Electrochemical method for separating yttrium and neodymium with similar properties

By co-depositing Y(III) and Nd(III) with Zn(II) in a eutectic molten salt, determining the separation potential and performing constant-potential electrolysis, an Nd-Zn alloy is formed, which solves the problem of separation of yttrium and neodymium and achieves low-cost , efficient separation of rare earth elements.

CN118756255AInactive Publication Date: 2024-10-11NANHUA UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411013649.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively separate yttrium and neodymium elements with similar electrochemical properties. The traditional method is complex and costly. The existing molten salt electrolysis method mainly targets rare earth elements with huge differences in electrochemical properties, and cannot effectively separate elements with similar electrochemical properties.

Method used

By preparing a eutectic molten salt, co-depositing Y(III) and Nd(III) with Zn(II), determining the separation potential, and using constant potential electrolysis to make Nd(III) and Zn form a Zn-rich phase Nd-Zn alloy. Achieve selective separation of yttrium and neodymium.

Benefits of technology

The selective separation of yttrium and neodymium has been achieved with simple process flow, low waste volume, cheap materials and low cost, and can effectively separate rare earth elements with similar electrochemical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756255A_ABST
    Figure CN118756255A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of chemical engineering and separation, and particularly relates to an electrochemical method for separating yttrium and neodymium with similar properties, which comprises the following steps: adding YCl3 and NdCl3 into eutectic molten salt, then inserting an electrode assembly into the eutectic molten salt containing Y (III) and Nd (III), connecting an electrochemical workstation, and measuring the reduction potentials of Y (III) and Nd (III) by adopting an electrochemical method; znCl2 is added into the eutectic molten salt containing Y (III) and Nd (III) for codeposition, the electrochemical properties and the reduction potential of Zn-Y and Zn-Nd alloys are measured, and the separation potential is determined; and carrying out constant potential electrolysis by using reduction potential difference, preferentially carrying out codeposition on Nd (III) and Zn (II) to form a Zn-Nd intermetallic compound which is deposited at the bottom, and retaining yttrium in molten salt. The method has the advantages of simple process flow, small waste amount, low material price and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical engineering and separation technology, and in particular relates to an electrochemical method for separating yttrium and neodymium with similar properties. Background Art

[0002] Nuclear energy is widely used around the world, and nuclear reactions produce a large number of fission products. The presence of rare earth elements in fission products will hinder the continued occurrence of nuclear reactions and cause great difficulties in the subsequent treatment of spent fuel. Yttrium and neodymium are two representative rare earth elements, which are present in high levels in fission products. In addition, neodymium plays an important role in aerospace, materials, rare earth industry and other fields, while yttrium can be used in superconductors, materials, medical and other fields. However, due to the similar physical, chemical and electrochemical properties of yttrium and neodymium, their separation is extremely difficult. Therefore, it is very important to choose a suitable method to treat yttrium and neodymium.

[0003] Traditional separation methods mainly utilize the differences in the chemical properties of rare earth ions in aqueous solutions, and use extractants for solvent extraction and separation, such as extraction chromatography and solution extraction. For example, patent CN202111290216.2 discloses an extractant and a method for separating yttrium from other heavy rare earth elements, and patent CN202210354862.9 discloses an extractant for extracting and separating neodymium (III) and its preparation method. The separation process is complicated and lengthy, the amount of waste generated is large, the price of the materials used is high, and the economy is low. Molten salt electrolysis has the advantages of high temperature resistance, radiation resistance, and simple process flow, and is often used to prepare various metals and alloys, and has important applications in the separation of metals. However, the existing technologies for separating rare earth elements by molten salt electrolysis are mainly aimed at rare earth elements with large deposition potential differences, that is, the separation between variable valence rare earths and constant valence rare earths. For example, patent CN202211606548.1 discloses a method for separating Yb and Lu elements and patent CN201110336585.0 discloses a method for separating Gd and Eu by molten salt electrolysis. Yb and Eu belong to variable valence rare earths. Yb(III) and Eu(III) will generate Yb(II) and Eu(II) during the electrolysis process. The redox potential of Yb(II) / Yb(0) and Eu(II) / Eu(0) is much smaller than that of Lu(III) / Lu(0) and Gd(III) / Gd(0). The huge difference in potential difference between them is more conducive to electrochemical separation. Therefore, it is urgent to develop a molten salt electrolysis technology that can separate rare earth elements with similar electrochemical properties.

[0004] At present, the separation method of rare earth elements in molten salt electrolysis usually relies on the huge difference in electrochemical properties between rare earth elements. For example, a method for separating ytterbium and lutetium elements disclosed in patent CN202211606548.1 uses the huge difference in electrochemical behavior between ytterbium and lutetium to directly electrolyze and separate them using inert electrodes. However, this method cannot effectively separate elements with similar electrochemical properties. The gadolinium and europium separated by molten salt electrolysis disclosed in patent CN201110336585.0 also have great differences in electrochemical behavior. The separation effect of elements with similar electrochemical properties is still unknown.

[0005] The existing patented technology of molten salt electrolysis can only separate rare earth elements with greatly different electrochemical properties, but lacks effective separation means for rare earth elements with similar electrochemical properties. Summary of the invention

[0006] In view of the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide an electrochemical method for separating yttrium and neodymium with similar properties. The present invention is based on the problem that the electrochemical properties of yttrium and neodymium are very similar, the reduction potentials of yttrium and neodymium are similar, and they cannot be directly separated by an electrochemical method. In the process of co-deposition of Y(III) and Nd(III) with Zn(II), Nb(III) is preferentially co-reduced with Zn(II) over Y(III), the separation potential is determined, constant potential electrolysis is performed at the separation potential, Nd preferentially forms a Zn-rich Nd-Zn alloy with Zn, and the selective separation of yttrium and neodymium is achieved.

[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0008] An electrochemical method for separating yttrium and neodymium of similar properties comprises the following steps:

[0009] preparing a eutectic molten salt, adding YCl3 and NdCl3 into the eutectic molten salt to obtain a eutectic molten salt containing Y(III) and Nd(III);

[0010] The electrode assembly was inserted into the eutectic molten salt containing Y(III) and Nd(III) and connected to the electrochemical workstation. In order to reduce the influence of impurities on the experiment, the electrode assembly was placed at -2.3 V vs Ag / Ag + The reduction potentials of Y(III) and Nd(III) on the inert electrode were determined by electrochemical method. It was found that the reduction potentials of yttrium and neodymium could not be distinguished, indicating that the electrochemical properties of yttrium and neodymium are very similar.

[0011] ZnCl2 was added to LiCl-KCl molten salt containing Y(III) and Nd(III) for co-deposition. The electrochemical properties of Zn-Y and Zn-Nd alloys and the reduction potentials of Y(III) and Nd(III) during co-deposition were determined. The effect of the coexistence of Y(III) and Nd(III) on alloy formation was analyzed by electrochemical technology, indicating that Nd forms intermetallic compounds with Zn preferentially over Y, and the separation potential was determined.

[0012] The reduction potential difference between the Zn-Y and Zn-Nd intermetallic compounds in the zinc-rich phase is used for electrolysis. Nd(III) preferentially co-precipitates with Zn(II) over Y(III) to form Zn-Nd intermetallic compounds deposited at the bottom, while yttrium is retained in the molten salt.

[0013] After the electrolysis is completed, the molten salt is cooled to room temperature, ultrapure water is used and an ultrasonic cleaner is used to assist in dissolving the molten salt, the solution is separated from the alloy precipitate, and the precipitate is placed in a 90°C oven for drying to obtain a neodymium-rich neodymium-zinc alloy.

[0014] In a preferred embodiment of the present invention, the molar ratio of YCl3 and NdCl3 added to the eutectic molten salt is 1:0.45-3, and the molar ratio of YCl3 and NdCl3 will affect the size of the separation factor. Because Nd is electrolyzed, the higher the content of NdCl3, the greater the separation factor after separation.

[0015] In a preferred embodiment of the present invention, the molar ratio of ZnCl2 added to the LiCl-KCl molten salt containing Y(III) and Nd(III) is 0.18-4:1:0.45-3.

[0016] In a preferred embodiment of the present invention, the eutectic molten salt is one of LiCl-KCl, NaCl-KCl, and NaCl-CaCl2 eutectic molten salts.

[0017] In a preferred embodiment of the present invention, the preparation method of the eutectic molten salt is: mixing two salts in the raw materials in a certain proportion, heating and melting, to obtain a eutectic molten salt. When the two salts are mixed in a certain proportion, the melting point of the mixed eutectic molten salt is the lowest.

[0018] In a preferred embodiment of the present invention, in the LiCl-KCl eutectic molten salt, the mass ratio of KCl to LiCl is 45:38, in the NaCl-KCl eutectic molten salt, the mass ratio of NaCl to KCl is 37:46, and in the NaCl-CaCl2 eutectic molten salt, the mass ratio of NaCl to CaCl2 is 28:56.

[0019] In a preferred embodiment of the present invention, the heating temperature is 500-750° C. and the holding time is 2-5 hours.

[0020] In a preferred embodiment of the present invention, the electrolysis method is constant potential electrolysis.

[0021] In a preferred embodiment of the present invention, the electrochemical method is one of cyclic voltammetry, square wave voltammetry, and chronopotentiometry.

[0022] In a preferred embodiment of the present invention, the electrochemical component consists of a reference electrode, an auxiliary electrode and a working electrode, the working electrode is silver / silver chloride, the auxiliary electrode is a graphite rod, and the working electrode is a tungsten wire.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The present invention is based on the problem that yttrium and neodymium have very similar electrochemical properties and similar reduction potentials, and cannot be directly separated by electrochemical methods. In the process of co-deposition of Y(III) and Nd(III) with Zn(II), Nd(III) preferentially undergoes co-reduction with Zn(II) rather than Y(III), and a separation potential is determined. Constant potential electrolysis is performed at the separation potential, and Nd preferentially forms a Zn-rich Nd-Zn alloy with Zn to achieve selective separation of yttrium and neodymium.

[0025] 2. The electrochemical method for separating yttrium and neodymium with similar properties provided by the present invention has the advantages of simple process flow, small amount of waste, cheap material price and low cost. It can separate yttrium and neodymium, rare earth elements with similar electrochemical properties, extract neodymium in the form of Nd-Zn alloy from the molten salt where Y(III) and Nd(III) coexist, while yttrium is retained in the molten salt, thereby realizing the selective separation of yttrium and neodymium. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A schematic diagram of an electrochemical device for separating yttrium and neodymium of similar properties according to the present invention;

[0027] Figure 2 500℃LiCl-KCl-YCl3(1.37×10 -4 mol cm -3 )-NdCl3(6.13×10 -5 mol cm -3 )Square wave voltammetry curve on a tungsten electrode in molten salt;

[0028] Figure 3 500℃LiCl-KCl-YCl3(1.37×10 -4 mol cm -3 )-ZnCl2(2.5×10 -5 mol cm -3)、LiCl-KCl-NdCl3(6.13×10 -5 mol cm -3 )-ZnCl2(2.5×10 -5 mol cm -3 ) and LiCl-KCl-YCl3(1.37×10 -4 mol cm -3 )-NdCl3(6.13×10 -5 mol cm -3 )-ZnCl2(2.5×10 -5 mol cm -3 )Square wave voltammetry curve on a tungsten electrode in molten salt;

[0029] Figure 4 500℃LiCl-KCl-YCl3(1.37×10 -4 mol cm -3 )-NdCl3(6.13×10 -5 mol cm -3 )-ZnCl2(2.75×10 -4 mol cm -3 ) XRD pattern of the alloy obtained by electrolytic separation of yttrium and neodymium in molten salt, with the inset being a photograph of the alloy product. DETAILED DESCRIPTION

[0030] The following is a detailed description of the technical solutions in the embodiments of the present invention in combination with the preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] It should be noted that all professional terms used in the present invention are only for the purpose of describing specific implementation cases and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.

[0032] Example 1

[0033] A method for separating yttrium and neodymium by molten salt electrolysis comprises the following steps:

[0034] (1) Weigh 45 g of anhydrous KCl and 38 g of anhydrous LiCl and mix them evenly in a corundum crucible, place them in a 90° C. oven to dry for 12 hours to remove water, place the dried corundum crucible containing the mixed salt in a resistance furnace in a glove box, heat them to 500° C. in the resistance furnace and keep them warm for 2 hours to stabilize the molten salt system, thereby obtaining a low melting point LiCl-KCl eutectic salt.

[0035] (2) Insert the reference electrode silver / silver chloride, the auxiliary electrode graphite rod, and the working electrode tungsten wire into the low melting point LiCl-KCl eutectic salt prepared in step (1), and connect the reference electrode RE, auxiliary electrode CE, and working electrode WE wires on the electrochemical workstation to form a three-electrode system, as shown in the schematic diagram. Figure 1 shown.

[0036] (3) Cyclic voltammetry was used to perform electrochemical tests to determine the deposition potential of impurities in the molten salt, and pre-electrolysis was performed at a potential of -2.3 V vsAg / AgCl to remove residual water and other impurities in the molten salt, thereby obtaining a pure LiCl-KCl eutectic molten salt.

[0037] (4) Weigh 1.4 g of anhydrous YCl3 and 0.8 g of anhydrous NdCl3, add them into the LiCl-KCl eutectic salt respectively, and stir them to fully dissolve them to obtain LiCl-KCl-YCl3, LiCl-KCl-NdCl3 and LiCl-KCl-YCl3-NdCl3 molten salt systems.

[0038] (5) The electrochemical behavior and deposition potential of Y(III) and Nd(III) on the W electrode were analyzed by cyclic voltammetry, and electrochemical analysis was performed on the W electrode in the LiCl-KCl-YCl3-NdCl3 molten salt system to determine the feasibility of separation when Y(III) and Nd(III) coexisted.

[0039] (6) 0.2 g ZnCl2 was added to the LiCl-KCl-YCl3 and LiCl-KCl-NdCl3 molten salt systems, respectively. The electrochemical properties of Zn-Y and Zn-Nd alloys and the reduction potentials of Y(III) and Nd(III) during the co-deposition process were determined to determine the feasibility of separation in the presence of Zn(II). It was found that the deposition potential difference between the Zn-rich Zn-Y and Zn-Nd alloys was 0.09 V. According to the Nernst equation, theoretically 98.3% of Nd was separated before Y deposition, proving that the presence of Zn(II) can promote the separation of Y(III) and Nd(III).

[0040] (7) 0.2 g ZnCl2 was added to the LiCl-KCl-YCl3-NdCl3 molten salt system, and the electrochemical data of the co-deposition process when Y(III) and Nd(III) coexisted were determined by electrochemical technology, and the reduction potentials of the Zn-Y and Zn-Nd alloys obtained in step (6) were compared and analyzed.

[0041] (8) Based on the previous electrochemical experimental data, 1.4 g YCl3, 0.8 g NdCl3 and 2.2 g ZnCl2 were added to the LiCl-KCl molten salt and then electrolyzed at a constant potential on a W electrode to separate Y(III) and Nd(III). The separation potential was -1.33 V vsAg / Ag + The electrolysis time was 5 hours. Since the alloy formed during the electrolysis process had poor adhesion on the W electrode, the electrolysis product was deposited at the bottom of the crucible.

[0042] (9) After the electrolysis is completed, the molten salt is cooled to room temperature and washed with ultrapure water to separate the product from the molten salt. At the same time, the product is washed with an ultrasonic cleaner to obtain a salt-free electrolysis product. Subsequently, the electrolysis product is placed in a 90° C. oven and dried to obtain a Nd-Zn alloy with a high neodymium content.

[0043] Example 2

[0044] A method for separating yttrium and neodymium by molten salt electrolysis comprises the following steps:

[0045] (1) 37 g of anhydrous NaCl and 46 g of anhydrous KCl were weighed and placed in a corundum crucible and mixed evenly, and then placed in a 90° C. oven for drying for 12 hours to remove water. The dried corundum crucible containing the mixed salt was placed in a resistance furnace in a glove box and heated to 750° C. in the resistance furnace for 5 hours to stabilize the molten salt system, thereby obtaining a low melting point NaCl-KCl eutectic salt.

[0046] (2) Insert the reference electrode silver / silver chloride, the auxiliary electrode graphite rod, and the working electrode tungsten wire into the low melting point NaCl-KCl eutectic salt prepared in step (1), and connect the reference electrode RE, auxiliary electrode CE, and working electrode WE wires on the electrochemical workstation to form a three-electrode system, as shown in the schematic diagram. Figure 1 shown.

[0047] (3) Cyclic voltammetry was used to perform electrochemical tests to determine the deposition potential of impurities in the molten salt, and pre-electrolysis was performed at a potential of -2.1 V vsAg / AgCl to remove residual water and other impurities in the molten salt, thereby obtaining a pure NaCl-KCl eutectic molten salt.

[0048] (4) Weigh 1.4 g of anhydrous YCl3 and 0.8 g of anhydrous NdCl3, add them into the NaCl-KCl eutectic salt respectively, and stir them to fully dissolve them to obtain NaCl-KCl-YCl3, NaCl-KCl-NdCl3 and NaCl-KCl-YCl3-NdCl3 molten salt systems.

[0049] (5) The electrochemical behavior and deposition potential of Y(III) and Nd(III) on the W electrode were analyzed by square wave voltammetry. Electrochemical analysis was also performed on the W electrode in the NaCl-KCl-YCl3-NdCl3 molten salt system to determine the feasibility of separation when Y(III) and Nd(III) coexisted.

[0050] (6) 0.2 g ZnCl2 was added to the NaCl-KCl-YCl3 and NaCl-KCl-NdCl3 molten salt systems, respectively. The electrochemical properties and reduction potentials of Zn-Y and Zn-Nd alloys during the co-deposition process were determined to determine the feasibility of separation in the presence of Zn(II). The deposition potential difference between the Zn-rich Zn-Y and Zn-Nd alloys was obtained, and the theoretical separation rate of Nd was calculated, demonstrating that the presence of Zn(II) can promote the separation of Y(III) and Nd(III).

[0051] (7) 0.2 g ZnCl2 was added to the NaCl-KCl-YCl3-NdCl3 molten salt system, and the electrochemical data of the co-deposition process when Y(III) and Nd(III) coexisted were determined by electrochemical technology, and the reduction potentials of the Zn-Y and Zn-Nd alloys obtained in step (6) were compared and analyzed.

[0052] (8) Based on the previous electrochemical experimental data, 1.4 g YCl3, 2.5 g NdCl3 and 2.5 g ZnCl2 were added to the NaCl-KCl molten salt and then subjected to constant potential electrolysis on the W electrode to separate Y(III) and Nd(III). Since the alloy formed during the electrolysis process had poor adhesion to the W electrode, the electrolysis products were deposited at the bottom of the crucible.

[0053] (9) After the electrolysis is completed, the molten salt is cooled to room temperature and washed with ultrapure water to separate the product from the molten salt. At the same time, the product is washed with an ultrasonic cleaner to obtain a salt-free electrolysis product. Subsequently, the electrolysis product is placed in a 90° C. oven and dried to obtain a Nd-Zn alloy with a high neodymium content.

[0054] Example 3

[0055] A method for separating yttrium and neodymium by molten salt electrolysis comprises the following steps:

[0056] (1) Weigh 28 g of anhydrous NaCl and 56 g of anhydrous CaCl2 in a corundum crucible and mix them evenly. Place the crucible in a 90°C oven and dry for 12 hours to remove water. Place the dried corundum crucible containing the mixed salt in a resistance furnace in a glove box and heat it to 650°C in the resistance furnace for 3 hours to stabilize the molten salt system, thereby obtaining a low melting point NaCl-CaCl2 eutectic salt.

[0057] (2) Insert the reference electrode silver / silver chloride, the auxiliary electrode graphite rod, and the working electrode tungsten wire into the low melting point NaCl-CaCl2 eutectic salt prepared in step (1), and connect the reference electrode RE, auxiliary electrode CE, and working electrode WE wires on the electrochemical workstation to form a three-electrode system, as shown in the schematic diagram. Figure 1 shown.

[0058] (3) Cyclic voltammetry was used to perform electrochemical tests to determine the deposition potential of impurities in the molten salt, and pre-electrolysis was performed at a potential of -2.1 V vsAg / AgCl to remove residual water and other impurities in the molten salt, thereby obtaining a pure NaCl-CaCl2 eutectic molten salt.

[0059] (4) Weigh 1.4 g of anhydrous YCl3 and 0.8 g of anhydrous NdCl3, add them into the NaCl-CaCl2 eutectic salt respectively, and stir them to fully dissolve them to obtain NaCl-CaCl2-YCl3, NaCl-CaCl2-NdCl3 and NaCl-CaCl2-YCl3-NdCl3 molten salt systems.

[0060] (5) The electrochemical behavior and deposition potential of Y(III) and Nd(III) on the W electrode were analyzed by electrochemical methods such as chronopotentiometry. Electrochemical analysis was also performed on the W electrode in the NaCl-CaCl2-YCl3-NdCl3 molten salt system to determine the feasibility of separation when Y(III) and Nd(III) coexisted.

[0061] (6) 0.2 g ZnCl2 was added to the NaCl-CaCl2-YCl3 and NaCl-CaCl2-NdCl3 molten salt systems, respectively. The electrochemical properties and reduction potentials of Zn-Y and Zn-Nd alloys during the co-deposition process were determined to determine the feasibility of separation in the presence of Zn(II). The deposition potential difference between the Zn-rich Zn-Y and Zn-Nd alloys was obtained, and the theoretical separation rate of Nd was calculated, demonstrating that the presence of Zn(II) can promote the separation of Y(III) and Nd(III).

[0062] (7) 0.2 g ZnCl2 was added to the NaCl-CaCl2-YCl3-NdCl3 molten salt system, and the electrochemical data of the co-deposition process when Y(III) and Nd(III) coexisted were determined by electrochemical technology, and the reduction potentials of the Zn-Y and Zn-Nd alloys obtained in step (6) were compared and analyzed.

[0063] (8) Based on the previous electrochemical experimental data, 1.4 g YCl3, 5.37 g NdCl3 and 3.87 g ZnCl2 were added to the NaCl-CaCl2 molten salt and then subjected to constant potential electrolysis on the W electrode to separate Y(III) and Nd(III). Since the alloy formed during the electrolysis process had poor adhesion to the W electrode, the electrolysis products were deposited at the bottom of the crucible.

[0064] (9) After the electrolysis is completed, the molten salt is cooled to room temperature and washed with ultrapure water to separate the product from the molten salt. At the same time, the product is washed with an ultrasonic cleaner to obtain a salt-free electrolysis product. Subsequently, the electrolysis product is placed in a 90° C. oven and dried to obtain a Nd-Zn alloy with a high neodymium content.

[0065] Figure 1 Schematic diagram of the electrochemical device for separating yttrium and neodymium of similar properties according to the present invention. Figure 2 500℃LiCl-KCl-YCl3(1.37×10 -4 mol cm -3 )-NdCl3(6.13×10 -5 mol cm -3 ) Square wave voltammetry curve on a tungsten electrode in molten salt. Figure 2 As shown, the reduction potentials of yttrium and neodymium were found to be indistinguishable, indicating that the electrochemical properties of yttrium and neodymium are very similar.

[0066] The deposition potential and corresponding alloy composition of Y(III), Nd(III) and Zn(II) co-deposited alloys were analyzed, such as Figure 3 shown. Figure 3 The results show that when Y(III) and Nd(III) coexist, only the Zn-rich Nd-Zn alloy is formed, and no Zn-rich Y-Zn alloy deposition signal is observed, indicating that Nd(III) preferentially co-deposits with Zn(II) to form intermetallic compounds over Y(III), and based on this, the separation potential is determined to be -1.33 V vs Ag / Ag. + .

[0067] The product was characterized and analyzed by XRD. The product photos and XRD patterns are shown in Figure 4 As shown, the results show that the product is NdZn 11The contents of Y(III) and Nd(III) in the molten salt were determined by ICP-OES, the contents of Y and Nd in the product were analyzed, and the separation coefficient β was calculated to be 43.37, ultimately achieving selective separation of yttrium and neodymium with similar properties.

[0068] In summary, the present invention is based on the problem that the electrochemical properties of yttrium and neodymium are very similar, the reduction potentials of yttrium and neodymium are similar, and they cannot be separated directly by electrochemical methods. In the process of co-deposition of Y(III) and Nd(III) with Zn(II), Nd(III) is preferentially co-reduced with Zn(II) to form an intermetallic compound over Y(III), the separation potential is determined, constant potential electrolysis is performed at the separation potential, Nd preferentially forms a Zn-rich Nd-Zn alloy with Zn, and the selective separation of yttrium and neodymium is achieved. The process of the present invention is simple, the amount of waste is small, the material price is cheap, and the cost is low.

[0069] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the implementation case, in order to avoid redundancy, the present invention describes a preferred implementation case. Although the preferred embodiments of the present invention have been described, once those skilled in the art know the basic creative concept, they can make additional changes and modifications to these embodiments. Therefore, the attached claims are intended to be interpreted as including the preferred embodiment and all changes and modifications that fall within the scope of the present invention.

[0070] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. An electrochemical method for separating yttrium and neodymium of similar properties, It is characterized in that The following steps are involved: Prepare eutectic molten salt, YCl 3 and NdCl 3 adding into the eutectic molten salt to obtain a eutectic molten salt containing Y(III) and Nd(III); The electrode assembly is inserted into a eutectic molten salt containing Y(III) and Nd(III), connected to an electrochemical workstation, and the deposition potential when Y(III) and Nd(III) coexist is measured by an electrochemical method; Adding ZnCl to the eutectic molten salt containing Y(III) and Nd(III) 2 Conduct codeposition, measure the electrochemical properties and reduction potential of Zn-Y and Zn-Nd alloys during codeposition, and determine the separation potential; By utilizing the reduction potential difference between the zinc-rich Zn-Y and Zn-Nd alloys for electrolysis, Nd(III) preferentially co-precipitates with Zn(II) rather than Y(III) to form a Zn-Nd intermetallic compound deposited at the bottom, while yttrium is retained in the molten salt, thus achieving the separation of yttrium and neodymium.

2. The electrochemical method for separating yttrium and neodymium of similar properties according to claim 1, It is characterized in that Add YCl to the eutectic molten salt 3 and NdCl 3 The molar ratio is 1:0.45~3.

3. The electrochemical method for separating yttrium and neodymium of similar properties according to claim 1, It is characterized in that In the eutectic molten salt containing Y(III) and Nd(III), ZnCl 2 The molar ratio of Y(III) to Nd(III) is 0.18~4:1:0.45~3.

4. The electrochemical method for separating yttrium and neodymium of similar properties according to claim 1, It is characterized in that The eutectic molten salt is LiCl-KCl, NaCl-KCl, NaCl-CaCl 2 One of the eutectic molten salts.

5. The electrochemical method for separating yttrium and neodymium of similar properties according to claim 4, It is characterized in that The preparation method of the eutectic molten salt is as follows: two salts in the raw materials are mixed in proportion, heated and melted, and the eutectic molten salt is obtained.

6. The electrochemical method for separating yttrium and neodymium of similar properties according to claim 5, It is characterized in that In the LiCl-KCl eutectic molten salt, the mass ratio of KCl to LiCl is 45:38, in the NaCl-KCl eutectic molten salt, the mass ratio of NaCl to KCl is 37:46, and in the NaCl-CaCl 2 In the eutectic molten salt, NaCl and CaCl 2 The mass ratio is 28:

56.

7. The electrochemical method for separating yttrium and neodymium of similar nature according to claim 5, It is characterized in that The heating temperature is 500-750°C and the insulation time is 2-5 hours.

8. The electrochemical method for separating yttrium and neodymium of similar properties according to claim 1, It is characterized in that The electrolysis method is constant potential electrolysis.

9. The electrochemical method for separating yttrium and neodymium of similar properties according to claim 1, It is characterized in that The electrochemical method is one of cyclic voltammetry, square wave voltammetry and chronopotentiometry.

10. The electrochemical method for separating yttrium and neodymium of similar properties according to claim 1, It is characterized in that The electrochemical component consists of a reference electrode, an auxiliary electrode and a working electrode.

Citation Information

Patent Citations

  • Method for separating Gd and Eu through fused salt electrolysis

    CN102373490A

  • Extracting agent for extracting and separating neodymium (III) as well as preparation method and application of extracting agent

    CN114853617A

  • Extracting agent and method for separating yttrium from other heavy rare earth elements

    CN116065020A

  • Ytterbium and lutetium element separation method

    CN116240589A