comprising: heating the above-mentioned glass powder to 340-550°C at a speed of 4-8°C / min, and keeping it warm for 2-2.5 hours.

[0014] In addition, the present invention also provides the application of the glass packaging material for lithium thionyl chloride batteries, and the material is packaged and used with a lithium thionyl chloride battery cover assembly.

[0015] The present invention provides a glass packaging material for lithium thionyl chloride battery and a preparation method thereof. After the material is packaged with a cover group and packaged into a battery, the cover group glass material is corrosion-free, which can ensure that the battery will not be short-circuited and unable to work due to corrosion of the packaging glass material. At the same time, within the allowable temperature range, the material can still maintain high strength and high air tightness.

[0016] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. DETAILED DESCRIPTION

[0017] The present invention is further explained below in conjunction with specific implementation schemes, but it is not intended to limit the protection scope of the present invention.

[0018] This embodiment aims to solve the common technical problem in the field of lithium primary batteries that the glass packaging material of the lithium thionyl chloride battery cover group is not resistant to thionyl chloride and reacts with it, which will cause the lithium thionyl chloride battery to short-circuit and cannot be used. Therefore, the present invention provides a special glass material that can achieve good packaging with the lithium thionyl chloride battery cover group.

[0019] Specifically, an alkali-boron-zinc-aluminum-silicate glass material composition is: SiO 2 , B 2 O 3 、Al 2 O 3 , ZnO, K 2 O、Na2 O, CaO, SrO, BaO, MgO, TiO 2 , ZrO 2 , La 2 O 3、 BeO. By mass percentage: Among them, SiO 2 is 20 - 55%, B 2 O 3 is 15 - 40%, Al 2 O 3 is 5 - 20%, ZnO is 5 - 15%, K 2 O is 1 - 5%, Na 2 O is 1 - 5%, CaO is 2 - 10%, SrO is 2 - 10%, BaO is 2 - 10%, MgO is 2 - 10%, TiO 2 / ZrO 2 is 6 - 10%, La 2 O 3 / BeO is 0.005 - 0.5%, and in TiO 2 / ZrO 2 the mass ratio of TiO 2 to ZrO 2 is 7:3, and in La 2 O 3 / BeO the mass ratio of La 2 O 3 to BeO is 2:1.

[0020] In addition, in the alkali borosilicate zinc aluminosilicate system glass material described in the present invention, Y 2 O 3 , V 2 O 5 , CuO or Li 2 O, CeO 2 or Pr 6 O 11 can also be added. Among them, Y 2 O 3 is 0 - 2%, V 2 O 5 is 0 - 2%, CuO is 0 - 2%, CeO 2 is 0 - 2%, Pr 6 O 11 is 0 - 2% or Li 2 O is 0 - 2%.

[0021] That is, an alkali borosilicate zinc aluminosilicate system glass material, including SiO 2 20 - 55%, B 2 O 3 15 - 40%, Al 2O 3 5 - 20%, ZnO 5 - 15%, K 2 O 1 - 5%, Na 2 O 1 - 5%, CaO 2 - 10%, SrO 2 - 10%, BaO 2 - 10%, MgO is 2 - 10%, TiO 2 / ZrO 2 6 - 10%, La 2 O 3 / BeO 0.005 - 0.5%, Y 2 O 3 0 - 2%, V 2 O 5 0 - 2%, CuO 0 - 2%, CeO 2 0 - 2%, Pr 6 O 11 0 - 2% or Li 2 O 0 - 2%, and TiO 2 / ZrO 2 中TiO 2 与ZrO 2 的质量比为7:3, La 2 O 3 / BeO中La 2 O 3 与BeO的质量比例为2:1.

[0022] The present invention also provides a preparation method of the above - mentioned material, including

[0023] Weigh the above - mentioned components according to mass percentage and mix them evenly.

[0024] Put the evenly - mixed raw materials into a platinum crucible, heat them at a heating rate of 2 °C / min to 160 - 360 °C and keep them warm for 0.5 - 2 hours; continue to heat them at a heating rate of 2 - 5 °C / min to 1400 - 1600 °C, cover the crucible to prevent the volatilization of boric acid, keep them warm for 1 - 2 hours, and melt the glass raw materials. Pour out the melted glass liquid, and successively carry out water quenching, drying, ball milling, and sieving through 80 - mesh to obtain the alkali - borosilicate - zinc - aluminum glass powder. Heat the above - mentioned glass powder at a speed of 4 - 8 °C / min to 340 - 550 °C and keep it warm for 2 - 2.5 hours to carry out crystallization treatment on the glass powder, and let the sample cool with the furnace to obtain the alkali - borosilicate - zinc - aluminum glass - ceramic material.

[0025] In the present invention, SiO 2 、B 2 O 3 are glass network formers, ZnO is a glass network - adjusting oxide, Al 2 O 3 is an intermediate oxide, TiO2 、ZrO 2 It is a mixed nucleating agent and a required oxide, in order to enable the solid solution to be smoothly precipitated from the microcrystalline state of the glass during the heat treatment process. 2 O、Na 2 O is a network external body formation, does not participate in the network, is generally outside the network, and is a required oxide. These two alkali metal oxides play a role in high-temperature melting and accelerate the melting of glass. CaO, SrO, BaO, and MgO are alkaline earth metal ions, which have the effect of surrounding and closing the alkali metal ions, and can prevent the effect of restricting the movement of alkali metal ions; La 2 O 3 The synergistic introduction of rare earth and alkaline earth as glass property regulators can significantly improve the corrosion resistance of glass; in addition, V 2 O 5 、CuO、Li 2 O、CeO 2 , Pr 6 O 11 etc. can be introduced as glass property regulators and La 2 O 3 / BeO rare earth and alkaline earth synergistically improve the corrosion resistance of glass.

[0026] The composition of the present invention adopts the method of synergistically introducing rare earth oxides and alkaline earth oxides to prepare alkali boron zinc aluminum silicate system microcrystalline glass powder material. As a packaging material for lithium thionyl chloride batteries, the microcrystalline glass powder material has good and stable thionyl chloride resistance and can be a special glass material that can be well packaged with a lithium thionyl chloride battery cover assembly. Within the allowable temperature range, it can still maintain high strength and high air tightness.

[0027] The present invention is further explained below in conjunction with specific embodiments, but is not intended to limit the protection scope of the present invention.

[0028] Embodiment 1:

[0029] An alkali-boron-zinc-aluminum-silicate system glass-ceramics powder material, the alkali-boron-zinc-aluminum-silicate system glass-ceramics powder components are calculated by mass %: SiO 2 35%, B 2 O 3 30%, Al 2 O 3 10%, ZnO 5%, K 2 O is 2%, Na 2 O is 3%, CaO is 4%, SrO is 3%, BaO is 4%, MgO is 3%, TiO 2 / ZrO 2 6%, Pr 6 O11 0.005%, La 2 O 3 / BeO is 0.005%.

[0030] The method for preparing the above-mentioned alkali-boron-zinc-aluminum-silicate system glass-ceramics powder material comprises the following steps:

[0031] The above components are weighed according to mass percentage and mixed evenly. Agate balls are used as grinding media during the grinding process.

[0032] Put the mixed raw materials into a platinum crucible and keep the temperature at 260°C for 2 hours at a heating rate of 2°C / min; continue to heat to 1550°C at a heating rate of 5°C / min, cover the crucible to prevent the volatilization of boric acid, keep the temperature for 2 hours, and melt the glass raw materials. Pour out the molten glass liquid, and then quench with water, dry, ball mill, and sieve 80 mesh in sequence to obtain alkali boron zinc aluminum silicate system glass powder. Heat the above glass powder to 480°C at a speed of 5°C / min and keep it warm for 2.5 hours, perform microcrystallization treatment on the glass powder, and cool the sample with the furnace to obtain alkali boron zinc aluminum silicate system microcrystalline glass powder.

[0033] The prepared alkali-boron-zinc-aluminum silicate system glass-ceramics powder was sprayed with 0.5% PVA binder, passed through an 80-mesh sieve, aged for 12 h, and dry-pressed into round rods with a diameter of 5 mm and a length of 40 mm at 15 MPa. The linear expansion coefficient was tested and the linear expansion coefficient was 95×10 -7 / ℃ (25~300℃); dry pressed into a glass blank with a diameter of 13mm and a thickness of 2mm using the same process, and sintered in two stages, first pre-sintered at 350℃ for 20min, then sintered at 1080℃ for 40min, cooled naturally to room temperature, and polished the test surface with a polisher. The polished glass block was then cleaned with alcohol and dried to test its electrical properties. At room temperature 1KHZ, the dielectric constant was 8.9, and the volume resistivity at room temperature was 1.5×10 15 Ω·cm, the breakdown strength at room temperature is 28kV / mm; the water resistance stability is tested to be level Ⅰ; the acid resistance chemical stability is H1; after packaging with the cover group, the vacuum leakage rate is tested to be 1.2×10 -9 Pa﹒ 3 / sec; After being packaged with the cover group to make a battery, it was baked at 80℃ for 4 months. After dissection, it was found that there was no corrosion of the glass material of the cover group to cause a short circuit.

[0034] Example 2

[0035] An alkali-boron-zinc-aluminum-silicate system glass-ceramic powder material. The components of the alkali-boron-zinc-aluminum-silicate system glass-ceramic powder are as follows: SiO 2 is 45%, B2 O 3 25%, Al 2 O 3 15%, ZnO 5%, K 2 O is 2%, Na 2 O is 3%, CaO is 3%, SrO is 3%, BaO is 3%, MgO is 3%, TiO 2 / ZrO 2 5%, La 2 O 3 / BeO is 0.005%, V 2 O 5 It is 0.003% and CuO is 0.002%.

[0036] The method for preparing the above-mentioned alkali-boron-zinc-aluminum-silicate system glass-ceramics powder material comprises the following steps:

[0037] The above components are weighed according to mass percentage and mixed evenly. Agate balls are used as grinding media during the grinding process.

[0038] The mixed raw materials are placed in a platinum crucible and kept warm for 2 hours at a heating rate of 2°C / min to 280°C; the temperature is continued to rise to 1600°C at a heating rate of 5°C / min, and the crucible is covered to prevent the volatilization of boric acid. The glass raw materials are melted for 2 hours. The molten glass liquid is poured out, and it is successively quenched with water, dried, ball milled, and sieved through 80 mesh to obtain alkali-boron-zinc-aluminum-silicate system glass powder. The above glass powder is heated to 480°C at a speed of 5°C / min and kept warm for 2.5 hours. The glass powder is microcrystallized and the sample is cooled with the furnace to obtain alkali-boron-zinc-aluminum-silicate system microcrystalline glass powder.

[0039] The prepared alkali-boron-zinc-aluminum silicate system glass-ceramics powder was sprayed with 0.5% PVA binder, passed through an 80-mesh sieve, aged for 12 h, and dry-pressed into round rod samples with a diameter of 5 mm and a length of 40 mm at 15 MPa. The linear expansion coefficient was tested and the linear expansion coefficient was 85×10 -7 / ℃ (25~300℃); the same process is used to dry press it into a glass blank with a diameter of 13mm and a thickness of 2mm. A two-stage sintering method is used, first pre-sintering at 350℃ for 20min, then sintering at 1080℃ for 40min, cooling naturally to room temperature, and polishing the test surface with a polishing machine. The polished glass block is then cleaned with alcohol on the polished surface and dried to test its electrical properties. At room temperature 1KHZ, the dielectric constant is 8.9, and the volume resistivity at room temperature is 1.3×10 15Ω·cm, the breakdown strength at room temperature is 27kV / mm; the water resistance stability is tested to be level Ⅰ; the acid resistance chemical stability is H1; after packaging with the cover group, the vacuum leakage rate is tested to be 1.3×10 -9 Pa﹒ 3 / sec; After being packaged with the cover group to make a battery, it was baked at 80℃ for 4 months. After dissection, it was found that there was no corrosion of the glass material of the cover group to cause a short circuit.

[0040] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the invention disclosed herein. This application is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not disclosed by the present invention. The specification and examples are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the following claims.

[0041] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. Glass packaging materials for lithium thionyl chloride batteries, It is characterized in that By mass percentage, it includes SiO 2 20 - 55%, B 2 O 3 15 - 40%, Al 2 O 3 5 - 20%, ZnO 5 - 15%, K 2 O 1 - 5%, Na 2 O 1 - 5%, CaO 2 - 10%, SrO 2 - 10%, BaO 2 - 10%, MgO is 2 - 10%, TiO 2 / ZrO 2 6 - 10%, La 2 O 3 / BeO 0.005 - 0.5%, and in TiO 2 / ZrO 2 the mass ratio of TiO 2 to ZrO 2 is 7:3, and in La 2 O 3 / BeO the mass ratio of La 2 O 3 to BeO is 2:

1.

2. The glass packaging material for lithium thionyl chloride batteries according to claim 1, It is characterized in that By mass percentage, it includes SiO 2 20 - 55%, B 2 O 3 15 - 40%, Al 2 O 3 5 - 20%, ZnO 5 - 15%, K 2 O 1 - 5%, Na 2 O 1 - 5%, CaO 2 - 10%, SrO 2 - 10%, BaO 2 - 10%, MgO is 2 - 10%, TiO 2 / ZrO 2 6 - 10%, La 2 O 3 / BeO 0.005 - 0.5%, Y 2 O 3 0 - 2%, V 2 O 5 0 - 2%, CuO 0 - 2%, CeO 2 0 - 2%, Pr 6 O 11 0 - 2% or Li 2 O 0 - 2%, and in TiO 2 / ZrO 2 the mass ratio of TiO 2 to ZrO 2 is 7:3, and in La 2 O 3 / BeO the mass ratio of La 2 O 3 to BeO is 2:

1.

3. A method for preparing a glass packaging material for a lithium thionyl chloride battery according to any one of claims 1 to 2, It is characterized in that include: Step 1: Weigh each component of the raw material according to mass percentage and mix them evenly, melt the evenly mixed raw materials, and obtain glass liquid after melting; Step 2: pour out the molten glass liquid, and sequentially perform water quenching, drying, ball milling, and sieving to obtain alkali-boron-zinc-aluminum silicate system glass powder; Step 3: Perform microcrystallization treatment on the alkali-boron-zinc-aluminum-silicate system glass powder, and allow the sample to cool in the furnace to obtain alkali-boron-zinc-aluminum-silicate system microcrystalline glass powder.

4. The method for preparing the glass packaging material for lithium thionyl chloride batteries according to claim 3, It is characterized in that The method for melting the mixed raw materials in step 1 includes: placing the mixed raw materials into a platinum crucible, heating the mixture to 160-360° C. at a heating rate of 2° C. / min for 0.5-2 hours; heating the mixture to 1400-1600° C. at a heating rate of 2-5° C. / min, covering the crucible to prevent the volatilization of boric acid, and heating the mixture for 1-2 hours.

5. The method for preparing the glass packaging material for lithium thionyl chloride batteries according to claim 3, It is characterized in that Step 3: microcrystallization treatment of alkali-boron-zinc-aluminum-silicate system glass powder, including: heating the above glass powder to 340-550° C. at a speed of 4-8° C. / min, and keeping it warm for 2-2.5 hours.

6. Application of the glass packaging material for lithium thionyl chloride batteries according to any one of claims 1-2, It is characterized in that The material is packaged with a lithium thionyl chloride battery cover assembly for use.

Citation Information

Cited By

  • Application of beryllium oxide in slurry development

    CN119707302A