Binder for battery diaphragm, preparation method of binder, battery diaphragm and secondary battery
By using polymer binders containing amine and cyano functional groups in lithium-ion batteries, the problem of HF generation caused by the decomposition of lithium hexafluorophosphate is solved, the cycle life and safety performance of the battery are improved, and the stability of the electrolyte is achieved and bonding strength.
Patent Information
- Application Number
- CN202411053893.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-11
AI Technical Summary
In existing lithium-ion batteries, lithium hexafluorophosphate decomposes under high temperature or water-containing conditions to produce hydrofluoric acid, which leads to the dissolution of transition metals in the cathode material and the decomposition of the binder, thereby accelerating the generation of HF, forming a vicious cycle and damaging the battery cycle performance.
Using a polymer binder containing amine and cyano functional groups, it is prepared through heat treatment and reaction with acrylonitrile monomers to form a binder with high dielectric constant and oxidation resistance stability, which can remove trace amounts of chemicals in the electrolyte. The HF formed by the oxidative decomposition reaction caused by water reduces the dissolution of transition metals in the cathode material.
It improves the cycle life and safety performance of lithium-ion batteries, enhances the bonding strength and electrolyte adsorption capacity of the battery separator, effectively removes HF, reduces the dissolution of cathode materials, and extends the cycle performance of the battery.
Smart Images

Figure BDA0004975748670000101 
Figure BDA0004975748670000181 
Figure BDA0004975748670000191
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a binder for battery separators and a preparation method thereof, a battery separator and a secondary battery. Background Art
[0002] As an efficient electrochemical energy storage device, lithium-ion batteries have attracted extensive attention from academia and industry due to their high energy density and low redox potential. The market places higher demands on the cycle life, energy density and safety performance of lithium-ion batteries. Electrolytes and binders are necessary components of lithium-ion batteries, but the commonly used electrolytes today contain lithium hexafluorophosphate and alkyl carbonate solvents; however, lithium hexafluorophosphate decomposes to produce hydrofluoric acid (HF) and hexafluorophosphate ions under high temperature or water conditions, which leads to the dissolution of transition metals (such as nickel, cobalt, manganese, etc.) in the positive electrode material and the decomposition of the binder, thereby accelerating the generation of HF to form a vicious cycle. Transition metal elements dissolve, migrate and deposit in the electrolyte to the negative electrode of the battery, destroying and regenerating the negative electrode SEI film, making it impossible to form a flat and dense structure. This leads to severe gas production and increased internal resistance of the battery, consuming a large amount of active lithium and causing a decrease in battery cycle performance.
[0003] In the prior art, there are a variety of technical means to solve or prevent the adverse consequences caused by the decomposition of lithium hexafluorophosphate to produce HF. For example, replacing lithium hexafluorophosphate with other lithium salts can fundamentally reduce the generation and diffusion of hydrofluoric acid, but the electron-withdrawing effect of the fluorine element helps to distribute negative charges, thereby reducing the lattice energy of the salt, improving ion dissociation, and promoting the dissolution of the salt in organic solvents. After replacement, the lithium salt has poor solubility and low ion conductivity. For example, patent CN116805715A, by adding an electrolyte additive containing a double-bond amine compound, that is, by introducing a double bond in the amine molecule, the functional additive can remove hydrofluoric acid while maintaining the ability to remove water, but it will cause adverse consequences such as decreased electrolyte conductivity and increased battery internal resistance.
[0004] Therefore, it is very important to develop a binder that has excellent adsorption effect on hydrofluoric acid and can ensure excellent cycle performance of the battery.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] One object of the present invention is to provide a binder for battery separators, which can improve the high cohesive energy between the coating and the positive and negative electrode sheets, while being able to remove HF formed by the oxidative decomposition reaction of the electrolyte caused by trace water during the circulation process, thereby reducing the dissolution of transition metals during the circulation of the positive electrode material, and thereby improving the cycle life of the lithium-ion battery.
[0007] Another object of the present invention is to provide a method for preparing the adhesive for battery separators, which is simple and easy to implement with low cost, and the obtained adhesive has excellent bonding performance and oxidation resistance stability.
[0008] Another object of the present invention is to provide a battery separator.
[0009] Another object of the present invention is to provide a secondary battery.
[0010] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0011] A binder for a battery separator, comprising a binder material, wherein the molecular structure of the binder material comprises a first structure and a second structure; the first structure comprises a polymer main chain structure containing a first functional group, wherein the first functional group comprises an amine group, or an amine group and an amide group; the second structure comprises a carbon chain containing a cyano group; and the group to which the nitrogen atoms in part of the first functional group are connected is the second structure.
[0012] In some embodiments, the first structure is derived from an amine-containing polymer and / or an amine- and amide-containing polymer.
[0013] In some embodiments, the molar ratio of the first functional group to the cyano group is 10:3-8.
[0014] In some embodiments, the molar ratio of the amide group to the first functional group is less than or equal to 20%.
[0015] In some embodiments, the amine-containing polymer contains primary amine groups, secondary amine groups and tertiary amine groups. Relative to the total amount of amine groups in the amine-containing polymer, the molar ratio N1 of the primary amine groups is 20% to 30%, the molar ratio N2 of the secondary amine groups is 40% to 60%, the molar ratio N3 of the tertiary amine groups is 20% to 30%, and N1+N2+N3=100%.
[0016] In some embodiments, the amine-containing polymer comprises polyethyleneimine.
[0017] In some embodiments, the weight average molecular weight of the amine-containing polymer is 10,000 to 300,000 g / mol.
[0018] In some embodiments, the number of carbon atoms in the carbon chain containing a cyano group is 3 to 8.
[0019] In some embodiments, the carbon chain containing a cyano group is derived from an olefin nitrile monomer.
[0020] In some embodiments, the swelling rate of the bonding material in the electrolyte is 100% to 400%.
[0021] In some embodiments, the D50 particle size of the bonding material is 0.01-0.25 μm.
[0022] In some embodiments, the battery separator binder further comprises water, and the solid content of the battery separator binder is 5% to 25%.
[0023] The method for preparing the adhesive for battery separator as described above comprises the following steps:
[0024] A mixture of a polymer material and water is heat-treated to obtain a first system, wherein the polymer material includes an amine-containing polymer and / or an amine- and amide-containing polymer; under protective gas conditions, the first system is mixed and reacted with olefin nitrile monomers, and then the residual olefin nitrile monomers are removed to obtain a binder for a battery separator.
[0025] In some embodiments, the amine-containing polymer contains primary amine groups, secondary amine groups and tertiary amine groups. Relative to the total amount of amine groups in the amine-containing polymer, the molar ratio N1 of the primary amine groups is 20% to 30%, the molar ratio N2 of the secondary amine groups is 40% to 60%, the molar ratio N3 of the tertiary amine groups is 20% to 30%, and N1+N2+N3=100%.
[0026] In some embodiments, the amine-containing polymer comprises polyethyleneimine.
[0027] In some embodiments, the weight average molecular weight of the amine-containing polymer is 10,000 to 300,000 g / mol.
[0028] In some embodiments, the molar ratio of the structural unit of the polymer material to the olefin nitrile monomer is 10:3-8.
[0029] In some embodiments, the heat treatment temperature is 50-70° C., and the heat treatment time is 0.5-1 h.
[0030] In some implementations, the mixing specifically includes: dropping the olefin nitrile monomer into the first system.
[0031] In some embodiments, the reaction time is 10 to 15 hours.
[0032] In some embodiments, the preparation method of the polymer containing amino groups and amide groups specifically includes: mixing a carboxyl-containing monomer and a hydroxide of M, where M is selected from lithium or sodium, to obtain an M salt of the carboxyl-containing monomer; hot mixing and reacting the M salt of the carboxyl-containing monomer with water and an amino-containing polymer, and removing the residual carboxyl-containing monomer to obtain an amino- and amide-containing polymer.
[0033] In some embodiments, the molar ratio of the structural units of the carboxyl-containing monomer, the hydroxide of M and the first amine-containing polymer is 1:1:4-10.
[0034] In some embodiments, during the preparation of the polymer containing amine groups and amide groups, the temperature of hot mixing is 50 to 65° C., and the reaction time is 10 to 15 hours.
[0035] In some embodiments, the solid content of the polymer containing amine groups and amide groups is 8% to 12%.
[0036] A battery separator comprises a base film and a heat-resistant layer located on at least one surface of the base film; the heat-resistant layer comprises an inorganic material and a bonding material in the bonding agent for the battery separator.
[0037] In some embodiments, the particle size D50 of the inorganic material is 0.1-1.2 μm, and the particle size D50 of the bonding material is 0.01-0.25 μm; the mass ratio of the inorganic material to the bonding material is 10:1-100:1.
[0038] In some embodiments, the base film has a thickness of 5 to 16 μm, and the heat-resistant layer has a thickness of 1 to 4 μm.
[0039] In some embodiments, the inorganic material includes at least one of aluminum oxide, silicon oxide, boehmite, titanium oxide, zirconium oxide, and aluminum hydroxide.
[0040] In some embodiments, the heat-resistant layer further includes a stabilizer, the mass of the stabilizer is 0.2% to 2% of the mass of the inorganic material; the stabilizer includes at least one of gelatin, hydroxyethyl cellulose, methyl cellulose, xanthan gum, β-cyclodextrin and sodium carboxymethyl cellulose.
[0041] In some embodiments, the heat-resistant layer is obtained by coating a coating slurry onto the surface of the base film and then drying the coating slurry; the coating slurry comprises the inorganic material, a binder for a battery separator, a stabilizer, and a wetting agent.
[0042] In some implementations, the mass of the wetting agent is 0.2% to 2% of the mass of the inorganic material; the wetting agent includes at least one of sodium dodecyl sulfate, fatty alcohol, sodium butyl naphthalene sulfonate and nonylphenol polyoxyethylene ether.
[0043] A secondary battery comprises the battery separator.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] (1) In the binder of the present invention, the binder material contains a first functional group and a cyano group, which can maintain excellent bonding strength and the alkalinity of the amine group. At the same time, the nitrile group structure has the advantages of high dielectric constant and oxidation resistance stability. While increasing the high cohesive energy between the coating and the positive and negative electrode sheets, it can remove HF formed by the oxidative decomposition reaction caused by trace water in the electrolyte during the circulation process, reduce the dissolution of transition metals in the positive electrode material during the circulation process, and thus improve the cycle life of the lithium ion battery.
[0046] (2) The preparation method of the binder for battery separator of the present invention is simple and easy. By combining various steps, a binder containing a first functional group and a cyano group can be obtained. The binder has excellent binder performance and oxidative stability. It can effectively remove HF formed by oxidative decomposition reaction caused by trace water in the electrolyte during circulation, reduce transition metal dissolution during the circulation of positive electrode materials, and improve the cycle performance and safety performance of the battery.
[0047] (3) The battery separator of the present invention has a heat-resistant layer with excellent bonding strength. When used to prepare a battery, the separator has an enhanced electrolyte adsorption capacity, can effectively remove HF, reduce transition metal dissolution during the cycle, and improve the battery capacity retention rate. DETAILED DESCRIPTION
[0048] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0049] According to one aspect of the present invention, the present invention relates to a binder for battery separators, the binder for battery separators comprising a binder material, the molecular structure of the binder material comprising a first structure and a second structure; the first structure comprising a polymer main chain structure containing a first functional group, the first functional group comprising an amine group, or an amine group and an amide group; the second structure comprising a carbon chain containing a cyano group; the group connected to the nitrogen atoms in part of the first functional group is the second structure.
[0050] In the binder of the present invention, the binder material contains both the first functional group and the cyano group. The binder can not only maintain excellent bonding strength and the alkalinity of the amine group, but also the nitrile structure has the advantages of high dielectric constant, oxidation resistance and stability, etc., and can improve the high cohesive energy between the coating and the positive and negative electrode sheets, while being able to remove HF formed by the oxidation decomposition reaction of the electrolyte caused by trace water during the circulation process, and reduce the dissolution of transition metals during the circulation process of the positive electrode material, thereby improving the cycle life of the lithium ion battery.
[0051] In some embodiments, the first structure is derived from an amine-containing polymer and / or an amine- and amide-containing polymer.
[0052] In some embodiments, the molar ratio of the first functional group to the cyano group is 10:3 to 8, including but not limited to 10:3, 10:4, 10:5, 10:6, 10:7 or 10:8, etc. In the binder of the present invention, the ratio of the molar number of the cyano group to the molar number of the first functional group is within the above-mentioned suitable range, which is more conducive to ensuring the adsorption effect of the obtained binder on hydrofluoric acid and can better ensure the cycle performance of the battery.
[0053] In some embodiments, the molar ratio of the amide group to the first functional group is less than or equal to 20%, including but not limited to 1%, 2%, 5%, 8%, 10%, 12%, 15%, 18% or 20%, or any range between the two.
[0054] In some embodiments, the weight average molecular weight of the amine-containing polymer is 10000-300000 g / mol, including but not limited to 10000 g / mol, 20000 g / mol, 50000 g / mol, 100000 g / mol, 200000 g / mol, 250000 g / mol, 300000 g / mol, etc., or a range between any two of the above. In some embodiments, the amine-containing polymer includes polyethyleneimine (PEI). In some embodiments, the amine-containing polymer contains primary amine groups, secondary amine groups and tertiary amine groups. Relative to the total amount of amine groups in the amine-containing polymer, the molar ratio N1 of the primary amine groups is 20% to 30%, including but not limited to 20%, 22%, 25%, 28% or 30%, or any range between the two; the molar ratio N2 of the secondary amine groups is 40% to 60%, including but not limited to 40%, 45%, 50%, 55% or 60%, etc., or any range between the two. The molar ratio N3 of the tertiary amine groups is 20% to 30%, including but not limited to 20%, 22%, 25%, 28% or 30%, etc., or any range between the two. And N1+N2+N3=100%.
[0055] In some embodiments, the carbon chain containing a cyano group has 3 to 8 carbon atoms. The carbon chain containing a cyano group is derived from an olefin nitrile monomer. In some embodiments, the olefin nitrile monomer includes acrylonitrile and / or crotononitrile.
[0056] In some embodiments, the swelling rate of the adhesive material in the electrolyte is 100% to 400%, including but not limited to 100%, 150%, 200%, 250%, 300%, 350% or 400%, or any range between the two. The adhesive material of the present invention has the characteristic of high swelling rate.
[0057] In some embodiments, the bonding material of the present invention has a suitable particle size range, and the D50 particle size of the bonding material is 0.01-0.25 μm, including but not limited to 0.01 μm, 0.05 μm, 0.08 μm, 0.1 μm, 0.2 μm, 0.25 μm, etc., or any range value between the two.
[0058] In some embodiments, the binder for battery separators further comprises water. The binder of the present invention has a suitable solid content. The solid content of the binder for battery separators is 5% to 25%, including but not limited to 5%, 8%, 10%, 15%, 20%, 25%, etc., or any range value between the two.
[0059] According to another aspect of the present invention, the present invention also relates to a method for preparing the binder for battery separator as described above, comprising the following steps:
[0060] A mixture of a polymer material and water is heat-treated to obtain a first system, wherein the polymer material includes an amine-containing polymer and / or an amine- and amide-containing polymer; under protective gas conditions, the first system is mixed and reacted with olefin nitrile monomers, and then the residual olefin nitrile monomers are removed to obtain a binder for a battery separator.
[0061] The preparation method of the battery separator binder of the present invention is simple and easy. The binder containing the first functional group and the cyano group can be obtained by combining the various steps, and the excellent bonding strength of PEI and the alkalinity of the amine group can be maintained. At the same time, the nitrile group structure has a high dielectric constant and oxidation resistance stability. The battery separator binder can remove HF formed by the oxidation decomposition reaction caused by trace water in the electrolyte during the circulation process and reduce the dissolution of transition metals in the circulation process of the positive electrode material, thereby improving the cycle life of the lithium ion battery.
[0062] In some embodiments, the amine-containing polymer contains primary amine groups, secondary amine groups and tertiary amine groups. Relative to the total amount of amine groups in the amine-containing polymer, the molar ratio N1 of the primary amine groups is 20% to 30%, such as 20%, 22%, 25%, 28% or 30%, etc., the molar ratio N2 of the secondary amine groups is 40% to 60%, such as 40%, 45%, 50%, 55%, 60%, etc., the molar ratio N3 of the tertiary amine groups is 20% to 30%, such as 20%, 22%, 25%, 28% or 30%, etc., and N1+N2+N3=100%. In some embodiments, the amine-containing polymer includes polyethyleneimine. The solid content of the amine-containing polymer is 30% to 40%. In some embodiments, the weight average molecular weight of the amine-containing polymer is 10,000 to 300,000 g / mol, including but not limited to 10,000 g / mol, 20,000 g / mol, 50,000 g / mol, 100,000 g / mol, 200,000 g / mol, 250,000 g / mol, 300,000 g / mol, etc. The present invention is more conducive to ensuring the comprehensive performance of the obtained binder by limiting the specific molecular weight of the amine-containing polymer and the molar ratio of the secondary amine group, the secondary amine group and the tertiary amine group contained therein, and is more conducive to ensuring the effect of removing HF formed by the oxidative decomposition reaction of the electrolyte caused by trace water during the circulation process, which is conducive to reducing the dissolution of transition metals during the circulation process of the positive electrode material and improving the cycle performance of the battery.
[0063] In some embodiments, the molar ratio of the structural unit of the polymer material to the olefin nitrile monomer is 10:3-8, for example, 10:3, 10:4, 10:5, 10:6, 10:7, 10:8, etc.
[0064] In some embodiments, the solid content of the mixture of the polymer material and water is 5% to 25%, such as 5%, 10%, 15%, 20% or 25%, etc. That is, the polymer material is diluted to 5% to 25% with water.
[0065] In some embodiments, the heat treatment temperature is 50-70°C, including but not limited to 50°C, 53°C, 55°C, 58°C, 60°C, 65°C, 70°C, etc., or any range between the two. The heat treatment time is 0.5-1h, such as 0.5h, 0.8h, 1h. The present invention can better disperse the amine-containing polymer by combining appropriate heat treatment temperature and time. Stirring is performed during the heat treatment process.
[0066] In some embodiments, under protective gas conditions, the specific acquisition method includes: introducing protective gas to expel oxygen, and the introduction time is 20 to 40 minutes.
[0067] In some embodiments, the mixing specifically includes: adding the olefin nitrile monomer dropwise to the first system. Adding the olefin nitrile monomer dropwise is more conducive to ensuring the reaction, thereby improving the conversion rate and ensuring the comprehensive performance of the final binder.
[0068] In some embodiments, the reaction time is 10 to 15 hours, including but not limited to 10 hours, 11 hours, 12 hours, 13 hours, 14 hours or 15 hours, or any range between two hours.
[0069] In some embodiments, the preparation method of the polymer containing amino groups and amide groups specifically comprises: mixing a carboxyl-containing monomer and a hydroxide of M, wherein M is selected from lithium or sodium, to obtain an M salt of the carboxyl-containing monomer; hot mixing and reacting the M salt of the carboxyl-containing monomer with water and an amino-containing polymer, and removing the residual carboxyl-containing monomer to obtain an amino- and amide-containing polymer. The molar ratio of the structural units of the carboxyl-containing monomer, the hydroxide of M and the first amino-containing polymer is 1:1:4-10. In some embodiments, during the preparation of the polymer containing amino groups and amide groups, the temperature of hot mixing is 50-65°C, such as 50°C, 55°C, 60°C, 65°C, etc., and the reaction time is 10-15h, such as 10h, 11h, 12h, 14h or 15h, etc. The solid content of the polymer containing amino groups and amide groups is 8%-12%, such as 8%, 10% or 12%, etc.
[0070] The above method can obtain an emulsion or dispersion of the bonding material, wherein the continuous phase is water or a solution with water as a solvent; and the diameter is 0.01 to 0.25 μm.
[0071] In some embodiments, the reaction of the polymer material and acrylonitrile is shown below, where formula (I) is the polymer material and formula (II) is the resulting bonding material.
[0072]
[0073] According to another aspect of the present invention, the present invention also relates to a battery separator, comprising a base film and a heat-resistant layer located on at least one side of the base film; the heat-resistant layer comprises an inorganic material and a bonding material in the bonding agent for the battery separator.
[0074] The battery separator of the present invention can ensure the comprehensive performance of the battery separator by combining the inorganic material and the bonding material.
[0075] In some embodiments, the particle size D50 of the inorganic material is 0.1 to 1.2 μm, such as 0.1 μm, 0.2 μm, 0.5 μm, 0.8 μm, 1 μm or 1.2 μm, or any range between the two. The particle size D50 of the bonding material is 0.01 to 0.25 μm, such as 0.01 μm, 0.05 μm, 0.08 μm, 0.1 μm, 0.2 μm, 0.25 μm, or any range between the two. In some embodiments, the thickness of the base film is 5 to 16 μm, such as 5 μm, 8 μm, 10 μm, 12 μm, 15 μm or 16 μm, etc. The thickness of the heat-resistant layer is 1 to 4 μm, such as 1 μm, 2 μm, 3 μm, 4 μm, etc. In some embodiments, the mass ratio of the inorganic material to the bonding material is 10:1 to 100:1, such as 10:1, 20:1, 30:1, 50:1, 60:1, 80:1 or 100:1, etc. In some embodiments, the inorganic material includes at least one of aluminum oxide, silicon oxide, boehmite, titanium oxide, zirconium oxide and aluminum hydroxide. In some embodiments, the inorganic material can be any one of the above, or a combination of several, such as a combination of silicon oxide and boehmite, a combination of titanium oxide, zirconium oxide and aluminum hydroxide, etc. The present invention adopts inorganic materials with suitable particle size and suitable mass ratio and bonding materials to form a heat-resistant layer of suitable thickness, which is more conducive to ensuring the comprehensive performance of the obtained battery separator and improving the cycle performance of the battery.
[0076] In the present invention, the heat-resistant layer is prepared from a coating slurry, the coating slurry comprises the above-mentioned inorganic material and a binder for a battery separator, and the battery separator is obtained by coating the coating slurry on the surface of the base film and further drying it.
[0077] In some embodiments, the heat-resistant layer further includes a stabilizer, and the mass of the stabilizer is 0.2% to 2% of the mass of the inorganic material, such as 0.2%, 0.5%, 0.6%, 0.8%, 1%, 1.5% or 2%, or any range between the two. The stabilizer includes at least one of gelatin, hydroxyethyl cellulose, methyl cellulose, xanthan gum, β-cyclodextrin and sodium carboxymethyl cellulose, such as a combination of hydroxyethyl cellulose and methyl cellulose, a combination of xanthan gum and β-cyclodextrin, etc. The heat-resistant layer is prepared from a coating slurry. By using a stabilizer, the performance of the coating slurry can be made more stable, which is beneficial to improving the comprehensive performance of the heat-resistant layer.
[0078] In some embodiments, the coating slurry further includes a wetting agent, the mass of which is 0.2% to 2% of the mass of the inorganic material, such as 0.2%, 0.5%, 0.8%, 1%, 1.5%, 2%, etc. At least one of the sodium dodecyl sulfate, fatty alcohol, sodium butyl naphthalene sulfonate and nonylphenol polyoxyethylene ether. The present invention uses a suitable amount of wetting agent in combination with other components to improve the adhesion of the inorganic material and the bonding material to the base film, so that the bonding performance of the heat-resistant coating is better.
[0079] According to another aspect of the present invention, the present invention also relates to a secondary battery comprising the battery separator as described above.
[0080] The battery prepared by the battery separator of the present invention has excellent cycle life and safety performance.
[0081] The following is further explained in conjunction with specific embodiments and comparative examples.
[0082] It should be noted that the “parts” of raw materials involved in each example are based on mass parts.
[0083] Example 1
[0084] A method for preparing a binder for a battery separator comprises the following steps:
[0085] (1) Add 2.78 parts of PEI (EPOMIN, polyethyleneimine, molecular weight 100,000, solid content 36%) and 12.22 parts of deionized water to a container with a stirrer, keep stirring and disperse at 60°C for 40 minutes, and introduce nitrogen into the container to remove oxygen for 30 minutes.
[0086] (2) 0.55 parts of acrylonitrile (McLean, molecular weight 53) was added dropwise into the container of step (1) by a peristaltic pump, and the reaction was carried out for 12 hours. The conversion rate was controlled at 91%, and the residual acrylonitrile monomer was removed by reduced pressure rotation to obtain a binder with a solid content of 10%.
[0087] A method for preparing a battery separator comprises the following steps:
[0088] Mix 200 parts of aluminum oxide and 400 parts of deionized water, stir at high speed for 40 minutes, then add 1.5 parts of methyl cellulose and stir at high speed for 60 minutes; then add 12 parts of binder, evacuate to -0.7MPa, and stir at high speed for 60 minutes; then add 1 part of sodium dodecyl sulfate and stir at low speed for 30 minutes to obtain a coating slurry; use micro-gravure technology to coat the above coating slurry on a PE base film with a thickness of 7μm (manufacturer: Enjie), and after baking and winding, a battery separator with a heat-resistant layer with a thickness of 2μm is obtained.
[0089] Example 2
[0090] A method for preparing a binder for a battery separator, which differs from Example 1 in that the molecular weight of PEI is 10,000.
[0091] A method for preparing a battery separator, which differs from Example 1 in that the binder in this example is used.
[0092] Example 3
[0093] A method for preparing a binder for a battery separator, which differs from Example 1 in that the molecular weight of PEI is 300,000.
[0094] Example 4
[0095] A method for preparing a binder for a battery separator, which differs from Example 1 in that: the amount of acrylonitrile is 0.33 parts.
[0096] A method for preparing a battery separator, which differs from Example 1 in that the binder in this example is used.
[0097] Example 5
[0098] A method for preparing a binder for a battery separator, which differs from Example 1 in that: the amount of acrylonitrile is 0.88 parts.
[0099] A method for preparing a battery separator, which differs from Example 1 in that the binder in this example is used.
[0100] Example 6
[0101] A method for preparing a binder for battery separators, which differs from Example 1 in that 10% PEI is amidated with lithium acrylic acid.
[0102] The invention discloses a method for preparing 10% PEI with lithium acrylic acid amidated, comprising: dissolving 0.11 parts of lithium hydroxide in an appropriate amount of deionized water, and restoring the room temperature; adding 0.11 parts of acrylic acid into a beaker and placing the beaker in ice water for ice water bath, and adding the lithium hydroxide solution dropwise into the beaker to form lithium acrylic acid with a solid content of 10%; adding 2.77 parts of PEI (Japan Catalyst EPOMIN, polyethyleneimine, molecular weight 10W, solid content 36%) and an appropriate amount of deionized water into a container with a stirrer, and stirring and dispersing the mixture at 60°C with heat preservation, introducing nitrogen into the container to remove oxygen for 30 minutes, and adding lithium acrylic acid dropwise into the container through a peristaltic pump, reacting for 12 hours, controlling the conversion rate at 91%, and removing the residual monomers through reduced pressure rotation to obtain a binder with a solid content of 10%.
[0103] A method for preparing a battery separator, which differs from Example 1 in that the binder in this example is used.
[0104] Example 7
[0105] A method for preparing a binder for a battery separator, which differs from Example 6 in that: acrylonitrile is 1.1 parts,
[0106] A method for preparing a battery separator, which differs from Example 1 in that the binder in this example is used.
[0107] Example 8
[0108] A method for preparing a binder for a battery separator comprises the following steps:
[0109] (1) Add 2.78 parts of PEI (EPOMIN, polyethyleneimine, molecular weight 100,000, solid content 36%) and 19 parts of deionized water to a container with a stirrer, keep stirring and disperse at 70°C for 60 minutes, and introduce nitrogen into the container to remove oxygen for 20 minutes.
[0110] (2) 0.55 parts of crotononitrile (McLean) was added dropwise into the container of step (1) by a peristaltic pump, and the reaction was carried out for 15 hours. The conversion rate was controlled at 92%, and the residual acrylonitrile monomer was removed by reduced pressure rotation to obtain a binder with a solid content of 10%.
[0111] A method for preparing a battery separator, which differs from Example 1 in that the binder in this example is used.
[0112] Example 9
[0113] A method for preparing a binder for a battery separator comprises the following steps:
[0114] (1) Add 2.78 parts of PEI (EPOMIN, polyethyleneimine, molecular weight 100,000, solid content 36%) and 19 parts of deionized water into a container with a stirrer, stir and disperse at 50°C for 40 minutes, and introduce nitrogen into the container to remove oxygen for 40 minutes.
[0115] (2) 0.26 parts of crotononitrile and 0.26 parts of acrylonitrile (McLean) were added dropwise into the container of step (1) by a peristaltic pump, and the reaction was carried out for 10 hours. The conversion rate was controlled at 91%, and the residual acrylonitrile monomer was removed by reduced pressure rotation to obtain a binder with a solid content of 10%.
[0116] A method for preparing a battery separator, which differs from Example 1 in that the binder in this example is used.
[0117] Comparative Example 1
[0118] A method for preparing a battery separator, which differs from Example 1 in that the adhesive is polyethyleneimine.
[0119] Comparative Example 2
[0120] A method for preparing a binder for a battery separator, which differs from Example 1 in that the molecular weight of PEI is 0.1w.
[0121] A method for preparing a battery separator, which differs from Example 1 in that the binder in this comparative example is used.
[0122] Comparative Example 3
[0123] A method for preparing a binder for a battery separator, which differs from Example 1 in that the molecular weight of PEI is 500,000.
[0124] A method for preparing a battery separator, which differs from Example 1 in that the binder in this comparative example is used.
[0125] Comparative Example 4
[0126] A method for preparing a binder for a battery separator, which differs from Example 1 in that: the amount of acrylonitrile is 1.1 parts.
[0127] A method for preparing a battery separator, which differs from Example 1 in that the binder in this comparative example is used.
[0128] Comparative Example 5
[0129] A method for preparing a binder for a battery separator, which differs from Example 1 in that: the amount of acrylonitrile is 0.11 parts.
[0130] A method for preparing a battery separator, which differs from Example 1 in that the binder in this comparative example is used.
[0131] Comparative Example 6
[0132] A method for preparing a binder for a battery separator, which differs from Example 1 in that the binder is polyacrylate.
[0133] A method for preparing a battery separator, which differs from Example 1 in that the binder in this comparative example is used.
[0134] Comparative Example 7
[0135] A method for preparing a binder for a battery separator, which differs from Example 1 in that the binder is polyacrylonitrile.
[0136] A method for preparing a battery separator, which differs from Example 1 in that the binder in this comparative example is used.
[0137] Experimental example
[0138] The battery separators prepared in the embodiments and comparative examples were subjected to the following performance tests.
[0139] (1) Electrolyte swelling test
[0140] Dry the adhesive, weigh 1g of the film, and soak it in a 60℃ electrolyte. The electrolyte is a 1mol / L LiPF6 solution, and the solvents are EC, EMC and DEC in a volume ratio of 3:5:2. After 24 hours, take out the glue block, wipe it clean, and then weigh it. Soak it for 10 consecutive days.
[0141] Swelling ratio = (m-m0) / m0×100%, m is the test mass after swelling, and m0 is the initial mass.
[0142] (2) Change in electrolyte color
[0143] Add 1000 ppm of water and 1 g of binder to 10 g of electrolyte, keep the mixture in a vacuum oven at 60°C for 72 h, and observe the color change of the electrolyte.
[0144] (3) Adhesion performance test
[0145] The adhesion between the battery separator and the positive electrode sheet was tested under the conditions of 3MPa, 5min, and 90°C. The positive electrode material layer of the positive electrode sheet included lithium manganese oxide, PVDF, and SP. The mass ratio was lithium manganese oxide: PVDF: SP = 96:2:2.
[0146] (4) Ionic conductivity performance test
[0147] In an argon glove box, the battery membrane was made into a 2016 button battery, and an appropriate amount of electrolyte was added (1 mol / L LiPF6 solution, the solvents were EC, EMC and DE, CEC:EMC:DEC=3:5:2 (volume ratio)). The AC impedance test in the electrochemical workstation showed that σ=L / (Rb×A), where σ is the ionic conductivity (S / cm); L is the thickness of the membrane (cm); Rb is the intrinsic resistance of the membrane (Ω); A is the effective area (cm 2 ).
[0148] (5) Battery performance test
[0149] The battery separator, positive electrode sheet, negative electrode sheet and electrolyte are assembled into a monolithic battery, wherein the positive electrode material layer of the positive electrode sheet includes lithium manganese oxide, PVDF and SP, and lithium manganese oxide: PVDF: SP = 96:2:2; the negative electrode material layer of the negative electrode sheet is graphite, SP, CMC and SBR, and graphite: SP: CMC: SBR = 96:0.7:1.3:2; the electrolyte is a 1 mol / L LiPF6 solution, and the solvents are EC, EMC and DE, and by volume ratio, EC:EMC:DEC = 3:5:2.
[0150] The two assembled monolithic batteries were subjected to cycle tests. The specific test method was as follows: a 0.5C / 1C charge-discharge cycle test was performed in a constant temperature box at 25°C with a voltage range of 2.75-4.2V.
[0151] Capacity retention rate: The battery is cycled 200 times at 25°C and 0.2C charge and discharge, and the capacity before and after the test cycle is measured. Capacity retention rate = capacity after cycle / capacity before cycle.
[0152] At the same time, the diaphragms of the two assembled monolithic batteries were subjected to ICP testing. The specific testing method was: the two monolithic batteries were immersed in aqua regia, diluted, and then the content of each element was tested.
[0153] The performance test results of the battery are shown in Table 2 below.
[0154] Table 1 Performance test results of adhesive
[0155]
[0156]
[0157] Table 2 Battery performance test
[0158]
[0159] As shown in Table 1, compared with Example 1-3 and Comparative Example 1-3, PEI has good water solubility, and is connected to acrylonitrile with a hydrophobic structure. Under the joint action of the hydrophilic and hydrophobic structures, particles are formed, and the solution becomes clear and light blue and milky white. PEI is dissolved in the electrolyte. By introducing acrylonitrile, PEI is subjected to a Michael addition reaction to obtain a binder, which can change its dissolution state in the electrolyte. Under the joint action of PEI and acrylonitrile, a stable structure is formed and it has a strong electrolyte adsorption capacity.
[0160] In Examples 4-5 and Comparative Examples 4-5, the electrolyte adsorption capacity increases with the increase of the acrylonitrile ratio, which is due to the strong polarity of acrylonitrile and the polarity of the polar electrolyte, and the formation of a granular structure with the function of locking the electrolyte. However, as the acrylonitrile content increases, the hydrophobicity of the polymer increases, resulting in its inability to disperse in water and precipitation.
[0161] Since the alkalinity of PEI itself is too strong, it is not conducive to the stability of the slurry. Therefore, by introducing acrylonitrile or acrylonitrile and lithium acrylate, the alkalinity of PEI can be reduced and the stability of the slurry can be improved. Comparing Examples 6-7 and Comparative Example 4, it can be seen that by adding lithium acrylate to PEI, the hydrophilicity of the PEI molecular chain is improved, and the Michael addition ratio of acrylonitrile to PEI is increased. It can be seen from Examples 8-9 that increasing the number of carbon atoms in the acrylonitrile monomer enhances the overall hydrophobicity of the binder, which has a certain negative impact on the adhesion, electrolyte swelling, HF acid capture and Mn ion adsorption.
[0162] Adding a small amount of water to the electrolyte causes the lithium hexafluorophosphate in the electrolyte to hydrolyze, forming highly corrosive hydrofluoric acid, making the electrolyte appear yellow and turbid. High temperature can accelerate this process. In Examples 1-9 and Comparative Examples 1 and 3, the electrolyte remains a clear liquid at high temperatures, showing that the primary and secondary amine groups have good HF adsorption effects, indicating that amine compounds can combine with the hydrofluoric acid already present in the electrolyte to form fluoroammonium salts, thereby achieving the purpose of removing free hydrofluoric acid. At the same time, its Lewis base properties enable it to stabilize lithium hexafluorophosphate and inhibit its hydrolysis. Comparative Example 2 shows that when the PEI molecular weight is low, the amine content is low, and the adsorption effect on HF is small; while Comparative Examples 5 and 6 cannot adsorb HF due to their own structures, resulting in the electrolyte appearing yellow.
[0163] As shown in Table 2, the adhesive of the present invention has good bonding performance, can reduce the dissolution of transition metals during the cycle, and improve the capacity retention rate of the battery. Specifically, the introduction of cyano groups can further improve the bonding effect of PEI binder and cause the strong polarity of cyano groups, which is helpful for ion conduction. 2+ Concentration detection shows that the binder obtained in each embodiment of the present invention can make Mn 2+ The concentration of HF is significantly reduced. This is because the amino structure in PEI can absorb the HF content, thereby curbing the corrosion of HF on the positive electrode material and reducing the transition metal Mn 2+ Dissolution during the cycle and reduction on the negative electrode surface form dendrites, thereby improving the cycle life and safety performance of lithium-ion batteries.
[0164] In summary, the binder obtained by the method of the present invention is applied to battery separators, which can ensure high swelling in the electrolyte, have a high bonding effect on the positive and negative electrode sheets, and can also remove HF formed by the oxidative decomposition reaction caused by trace water in the electrolyte during the circulation process, reduce the dissolution of transition metals in the circulation process of the positive electrode material, and further improve the cycle life and safety performance of lithium-ion batteries.
[0165] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A battery separator adhesive, characterized in that: The adhesive for the battery separator comprises an adhesive material, the molecular structure of which comprises a first structure and a second structure; the first structure comprises a polymer main chain structure containing a first functional group, the first functional group comprises an amine group, or an amine group and an amide group; the second structure comprises a carbon chain containing a cyano group; the group to which the nitrogen atoms in part of the first functional group are connected is the second structure.
2. The adhesive for battery separator according to claim 1, characterized in that: Contains at least one of the following features (1) to (3): (1) The first structure is derived from an amine-containing polymer and / or an amine- and amide-containing polymer; (2) the molar ratio of the first functional group to the cyano group is 10:3 to 8; (3) The molar ratio of the amide group to the first functional group is less than or equal to 20%.
3. The adhesive for battery separator according to claim 2, characterized in that: Contains at least one of the following features (1) to (4): (1) The amine-containing polymer contains primary amine groups, secondary amine groups and tertiary amine groups. Relative to the total amount of amine groups in the amine-containing polymer, the molar ratio N1 of the primary amine groups is 20% to 30%, the molar ratio N2 of the secondary amine groups is 40% to 60%, the molar ratio N3 of the tertiary amine groups is 20% to 30%, and N1+N2+N3=100%; (2) the amine-containing polymer comprises polyethyleneimine; (3) The weight average molecular weight of the amine-containing polymer is 10,000 to 300,000 g / mol.
4. The battery separator binder according to any one of claims 1 to 3, characterized in that Contains at least one of the following features (1) to (2): (1) The number of carbon atoms in the carbon chain containing a cyano group is 3 to 8; (2) The carbon chain containing a cyano group is derived from an olefin nitrile monomer.
5. The adhesive for battery separator according to claim 1, characterized in that: Contains at least one of the following features (1) to (3): (1) The swelling rate of the bonding material in the electrolyte is 100% to 400%; (2) The D50 particle size of the bonding material is 0.01 to 0.25 μm; (3) The battery separator binder further comprises water, and the solid content of the battery separator binder is 5% to 25%.
6. The method for preparing a binder for a battery separator according to any one of claims 1 to 5, characterized in that: The following steps are involved: A mixture of a polymer material and water is heat-treated to obtain a first system, wherein the polymer material includes an amine-containing polymer and / or an amine- and amide-containing polymer; under protective gas conditions, the first system is mixed and reacted with olefin nitrile monomers, and then the residual olefin nitrile monomers are removed to obtain a binder for a battery separator.
7. The method for preparing a binder for a battery separator according to claim 6, characterized in that: Contains at least one of the following features (1) to (10): (1) The amine-containing polymer contains primary amine groups, secondary amine groups and tertiary amine groups. Relative to the total amount of amine groups in the amine-containing polymer, the molar ratio N1 of the primary amine groups is 20% to 30%, the molar ratio N2 of the secondary amine groups is 40% to 60%, the molar ratio N3 of the tertiary amine groups is 20% to 30%, and N1+N2+N3=100%; (2) the amine-containing polymer comprises polyethyleneimine; (3) The weight average molecular weight of the amine-containing polymer is 10,000 to 300,000 g / mol; (4) The molar ratio of the structural unit of the polymer material to the olefin nitrile monomer is 10:3-8; (5) The temperature of the heat treatment is 50 to 70° C., and the time of the heat treatment is 0.5 to 1 h; (6) The mixing specifically comprises: dropping the olefin nitrile monomer into the first system; (7) The reaction time is 10 to 15 hours; (8) The method for preparing the polymer containing amino groups and amide groups specifically comprises: mixing a carboxyl-containing monomer and a hydroxide of M, wherein M is selected from lithium or sodium, to obtain a salt of the carboxyl-containing monomer; hot mixing and reacting the salt of the carboxyl-containing monomer with water and a first polymer containing amino groups, and removing the residual carboxyl-containing monomer to obtain a polymer containing amino groups and amide groups; the molar ratio of the structural units of the carboxyl-containing monomer, the hydroxide of M and the first polymer containing amino groups is 1:1:4-10; (9) During the preparation of the polymer containing amino groups and amide groups, the temperature of hot mixing is 50 to 65° C. and the reaction time is 10 to 15 hours; (10) The solid content of the polymer containing amino groups and amide groups is 8% to 12%.
8. A battery separator, characterized in that: It comprises a base film and a heat-resistant layer located on at least one surface of the base film; the heat-resistant layer comprises an inorganic material and the adhesive material of the adhesive for battery separator according to any one of claims 1 to 5.
9. The battery separator according to claim 8, characterized in that: The invention comprises at least one of the following features (1) to (6): (1) The particle size D50 of the inorganic material is 0.1 to 1.2 μm, and the particle size D50 of the bonding material is 0.01 to 0.25 μm; the mass ratio of the inorganic material to the bonding material is 10:1 to 100:1; (2) The thickness of the base film is 5 to 16 μm, and the thickness of the heat-resistant layer is 1 to 4 μm; (3) The inorganic material includes at least one of aluminum oxide, silicon oxide, boehmite, titanium oxide, zirconium oxide and aluminum hydroxide; (4) The heat-resistant layer further comprises a stabilizer, the mass of which is 0.2% to 2% of the mass of the inorganic material; the stabilizer comprises at least one of gelatin, hydroxyethyl cellulose, methyl cellulose, xanthan gum, β-cyclodextrin and sodium carboxymethyl cellulose; (5) The heat-resistant layer is obtained by coating a coating slurry on the surface of the base film and then drying it; the coating slurry comprises the inorganic material, a binder for a battery separator, a stabilizer and a wetting agent; (6) The mass of the wetting agent is 0.2% to 2% of the mass of the inorganic material; the wetting agent includes at least one of sodium dodecyl sulfate, fatty alcohol, sodium butylnaphthalenesulfonate and nonylphenol polyoxyethylene ether.
10. A secondary battery, characterized in that: A battery separator comprising the battery separator according to claim 8 or 9.
Citation Information
Cited By
Negative electrode binder as well as preparation method and application thereof
CN120955138A