Fluorine-containing polymer, undercoat slurry, secondary battery, and electric device

CN118765291APending Publication Date: 2024-10-11CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280092924.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-11-04
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing technology, the primer slurry has a short process window and poor filterability, resulting in low production efficiency of secondary battery pole pieces, and a dispersant needs to be added to improve processing performance.

Method used

Develop a fluoropolymer, through a combination of structural units derived from specific monomers, to form a polymer for the preparation of base coatings, improve the viscosity and filterability of slurries, reduce reliance on dispersants, and optimize the coating process .

Benefits of technology

It significantly broadens the process window of primer slurry, improves production efficiency and product quality, enhances the stability and bonding performance of the primer, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765291A_ABST
    Figure CN118765291A_ABST
Patent Text Reader

Abstract

The invention provides a fluorine-containing polymer, a prime coat slurry, a secondary battery and an electric device. The fluorine-containing polymer comprises a structural unit derived from a monomer as shown in a formula I and a structural unit derived from a monomer as shown in a formula II, the molar content of the structural unit derived from the monomer as shown in the formula I is 70%-90%, and based on the total mass of the structural units in the fluorine-containing polymer, R1, R2 and R3 are independently selected from one or more of hydrogen, fluorine, chlorine and fluorine-substituted C1-3 alkyl, and R1, R2 and R3 are independently selected from one or more of hydrogen, fluorine, chlorine and fluorine-substituted C1-3 alkyl. R4, R5 and R6 are independently selected from one or more of hydrogen and substituted or unsubstituted C1-5 alkyl groups, and R7 is selected from substituted or unsubstituted C1-9 alkyl groups.
Need to check novelty before this filing date? Find Prior Art

Description

Fluoropolymer, primer slurry, secondary battery, and electrical device Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a fluorine-containing polymer, a primer slurry, a secondary battery, and an electrical device. Background Art

[0002] During the production of secondary battery electrodes, a primer is applied between the current collector and the active material layer to provide electrical conductivity between the active material layer and the current collector, thereby reducing the contact resistance between the two. This primer is typically prepared by applying a primer slurry containing a binder, a conductive agent, and additives to the surface of the current collector. However, existing primer slurries suffer from a short process window, poor filterability, and are prone to precipitation and pipe clogging, severely impacting electrode production efficiency. Therefore, there is an urgent need to develop a polymer that can function as a binder while also ensuring good dispersibility in the slurry to improve its processing performance.

[0003] Summary of the Invention

[0004] The present application is made in view of the above-mentioned problems, and its purpose is to provide a fluoropolymer and a coating containing the fluoropolymer to optimize the process window for coating preparation and improve the production efficiency of the primer layer.

[0005] The first aspect of the present application provides a fluorine-containing polymer, which comprises a structural unit derived from a monomer represented by formula I and a structural unit derived from a monomer represented by formula II, wherein the molar content of the structural unit derived from the monomer represented by formula I is 70% to 90%, based on the total molar number of the structural units in the fluorine-containing polymer.

[0006]

[0007] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine atoms, fluorine-substituted C 1-3 One or more of the alkyl groups, R4, R5, and R6 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 One or more of alkyl, R7 is selected from substituted or unsubstituted C 1-9 alkyl.

[0008] Compared with the polyvinyl difluoride binder commonly used in the prior art, the fluorine-containing polymer provided in the present application reduces the viscosity of the slurry, improves the filterability, and improves the processability of the primer slurry, so that the primer slurry can meet the production requirements of the primer slurry without adding a dispersant, which is beneficial to optimizing the production process of the primer slurry and improving its production quality.

[0009] In any embodiment, R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine, and trifluoromethyl, and R5 and R6 are each independently selected from one or two of hydrogen and methyl.

[0010] In any embodiment, the molar content of the structural unit derived from the monomer represented by formula II is 10% to 30%, based on the total molar number of the structural units in the fluorine-containing polymer.

[0011] Based on the total molar number of structural units of the fluoropolymer, when the molar content of the structural units derived from the monomer represented by Formula II is 10% to 30%, the viscosity of the fluoropolymer is appropriate, which can comprehensively improve the processability and adhesion of the slurry, taking into account the processing performance and performance of the primer layer.

[0012] In any embodiment, the weight average molecular weight of the fluorine-containing polymer is 400,000 to 500,000.

[0013] Fluorine-containing polymers with a weight-average molecular weight of 400,000 to 500,000 have an appropriate viscosity and can comprehensively improve the processability and adhesion of the slurry, while taking into account the processing performance and performance of the primer layer.

[0014] In any embodiment, the monomer represented by formula I is selected from one or more of vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.

[0015] In any embodiment, the monomer represented by formula II is selected from one or more of methyl acrylate, ethyl acrylate, butyl acrylate, isoamyl acrylate, isooctyl acrylate, methyl methacrylate, ethyl methacrylate, hydroxyethyl acrylate, and hydroxypropyl acrylate.

[0016] A second aspect of the present application provides a method for preparing a fluorinated polymer, comprising the following steps:

[0017] Under polymerizable conditions, at least one monomer represented by formula I and at least one monomer represented by formula II are polymerized, wherein the molar content of the monomer represented by formula I is 70% to 90%, based on the total moles of the monomer represented by formula I and the monomer represented by formula II.

[0018]

[0019] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, fluorine-substituted C 1-3 One or more of the alkyl groups, R4, R5, and R6 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 One or more of alkyl, R7 is selected from substituted or unsubstituted C 1-9 alkyl.

[0020] Compared with traditional binders, the fluorine-containing polymer prepared by this method can improve the stability and bonding performance of the primer slurry, significantly broaden the process window of the primer slurry, and improve the performance of the primer slurry.

[0021] In any embodiment, R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine, and trifluoromethyl, and R5 and R6 are each independently selected from one or two of hydrogen and methyl.

[0022] In any embodiment, the molar content of the monomer represented by formula II is 10% to 30%, based on the total moles of the monomer represented by formula I and the monomer represented by formula II.

[0023] Based on the total molar content of the structural units of the fluoropolymer, when the molar content of the structural units derived from the monomer represented by Formula II is 10% to 30%, the viscosity of the fluoropolymer is appropriate, which can comprehensively improve the processability and adhesion of the slurry, taking into account the processing performance and use performance of the primer layer.

[0024] In any embodiment, the polymerization reaction includes a first stage polymerization and a second stage polymerization,

[0025] First stage polymerization: adding an initiator, a first emulsifier, at least one monomer represented by formula I and an aqueous medium into a reaction vessel to carry out first stage polymerization, and continuously feeding the monomer represented by formula I into the first stage polymerization;

[0026] Second stage polymerization: After a period of reaction, an initiator, a second emulsifier, at least one monomer represented by formula II and an aqueous medium are added to the reaction vessel to carry out a second stage polymerization, in which the monomer represented by formula I is continuously fed.

[0027] The method provided by the present application first continuously feeds the monomer represented by formula I to form a fluorine-containing chain segment, ensuring that the fluorine-containing polymer has high bonding properties; then introduces the monomer represented by formula II to reduce the contact of the fluorine-containing chain segment with the external environment, which can effectively reduce the viscosity of the slurry. The fluorine-containing polymer prepared by this method can more effectively improve the stability and bonding properties of the primer slurry than the fluorine-containing polymer prepared by simultaneously polymerizing all the monomers into the reaction vessel, further broaden the process window and storage performance of the primer slurry, and help reduce the manufacturing cost of the primer layer.

[0028] In any embodiment, the mass of the monomer of formula I introduced in the first stage polymerization is 90% to 95% of the total mass of the monomer of formula I supplied in the polymerization reaction, and the mass of the monomer of formula I introduced in the second stage polymerization reaction is 5% to 10% of the total mass of the monomer of formula I supplied in the polymerization reaction.

[0029] In any embodiment, the initiator provided in the first stage polymerization and the initiator provided in the second stage polymerization are both persulfate, and the mass percentage of the initiator provided in the first stage polymerization is 0.05% to 0.1%, based on the total mass of the monomer represented by formula I and the monomer represented by formula II; the mass percentage of the initiator provided in the second stage polymerization is 0.05% to 0.1%, based on the mass of the monomer represented by formula II.

[0030] In any embodiment, the mass percentage of the first emulsifier is 0.2% to 0.7%, based on the total mass of the monomer represented by formula I and the monomer represented by formula II.

[0031] In any embodiment, the mass percentage of the second emulsifier is 0.5% to 1.5%, based on the mass of the monomer represented by formula II.

[0032] In any embodiment, the mass percentage of the aqueous medium provided in the first stage polymerization is 200% to 500%, and the mass percentage of the aqueous medium provided in the second stage polymerization is 100% to 200%, based on the total mass of the monomer represented by formula I and the monomer represented by formula II.

[0033] In any embodiment, the reaction pressure of the first stage polymerization is 5.5-7.5 MPa, and the reaction temperature is 75° C.-85° C.

[0034] In any embodiment, the reaction pressure of the second stage polymerization is 4.5-6.5 MPa, and the reaction temperature is 86° C.-95° C.

[0035] In any embodiment, after the reaction for a period of time, providing an initiator, a second emulsifier, at least one monomer represented by formula II, and an aqueous medium into the reaction container for a second stage polymerization comprises:

[0036] After adding the initiator into the reaction container, a premixed solution comprising the initiator, a second emulsifier, at least one monomer represented by formula II and an aqueous medium is added.

[0037] In any embodiment, the first emulsifier is an alkali metal perfluorooctanoate.

[0038] In any embodiment, the second emulsifier is one or both of polyoxyethylene-4-phenol ether ammonium sulfate and nonylphenol polyoxyethylene ether ammonium sulfate.

[0039] The third aspect of the present application provides an application of the fluorine-containing polymer of the first aspect in a secondary battery. Optionally, the secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.

[0040] The fourth aspect of the present application provides a primer slurry comprising a binder, a conductive agent and a solvent, wherein the binder comprises the fluorine-containing polymer according to the first aspect of the present application.

[0041] The primer slurry is easy to process and prepare and has good uniformity, which helps to improve battery production capacity.

[0042] In any embodiment, the mass fraction of the binder is 0.5% to 5%, based on the mass of the conductive agent.

[0043] In any embodiment, the solid content of the primer slurry is 15% to 30%, and the viscosity of the primer slurry is 100 mPa·s to 1000 mPa·s.

[0044] Primer slurries with a solids content of 15% to 30% have a viscosity of 100 to 1000 mPa·s. This eliminates the need for additional dispersants or thickeners to improve processing performance when using fluoropolymers, helping to increase production efficiency and optimize the manufacturing process. Primer slurries within this viscosity range also offer stability, fluidity, and adhesion, enhancing the adhesion of the primer layer while ensuring uniform coating, contributing to improved batch stability.

[0045] In any embodiment, the solvent is an organic solvent.

[0046] In any embodiment, the solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylpropionamide, N,N-diethylpropionamide, N,N-dipropylpropionamide, N,N-dibutylpropionamide, N,N-dimethylethylpropionamide and 3-butoxy-N-methylpropionamide.

[0047] A fifth aspect of the present application provides a method for preparing a primer layer, comprising the following steps:

[0048] gravure coating the primer slurry on the surface of the current collector, wherein the primer slurry is the primer slurry of the fourth aspect of the present application;

[0049] After drying, a base coating layer is obtained, and the thickness of the base coating layer is 1 μm to 3 μm.

[0050] The primer slurry is gravure coated on the surface of the current collector. After drying, the primer layer with a thickness of 1um to 3um has a lower membrane resistance, which can ensure the electrical performance of the electrode and at the same time take into account the adhesion of the primer layer.

[0051] The sixth aspect of the present application provides a secondary battery comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the negative electrode sheet comprises the primer layer of the fifth aspect of the present application.

[0052] In any embodiment, the secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.

[0053] A seventh aspect of the present application provides a battery module including the secondary battery according to the sixth aspect of the present application.

[0054] An eighth aspect of the present application provides a battery pack comprising the secondary battery of the sixth aspect of the present application or the battery module of the seventh aspect of the present application.

[0055] The ninth aspect of the present application provides an electrical device comprising at least one selected from the secondary battery of the sixth aspect of the present application, the battery module of the seventh aspect of the present application, or the battery pack of the eighth aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] FIG1 is a schematic diagram of a gravure coating process according to an embodiment of the present application;

[0057] FIG2 is a schematic diagram of a secondary battery according to an embodiment of the present application;

[0058] FIG3 is an exploded view of the secondary battery according to one embodiment of the present application shown in FIG2 ;

[0059] FIG4 is a schematic diagram of a battery module according to an embodiment of the present application;

[0060] FIG5 is a schematic diagram of a battery pack according to an embodiment of the present application;

[0061] FIG6 is an exploded view of the battery pack shown in FIG5 according to an embodiment of the present application;

[0062] FIG. 7 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.

[0063] Description of reference numerals:

[0064] 1 Battery pack; 2 Upper box; 3 Lower box; 4 Battery module; 5 Secondary battery; 51 Housing; 52 Electrode assembly; 53 Cover plate; 6 Gravure coating device; 61 Press roller; 62 Gravure roller; 63 Current collector; 64 Scraper; 65 Slurry tank. DETAILED DESCRIPTION

[0065] Below, the embodiments of the binder, preparation method, electrode, battery, and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided to enable those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0066] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0067] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0068] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0069] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0070] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0071] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0072] The conductivity of the electrode is one of the most important research topics in secondary batteries. During the preparation process of the secondary battery pole piece, a primer layer is coated between the current collector and the active material layer to provide electrical conduction between the active material layer and the current collector, thereby reducing the contact resistance between the active material layer and the current collector and improving the performance of the battery. In the prior art, binders and conductive agents are generally used to prepare the primer layer. Traditional polyvinylidene fluoride binders will make the slurry have high viscosity and poor filterability, making it difficult to apply evenly. Therefore, a dispersant needs to be added during the slurry preparation process to improve the processing performance of the slurry. This will undoubtedly complicate the production process of the slurry, affect production efficiency and lead to poor stability of the slurry between batches. Based on the above technical problems, the present application has developed a polymer that can play the role of a binder and a dispersant in the primer slurry, improve the filterability and stability of the primer slurry, and help improve the production efficiency and production quality of the primer layer.

[0073] Based on this, the present application proposes a fluorine-containing polymer, which comprises a structural unit derived from a monomer represented by formula I and a structural unit derived from a monomer represented by formula II, wherein the molar content of the structural unit derived from the monomer represented by formula I is 70% to 90%, based on the total molar number of the structural units of the fluorine-containing polymer.

[0074]

[0075] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, fluorine-substituted C 1-3 One or more of the alkyl groups, R4, R5, and R6 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 One or more of alkyl, R7 is selected from substituted or unsubstituted C 1-9 alkyl.

[0076] As used herein, the term "fluoropolymer" refers to a polymer containing fluorine in its structural units.

[0077] As used herein, the term "polymer" includes, on the one hand, a collection of chemically homogeneous macromolecules prepared by polymerization, but differing in degree of polymerization, molar mass, and chain length. The term also includes derivatives of such collections of macromolecules formed by polymerization, i.e., products that can be obtained by reaction of functional groups in the aforementioned macromolecules, such as addition or substitution, and can be chemically homogeneous or chemically heterogeneous.

[0078] In this article, the term “C 1-5 "Alkyl" refers to a straight or branched hydrocarbon chain radical consisting solely of carbon and hydrogen atoms, with no unsaturation present, having from one to five carbon atoms, and attached to the remainder of the molecule by a single bond. 1-3 Alkyl", the term "C 1-9 "Alkyl" should be interpreted accordingly. C 1-5 Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, 1-methylethyl (isopropyl), butyl, and pentyl. 1- 3 Alkyl is -CF3, -CH3CH2F, -CH2FCH2F. 1-9 Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, and n-nonyl.

[0079] As used herein, the term "substituted" refers to a compound or chemical moiety in which at least one hydrogen atom is replaced by another chemical moiety, wherein the substituents are each independently selected from the group consisting of hydroxyl, thiol, amino, cyano, nitro, aldehyde, halogen, alkenyl, alkynyl, aryl, heteroaryl, C 1-6 Alkyl, C 1-6 Alkoxy.

[0080] In this article, the term "process window" refers to the process range that can ensure product quality, including but not limited to temperature range, pressure range, storage time length, etc. It can be understood that the wider the process window, the lower the requirement for process accuracy.

[0081] In some embodiments, R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine atoms, and trifluoromethyl groups, and R5 and R6 are each independently selected from one or both of hydrogen and methyl groups.

[0082] In some embodiments, the monomer represented by Formula I is selected from one or more of vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.

[0083] In some embodiments, the monomer represented by formula II is selected from one or more of methyl acrylate, ethyl acrylate, butyl acrylate, isoamyl acrylate, isooctyl acrylate, methyl methacrylate, ethyl methacrylate, hydroxyethyl acrylate, and hydroxypropyl acrylate.

[0084] In some embodiments, the polymer comprises one or more structural units derived from the monomers shown in formula I. In some embodiments, the polymer comprises one or more structural units derived from the monomers shown in formula II. In some embodiments, the polymer includes but is not limited to vinylidene fluoride-methyl acrylate copolymer, vinylidene fluoride-ethyl acrylate copolymer, vinylidene fluoride-butyl acrylate copolymer, vinylidene fluoride-isoamyl acrylate copolymer, vinylidene fluoride-isooctyl acrylate copolymer, vinylidene fluoride-methyl methacrylate copolymer, vinylidene fluoride-ethyl methacrylate copolymer, vinylidene fluoride-hydroxyethyl acrylate copolymer, vinylidene fluoride-hydroxypropyl acrylate copolymer, vinylidene fluoride-tetrafluoroethylene-butyl acrylate copolymer, vinylidene fluoride-tetrafluoropropylene-methyl acrylate copolymer, vinylidene fluoride-fluorinated vinyl-butyl acrylate copolymer, vinylidene fluoride-chlorotrifluoroethylene-butyl acrylate copolymer, vinylidene fluoride-hexafluoropropylene-butyl acrylate copolymer, vinylidene fluoride-hexafluoropropylene-methyl acrylate copolymer, vinylidene fluoride-hexafluoropropylene-isooctyl acrylate copolymer.

[0085] In some embodiments, the molar content of the structural units derived from the monomer represented by Formula I can be selected from 70%, 75%, 80%, 85% or 90%, based on the total moles of the structural units in the fluoropolymer.

[0086] The fluorine element in the structural unit derived from the monomer represented by formula I can form hydrogen bonds with the hydroxyl group and / or carboxyl group on the surface of the current collector, so that the primer layer has good adhesion and is not easy to fall off during the manufacturing and use process, causing safety accidents; the structural unit derived from the monomer represented by formula II can effectively reduce the fluorine content of the fluorine-containing polymer, so that the mass content of the structural unit derived from the monomer represented by formula I is between 70% and 90%, which helps to adjust the slurry viscosity, improve the phenomenon of excessive viscosity of the primer slurry caused by fluorine element, and improve the processability of the slurry.

[0087] Compared with the polyvinyl difluoride binder commonly used in the prior art, the fluorine-containing polymer provided in the present application reduces the viscosity of the slurry, improves the filterability, and improves the processability of the primer slurry, so that the primer slurry can meet the production requirements of the primer slurry without adding a dispersant, which is beneficial to optimizing the production process of the primer slurry and improving its production quality.

[0088] In some embodiments, the molar content of the structural units derived from the monomers of Formula II is 10% to 30%, based on the total moles of the structural units in the fluoropolymer. In some embodiments, the molar content of the structural units derived from the monomers of Formula II can be any one of 12%, 15%, 18%, 20%, 22%, 25%, and 30%, based on the total moles of the structural units in the fluoropolymer.

[0089] Based on the total molar content of the structural units of the fluoropolymer, when the molar content of the structural units derived from the monomer represented by Formula II is 10% to 30%, the viscosity of the fluoropolymer is appropriate, so that the electrode has good adhesion. At the same time, the appropriate viscosity makes the slurry have good fluidity and filterability, which can comprehensively improve the processability and adhesion of the slurry, taking into account the processing performance and performance of the primer layer.

[0090] In some embodiments, the weight average molecular weight of the fluorine-containing polymer is 400,000 to 500,000. In some embodiments, the weight average molecular weight of the fluorine-containing polymer can be any one of 430,000, 450,000, and 480,000.

[0091] As used herein, the term "weight average molecular weight" refers to the sum of the weight fractions of molecules of different molecular weights in a polymer multiplied by their corresponding molecular weights.

[0092] In the present application, the weight-average molecular weight of the polymer can be tested using methods known in the art, such as gel chromatography, such as using a Waters 2695 Isocratic HPLC gel chromatograph (differential refractive index detector 2141). In some embodiments, the testing method is to use a polystyrene solution sample with a mass fraction of 3.0% as a reference and select a matching chromatographic column (oily: Styragel HT5DMF7.8*300mm+Styragel HT4). Use purified N-methylpyrrolidone (NMP) solvent to prepare a 3.0% fluoropolymer glue, and let the prepared solution stand for one day for use. During the test, first use a syringe to draw tetrahydrofuran, rinse, and repeat several times. Then draw 5 ml of the experimental solution, expel the air in the syringe, and wipe the needle tip dry. Finally, slowly inject the sample solution into the injection port. After the reading stabilizes, obtain the data and read the weight-average molecular weight.

[0093] Fluoropolymers with a weight-average molecular weight of 400,000 to 500,000 have an appropriate viscosity, which enables the electrode to have good adhesion. At the same time, the appropriate viscosity is conducive to subsequent coating work, and can comprehensively improve the processability and adhesion of the slurry, taking into account the processing performance and use performance of the primer layer.

[0094] In one embodiment of the present application, a method for preparing a fluorine-containing polymer is provided, comprising the following steps:

[0095] Under polymerizable conditions, at least one monomer represented by formula I and at least one monomer represented by formula II are polymerized, wherein the molar content of the monomer represented by formula I is 70% to 90%, based on the total moles of the monomer represented by formula I and the monomer represented by formula II.

[0096]

[0097] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, fluorine-substituted C 1-3 One or more of the alkyl groups, R4, R5, and R6 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 One or more of alkyl, R7 is selected from substituted or unsubstituted C 1-9 alkyl.

[0098] As used herein, the term "polymerizable conditions" refers to those conditions including temperature, pressure, reactant concentrations, optional solvents / diluents, reactant mixing / addition parameters selected by one skilled in the art, and other conditions that facilitate the reaction of one or more monomers within at least one polymerization reactor.

[0099] Compared with traditional binders, the fluorine-containing polymer prepared by this method can improve the stability and bonding performance of the primer slurry, significantly broaden the process window of the primer slurry, and improve the performance of the primer slurry.

[0100] In some embodiments, R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine, and trifluoromethyl, and R5 and R6 are each independently selected from one or both of hydrogen and methyl.

[0101] In some embodiments, the molar content of the monomer represented by Formula II is 10% to 30%, based on the total molar amount of the monomer represented by Formula I and the monomer represented by Formula II. In some embodiments, the molar content of the structural unit derived from the monomer represented by Formula II can be any one of 12%, 15%, 18%, 20%, 22%, 25%, and 30%, based on the total molar amount of the monomer represented by Formula I and the monomer represented by Formula II.

[0102] Based on the total molar content of the structural units of the fluoropolymer, when the molar content of the structural units derived from the monomer represented by Formula II is 10% to 30%, the viscosity of the fluoropolymer is appropriate, which can comprehensively improve the processability and adhesion of the slurry, taking into account the processing performance and use performance of the primer layer.

[0103] In some embodiments, the polymerization reaction includes a first stage polymerization and a second stage polymerization,

[0104] First stage polymerization: adding an initiator, a first emulsifier, at least one monomer represented by formula I and an aqueous medium into a reaction vessel to carry out first stage polymerization, and continuously feeding the monomer represented by formula I into the first stage polymerization;

[0105] Second stage polymerization: After a period of reaction, an initiator, a second emulsifier, at least one monomer represented by formula II and an aqueous medium are added to the reaction vessel to carry out the second stage polymerization, and the monomer represented by formula I is continuously fed into the second stage polymerization.

[0106] As used herein, the term "continuous feeding" refers to the slow, small, incremental addition of monomers.

[0107] The method provided by the present application first continuously feeds the monomer represented by formula I to form a fluorine-containing chain segment, ensuring that the fluorine-containing polymer has high bonding properties; then introduces the monomer represented by formula II to reduce the contact of the fluorine-containing chain segment with the external environment, which can effectively reduce the viscosity of the slurry. The fluorine-containing polymer prepared by this method can more effectively improve the stability and bonding properties of the primer slurry than the fluorine-containing polymer prepared by simultaneously polymerizing all the monomers into the reaction vessel, further broaden the process window and storage performance of the primer slurry, and help reduce the manufacturing cost of the primer layer.

[0108] In some embodiments, the initiator provided in the first stage polymerization and the initiator provided in the second stage polymerization are both persulfate, and the mass percentage of the initiator provided in the first stage polymerization is 0.05% to 0.1%, based on the total mass of the monomer represented by Formula I and the monomer represented by Formula II; the mass percentage of the initiator provided in the second stage polymerization is 0.05% to 0.1%, based on the mass of the monomer represented by Formula II.

[0109] In some embodiments, the initiator persulfate may be potassium persulfate, which effectively decomposes at temperatures above 60° C. to generate free radical ions or ionic radicals, and is suitable as an initiator for emulsion polymerization.

[0110] In some embodiments, the mass percentage of the initiator provided in the first stage polymerization is 0.05%, 0.07%, 0.09% or 0.1%, based on the total mass of the monomer represented by formula I and the monomer represented by formula II.

[0111] In some embodiments, the weight percentage of the initiator provided in the second stage polymerization is 0.05%, 0.07%, 0.09% or 0.1%, based on the weight of the monomer represented by Formula II.

[0112] In some embodiments, the mass percentage of the first emulsifier is 0.2% to 0.7%, based on the total mass of the monomer represented by Formula I and the monomer represented by Formula II. In some embodiments, the mass percentage of the first emulsifier is 0.2%, 0.5% or 0.7%, based on the total mass of the monomer represented by Formula I and the monomer represented by Formula II.

[0113] In some embodiments, the first emulsifier is an alkali metal perfluorooctanoate.

[0114] In some embodiments, the weight percentage of the second emulsifier is 0.5% to 1.5%, based on the weight of the monomer represented by formula II. In some embodiments, the weight percentage of the second emulsifier is 0.5%, 0.75%, 1.0%, 1.25% or 1.5%, based on the weight of the monomer represented by formula II.

[0115] In some embodiments, the second emulsifier is one or both of polyoxyethylene-4-phenol ether ammonium sulfate and nonylphenol polyoxyethylene ether ammonium sulfate.

[0116] In some embodiments, the mass percentage of the aqueous medium provided in the first stage of polymerization is 200% to 500%, and the mass percentage of the aqueous medium provided in the second stage of polymerization is 100% to 200%, based on the total mass of the monomer represented by Formula I and the monomer represented by Formula II. In some embodiments, the mass percentage of the aqueous medium provided in the first stage of polymerization is 200%, 300%, 400%, or 500%, and the mass percentage of the aqueous medium provided in the second stage of polymerization is 100%, 150%, or 200%, based on the total mass of the monomer represented by Formula I and the monomer represented by Formula II. In some embodiments, the aqueous medium is an aqueous solvent, which can be deionized water or a mixture of deionized water and other hydrophilic solvents, such as alcohol or ethyl acetate.

[0117] In some embodiments, the reaction pressure of the first stage polymerization is 5.5-7.5 MPa, and the reaction temperature is 75° C.-85° C. In some embodiments, the reaction pressure of the first stage polymerization is 5.5 MPa, 6.5 MPa, or 7.5 MPa, and the reaction temperature is 75° C., 80° C., or 85° C.

[0118] In some embodiments, the reaction pressure of the second stage polymerization is 4.5-6.5 MPa, and the reaction temperature is 86° C.-95° C. In some embodiments, the reaction pressure of the second stage polymerization is 4.5 MPa, 5.5 MPa, or 6.5 MPa, and the reaction temperature is 86° C., 90° C., or 95° C.

[0119] In some embodiments, the mass of the monomer of Formula I introduced into the first stage of polymerization is 90% to 95% of the total mass of the monomer of Formula I supplied in the polymerization reaction, and the mass of the monomer of Formula I introduced into the second stage of polymerization is 5% to 10% of the total mass of the monomer of Formula I supplied in the polymerization reaction. In some embodiments, the mass of the monomer of Formula I introduced into the first stage of polymerization is 90%, 92% or 95% of the total mass of the monomer of Formula I supplied in the polymerization reaction, and the mass of the monomer of Formula I introduced into the second stage of polymerization is 5%, 7% or 10% of the total mass of the monomer of Formula I supplied in the polymerization reaction.

[0120] In some embodiments, after a period of reaction, providing an initiator, a second emulsifier, at least one monomer represented by Formula II, and an aqueous medium into a reaction vessel for a second stage polymerization comprises:

[0121] After adding the initiator into the reaction container, a premixed solution comprising the initiator, a second emulsifier, at least one monomer represented by formula II and an aqueous medium is added.

[0122] In one embodiment of the present application, a fluoropolymer according to any embodiment is provided for use in a secondary battery. Optionally, the secondary battery comprises at least one of a lithium-ion battery, a sodium-ion battery, a magnesium-ion battery, and a potassium-ion battery. In some embodiments, the fluoropolymer is used as a binder in a secondary battery. In some embodiments, the fluoropolymer is used as a binder for a primer layer in a secondary battery.

[0123] [Primer slurry]

[0124] In one embodiment of the present application, a primer slurry is provided, comprising a binder, a conductive agent, and a solvent, wherein the binder comprises a fluorine-containing polymer in any embodiment.

[0125] As used herein, the term "binder" refers to a chemical compound, polymer, or mixture that forms a colloidal solution or colloidal dispersion in a dispersion medium.

[0126] In the present application, the term "conductive agent" refers to a substance that collects microcurrents, including but not limited to at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0127] In some embodiments, the solvent is an organic solvent.

[0128] Organic solvents are organic compounds containing carbon atoms. They can dissolve some water-insoluble substances. Using organic solvents as the solvent for the undercoat layer makes the undercoat slurry suitable for preparing the undercoat layer for the negative electrode sheet. This undercoat layer is not easily dissolved during the negative electrode film preparation process and has high stability.

[0129] In some embodiments, the solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylpropionamide, N,N-diethylpropionamide, N,N-dipropylpropionamide, N,N-dibutylpropionamide, N,N-dimethylethylpropionamide, and 3-butoxy-N-methylpropionamide.

[0130] The primer slurry is easy to process and prepare and has good uniformity, which helps to improve battery production capacity.

[0131] In some embodiments, the mass fraction of the binder is 0.5% to 5%, based on the mass of the conductive agent. In some embodiments, the mass fraction of the binder can be any one of 0.5%, 1.0%, 2.0%, 4.0%, and 5.0%, based on the mass of the conductive agent.

[0132] When the mass content of the binder is within an appropriate range, there is sufficient adhesion between the primer layer and the current collector, avoiding the risk of the primer layer falling off during the use of the battery cell; at the same time, when the mass content of the binder is within an appropriate range, the primer slurry has an appropriate viscosity, and the slurry has good fluidity and filterability, which is beneficial to subsequent coating work.

[0133] In some embodiments, the solid content of the primer slurry is 15% to 30%, and the viscosity of the primer slurry is 100 mPa·s to 1000 mPa·s. In some embodiments, when the solid content of the primer slurry is 15% to 30%, the viscosity of the primer slurry is 100 mPa·s, 200 mPa·s, 300 mPa·s, 400 mPa·s, 500 mPa·s, 600 mPa·s, 700 mPa·s, 800 mPa·s, 900 mPa·s, or 1000 mPa·s.

[0134] The viscosity of the primer slurry is within an appropriate range, which is beneficial for subsequent coating and drying. On the other hand, the appropriate viscosity can improve the stability of the slurry, making the slurry have good fluidity and filterability.

[0135] In the present application, the viscosity of the fluoropolymer primer slurry can be tested by methods known in the art, such as using a rotary viscometer.

[0136] Primer slurries with a solids content of 15% to 30% have a viscosity of 100 to 1000 mPa·s. This eliminates the need for additional dispersants or thickeners to improve processing performance when using fluoropolymers, helping to increase production efficiency and optimize the manufacturing process. Primer slurries within this viscosity range also offer stability, fluidity, and adhesion, enhancing the adhesion of the primer layer while ensuring uniform coating, contributing to improved batch stability.

[0137] In one embodiment of the present application, a method for preparing a primer layer is provided, comprising the following steps:

[0138] The primer slurry is gravure coated on the surface of the current collector, and the primer slurry is the primer slurry in any embodiment; and the primer coating layer is obtained after the primer slurry is dried.

[0139] In some embodiments, the gravure coating process is shown in FIG1 . A gravure roller 62 in a gravure coating apparatus 6 is partially immersed in the slurry in a slurry tank 65 . The rotation of the gravure roller 62 drives the slurry to move. A scraper 64 scrapes the slurry from the smooth surface of the gravure roller 62 . The slurry remaining in the pits on the surface of the gravure roller 62 is transferred to the surface of the current collector 63 under the pressure of the pressure roller 61 . The rotation direction of the gravure roller 62 is opposite to the movement direction of the pressure roller 61. The depth of the pits on the surface of the gravure roller 62 can be adjusted according to the desired thickness of the primer layer, and the depth of the pits can be selected to be 10-100 μm.

[0140] The surface of the primer layer prepared by gravure coating is rough, and the bonding performance between the primer layer and the membrane layer or current collector can be improved by mechanical riveting, so that the pole piece has better bonding force.

[0141] In some embodiments, the thickness of the primer layer is 1 um to 3 um.

[0142] The primer slurry is gravure coated on the surface of the current collector. After drying, the primer layer with a thickness of 1um to 3um has excellent adhesion and low membrane resistance, which can ensure the mechanical and electrochemical properties of the electrode.

[0143] In one embodiment of the present application, a secondary battery is provided, comprising a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte, wherein the negative electrode sheet comprises a primer layer as described in any embodiment. In some embodiments, the secondary battery comprises at least one of a lithium-ion battery, a sodium-ion battery, a magnesium-ion battery, and a potassium-ion battery.

[0144] During the battery's charge and discharge processes, active ions are embedded in and extracted from the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. A separator, located between the positive and negative electrodes, prevents short circuits while allowing ions to pass through.

[0145] [Positive electrode]

[0146] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector.

[0147] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0148] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0149] In some embodiments, the positive electrode active material may adopt the positive electrode active material for batteries that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0150] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0151] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0152] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0153] [Negative electrode]

[0154] The negative electrode sheet includes a negative electrode current collector, a primer layer disposed on at least one surface of the negative electrode current collector, and a negative electrode film layer disposed on the primer layer, wherein the negative electrode film layer includes a negative electrode active material.

[0155] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0156] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0157] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0158] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0159] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0160] In some embodiments, the negative electrode film layer may optionally further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0161] In some embodiments, the negative electrode sheet can be prepared by dispersing the above-mentioned components for preparing the primer layer, such as a fluoropolymer and a conductive agent, in N-methyl-2-pyrrolidone to form a primer slurry; gravure coating the primer slurry on the surface of a copper foil current collector to obtain a current collector having a primer layer; dispersing the above-mentioned components for preparing the negative electrode film layer, such as the negative electrode active material, conductive agent, binder, and any other components, in a solvent (such as deionized water) to form a negative electrode slurry; coating the negative electrode slurry on the current collector having the primer layer; and drying, cold pressing, and other processes to obtain the negative electrode sheet.

[0162] [Electrolytes]

[0163] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.

[0164] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.

[0165] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0166] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0167] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0168] [Isolation film]

[0169] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0170] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0171] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0172] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0173] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0174] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG2 shows a secondary battery 5 having a square structure as an example.

[0175] In some embodiments, referring to Figure 3, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0176] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0177] Figure 4 shows an example battery module 4. Referring to Figure 4 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.

[0178] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0179] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0180] Figures 5 and 6 illustrate an example battery pack 1. Referring to Figures 5 and 6 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be positioned over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0181] In addition, the present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0182] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0183] Figure 7 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.

[0184] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.

[0185] Example

[0186] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0187] 1. Preparation method

[0188] Example 1

[0189] 1) Preparation of fluorinated polymers

[0190] 26 kg of deionized water, 37.3 g of sodium perfluorooctanoate, and 112 g of a 5% potassium persulfate solution, wherein the conductivity of the deionized water is less than or equal to 2 μs / cm, are sequentially added into the reactor, and the reactor is closed;

[0191] The reactor was vacuumed and filled with nitrogen, and the operation was repeated until the oxygen concentration in the reactor was less than 100 ppm;

[0192] Vinylidene fluoride monomer was introduced into the reactor, and the pressure in the reactor was 7.5 MPa. The reaction began when the temperature in the reactor was raised to 85°C. Vinylidene fluoride monomer was continuously introduced during the reaction to maintain the reaction pressure in the reactor constant.

[0193] 11.2 kg of deionized water, 29.8 g of polyoxyethylene-4-phenol ether ammonium sulfate, and 23.3 mol of butyl acrylate were added to a stirring tank and stirred uniformly, wherein the conductivity of the deionized water was less than or equal to 2 μs / cm, to obtain a premixed solution;

[0194] When the total amount of vinylidene fluoride monomer introduced was 66.5 mol, 44.8 g of 5% concentration of ammonium persulfate was added, the reaction pressure was adjusted to 6.0 MPa, the temperature was raised to 90°C, and the premix was slowly added to the reactor. The entire addition time of the premix was 2.5 hours. At the same time, the remaining 3.5 mol of vinylidene fluoride monomer was gradually introduced;

[0195] When the pressure in the autoclave drops to 0.2 MPa, the reaction is stopped;

[0196] The reaction product is cooled to room temperature, and then condensed, washed, separated, dried, and crushed to obtain a vinylidene fluoride-butyl acrylate copolymer binder.

[0197] 2) Preparation of primer slurry

[0198] Weigh 5.88 kg of conductive carbon black and 0.12 kg of vinylidene fluoride-butyl acrylate copolymer binder and add them into the stirring tank in sequence. Set the stirring speed to 300 rpm and stir for 10 minutes.

[0199] Weigh 14 kg of N-methylpyrrolidone and add it to the stirring tank. Set the stirring speed to 1200 rpm and stir for 120 minutes.

[0200] Then weigh 10 kg of N-methylpyrrolidone and add it to the stirring tank. Set the stirring speed to 1500 rpm and stir for 120 minutes.

[0201] The slurry was filtered through a 200-mesh filter to obtain a primer slurry.

[0202] 3) Preparation of base coating

[0203] The primer slurry is coated using the gravure coating device shown in Figure 1. The primer slurry is first injected into the slurry tank, and the primer slurry is carried by the rotation of the gravure roller. After the primer slurry on the smooth part is scraped off by the scraper, the remaining primer slurry remains only in the pits on the surface of the gravure roller. The depth of the pits is 50um. Under the pressure of the pressure roller, the primer slurry in the pits can be transferred to the surface of the copper foil current collector substrate and dried to obtain a primer layer with a thickness of 2um.

[0204] 4) Preparation of negative electrode sheet

[0205] Graphite material, conductive agent carbon black, styrene-butadiene binder, sodium carboxymethyl cellulose, and N-methylpyrrolidone (NMP) are stirred and mixed uniformly in a weight ratio of 97.15:0.04:1.95:0.5:0.36 to obtain a negative electrode slurry with a solid content of 64%;

[0206] The negative electrode slurry is evenly coated on the base coating, and then dried, cold pressed, and cut to obtain the negative electrode sheet.

[0207] In Examples 2 and 3, the ratio of each monomer in the fluorine-containing polymer was adjusted, and other parameters remained the same as in Example 1. Specific parameters are shown in Tables 1 and 2.

[0208] In Examples 4 to 7, the reaction conditions for synthesizing the fluoropolymers were adjusted to achieve different weight-average molecular weights. Other parameters remained the same as in Example 1. Specific parameters are shown in Tables 1 and 2. Specifically, the method for preparing the fluoropolymer with a weight-average molecular weight of 300,000 in Example 4 was essentially the same as in Example 1, except that the amount of 5% potassium persulfate solution added was adjusted to 99.00 g.

[0209] The preparation method of the fluorine-containing polymer with a weight average molecular weight of 400,000 in Example 5 is basically the same as the steps in Example 1, except that the amount of 5% potassium persulfate solution added is adjusted to 99.45 g.

[0210] The preparation method of the fluorine-containing polymer with a weight average molecular weight of 500,000 in Example 6 is basically the same as the steps in Example 1, except that the reaction temperature is adjusted to 80° C. and the amount of 5% potassium persulfate solution added is adjusted to 89.45 g.

[0211] The preparation method of the fluorine-containing polymer with a weight average molecular weight of 600,000 in Example 7 is basically the same as that in Example 1, except that the reaction temperature is adjusted to 80° C. and the amount of 5% potassium persulfate solution added is adjusted to 81.00 g.

[0212] In Examples 8 to 11, the mass fraction of the binder in the primer slurry was adjusted, and other parameters remained the same as in Example 1. Specific parameters are shown in Tables 1 and 2.

[0213] In Examples 12 to 15, the solid content of the primer slurry was adjusted, and other parameters remained the same as in Example 1. Specific parameters are shown in Tables 1 and 2.

[0214] In Example 16, the ethyl acrylate monomer was replaced with isooctyl acrylate monomer, and the other parameters were the same as in Example 1. For specific parameters, see Tables 1 and 2.

[0215] In Example 17, the base coating layer was prepared by a doctor blade coating method. Other methods were the same as in Example 1. For specific parameters, see Tables 1 and 2.

[0216] In Example 18, the preparation method is consistent with that of Example 1, except that the binder in the primer layer is a vinylidene fluoride-butyl acrylate copolymer prepared by a traditional method, and the synthesis method thereof is:

[0217] 37.2 kg of deionized water (conductivity less than or equal to 2 μs / cm), 37.3 g of sodium perfluorooctanoate, 112 g of 5% potassium persulfate solution, 44.8 g of 5% ammonium persulfate solution, and 29.8 g of polyoxyethylene-4-phenol ether ammonium sulfate were added to the reactor in sequence, and the reactor was closed;

[0218] The reactor was vacuumed and filled with nitrogen, and the operation was repeated until the oxygen concentration in the reactor was less than 100 ppm;

[0219] Vinylidene fluoride monomer and 23.3 mol of butyl acrylate were introduced into the reactor until the pressure inside the reactor reached 7.5 MPa;

[0220] The temperature in the kettle was raised to 85°C to start the reaction. During the reaction, vinylidene fluoride monomer was continuously introduced to maintain the reaction pressure in the kettle constant. The molar number of vinylidene fluoride monomer introduced was 70 mol.

[0221] The reaction was stopped when the pressure in the autoclave dropped to 0.2 MPa;

[0222] The mixture is cooled to room temperature, condensed, washed, separated, dried and crushed to obtain a fluorine-containing polymer, namely, a vinylidene fluoride-butyl acrylate copolymer.

[0223] In Comparative Example 1, the preparation method is consistent with that of Example 1, except that in Comparative Example 1, vinylidene fluoride polymer is used as the binder of the primer slurry, which is HSV900 model produced by Arkema, France.

[0224] Comparative Example 2 is basically the same as Comparative Example 1, except that the preparation method of the primer layer is adjusted. The specific preparation method is as follows:

[0225] The primer slurry was coated on the surface of the copper foil current collector substrate using a doctor blade and dried to obtain a primer layer with a thickness of 2 μm.

[0226] In Comparative Examples 3 and 4, the ratios of the monomers in the fluorine-containing polymer were adjusted, and other parameters remained the same as those in Example 1. Specific parameters are shown in Tables 1 and 2.

[0227] The relevant parameters of the primer slurries and coatings of Examples 1 to 18 and Comparative Examples 1 to 4 are shown in Tables 1 and 2 below.

[0228] In addition, the primer slurries and coatings obtained in Examples 1 to 18 and Comparative Examples 1 to 4 were subjected to performance tests.

[0229] 2. Test Method

[0230] 1. Weight average molecular weight test

[0231] A Waters 2695 Isocratic HPLC gel chromatograph (differential refractive index detector 2141) was used. A 3.0% polystyrene solution sample was used as a reference, and a matching chromatographic column was selected (oily: Styragel HT5DMF7.8×300mm+Styragel HT4). A 3.0% fluoropolymer solution was prepared using purified N-methylpyrrolidone (NMP) solvent. The prepared solution was allowed to stand for one day before use. During the test, tetrahydrofuran was first drawn into a syringe and rinsed several times. Then 5 ml of the experimental solution was drawn, the air in the syringe was expelled, and the needle tip was wiped dry. Finally, the sample solution was slowly injected into the injection port. After the reading stabilized, the data was acquired and the weight-average molecular weight was read.

[0232] 2. Primer slurry viscosity test

[0233] Use a rotating viscometer to measure the viscosity of the primer slurry. Select a suitable rotor, secure the viscometer rotor, and place the primer slurry under the viscometer rotor, so that the slurry just covers the rotor scale line. Instrument model: Shanghai Fangrui NDJ-5S, rotor #62, speed of 30 rpm, measurable slurry viscosity range of 0-1000 mPa·s; rotor #63, speed of 30 rpm, measurable slurry viscosity range of 0-2000 mPa·s). Test temperature: 25°C, test time: 5 minutes, wait for the display to stabilize and read the data.

[0234] 3. Primer slurry filtration performance test

[0235] Take a 500ml beaker and place it at the lower end of the 200-mesh filter bracket, take 500ml of the primer slurry, and place it in the filter for filtration. When the slurry volume in the beaker reaches 300ml and the filtration time is less than 120s, it indicates that the filtration performance of the slurry is good and is judged as "Y". If the slurry cannot pass through the filter within 120s, it indicates that the filtration performance of the slurry is poor and is judged as "N".

[0236] 4. Solid content of primer slurry and the difference in solid content after standing for 24 hours

[0237] Weigh the copper foil in the weight loss meter, record it as M0, and reset the weight loss meter;

[0238] Take a small amount of the primer slurry and apply it on the copper foil, then put it into the weight loss meter and weigh it, which is recorded as M1;

[0239] Close the device and start drying;

[0240] After the test, record the weighing data as M2 and calculate the solid content as (M2-M0) / (M1-M0);

[0241] The solid content of the upper and lower primer slurries was measured in the same way after standing for 24 hours, and the solid content of the lower primer slurry minus the solid content of the upper primer slurry was taken as the difference in solid content of the primer slurry after standing for 24 hours.

[0242] 5. Adhesion of the electrode

[0243] With reference to GB-T2790-1995 national standard "Test method for 180° peel strength of adhesives", the adhesion test process of the examples and comparative examples of this application is as follows: Use a blade to cut a sample with a width of 30mm and a length of 150mm, and stick a special double-sided tape on the steel plate with a width of 20mm and a length of 100mm. Stick the negative electrode film layer of the electrode sample cut earlier on the double-sided tape, and then roll it three times in the same direction with a 2kg roller. Fix a paper tape with a width equal to the width of the electrode and a length of 250mm on the electrode current collector and fix it with wrinkle glue. Turn on the power of the Sansi tensile testing machine (sensitivity is 1N), the indicator light will light up, adjust the limit block to the appropriate position, and fix the end of the steel plate without the electrode with the lower clamp. Fold the paper tape upwards and fix it with the upper clamp. Use the "up" and "down" buttons on the manual controller included with the tensile testing machine to adjust the position of the upper clamp. Then test and read the value. The tensile speed is 50mm / min. The force when the electrode is under force balance divided by the width of the tape is used as the bonding force per unit length of the negative electrode to characterize the bonding strength between the film layer on the current collector and the current collector.

[0244] 6. Diaphragm resistance of the electrode

[0245] Cut the dried electrode sheet at the left, center, and right sides of the electrode into small discs with a diameter of 30mm. Turn on the Yuanneng Technology electrode resistance meter, place it in the appropriate position on the "probe" of the electrode resistance meter, click the "Start" button, and wait for the reading to stabilize before reading. Test two positions on each small disc, and calculate the average of the six measurements to obtain the film resistance of the electrode.

[0246] 7. Thickness of base coating

[0247] Place the polished copper foil on a flat table, with the foil extending about 5cm beyond the table. Press down on the copper foil on the table to prevent it from moving.

[0248] Open the micrometer and reset it to zero. The micrometer was purchased from Mitutoyo Co., Ltd. of Japan.

[0249] Test at different positions of the copper foil in sequence, take the average value of five points and record it as L1;

[0250] After gravure coating and drying on one side of the copper foil, place it on a flat table. The copper foil should extend about 5 cm beyond the table. The copper foil on the table should be pressed to prevent it from moving.

[0251] Open the micrometer and reset it to zero;

[0252] Test at different positions of the copper foil in sequence, take the average value of five points and record it as L2;

[0253] Thickness of the primer layer = (L2 - L1).

[0254] 3. Results Analysis

[0255] Table 1 Preparation parameters and results of examples and comparative examples

[0256]

[0257]

[0258] Table 2 Preparation parameters and results of examples and comparative examples

[0259]

[0260]

[0261] As shown in Table 1, the binders in Examples 1-18 are all fluoropolymers comprising structural units derived from vinylidene fluoride and structural units derived from acrylates. The molar content of the structural units derived from vinylidene fluoride in the polymers is 70% to 90%, based on the total molar number of structural units in the fluoropolymers. The use of these fluoropolymers as binders has achieved good results. Compared to the polyvinylidene fluoride in Comparative Example 1, the fluoropolymers provided in this application reduce the viscosity of the slurry and improve filterability, making them suitable for preparing primers.

[0262] From the comparison of Examples 1-3 with Comparative Examples 3 and 4, it can be seen that when the molar content of the structural units derived from acrylate in the fluoropolymer is 10% to 30% based on the total molar content of all structural units in the fluoropolymer, the viscosity of the fluoropolymer is appropriate, which can comprehensively improve the processability and adhesion of the slurry, taking into account the processing performance and performance of the primer layer.

[0263] From the comparison of Examples 4-7, it can be seen that when the weight average molecular weight of the fluoropolymer is 400,000 to 500,000, the viscosity of the fluoropolymer is appropriate, which can comprehensively improve the processability and adhesion of the slurry, taking into account the processing performance and performance of the primer layer.

[0264] It can be seen from Examples 8-11 that the mass fraction of the fluoropolymer is 0.5% to 5%. Based on the mass of the conductive agent, the viscosity of the fluoropolymer is appropriate and suitable for preparing a uniform primer layer. It can comprehensively improve the processability and adhesion of the slurry, taking into account the processing performance and use performance of the primer layer.

[0265] As can be seen from Examples 12-15, the viscosity of the primer slurry with a mass fraction of 0.5% to 5% of the fluoropolymer and a solid content of 15% to 30% is 100 mPa·s-1000 mPa·s, which means that the primer slurry prepared from the fluoropolymer does not require the addition of additional dispersants or thickeners to improve processing performance, which helps to reduce the variability between slurry batches, improve production efficiency, and optimize the production process.

[0266] From the comparison of Examples 1-16 and Example 18, it can be seen that the fluorine-containing polymers prepared by the method disclosed in the present application can more effectively improve the stability of the slurry, expand the process window of the slurry coating, and improve the processing performance of the slurry compared to the fluorine-containing copolymers synthesized by traditional methods.

[0267] From the comparison between Examples 1-16 and Example 17, it can be seen that the primer layer prepared by gravure coating has higher adhesion than the primer layer prepared by the doctor blade method commonly used in the prior art.

[0268] From the comparison of Examples 1-16 and Comparative Example 2, it can be seen that the base coating layer prepared by gravure coating in the present application has comparable electrode bonding strength to the base coating layer prepared by gravure coating using a slurry containing a traditional binder in the prior art, showing excellent application prospects.

[0269] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A fluorine-containing polymer, characterized in that It comprises a structural unit derived from a monomer represented by formula I and a structural unit derived from a monomer represented by formula II, wherein the molar content of the structural unit derived from the monomer represented by formula I is 70% to 90%, based on the total molar number of the fluorinated polymer. wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or fluorine-substituted C 1-3 Alkyl, R4, R5, R6 are each independently selected from hydrogen or substituted or unsubstituted C 1-5 Alkyl, R7 is selected from substituted or unsubstituted C 1-9 alkyl.

2. The fluorinated polymer according to claim 1, wherein R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine, and trifluoromethyl, and R5 and R6 are each independently selected from one or two of hydrogen and methyl.

3. The fluorinated polymer according to claim 1 or 2, characterized in that The molar content of the structural unit derived from the monomer represented by formula II is 10% to 30%, based on the total molar number of the structural units of the fluorine-containing polymer.

4. The fluorinated polymer according to any one of claims 1 to 3, characterized in that The weight average molecular weight of the fluorine-containing polymer is 400,000 to 500,000.

5. The fluorine-containing polymer according to claim 1, characterized in that The monomer represented by formula I is selected from one or more of vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.

6. The fluorinated polymer according to any one of claims 1 to 5, characterized in that The monomer represented by formula II is selected from one or more of methyl acrylate, ethyl acrylate, butyl acrylate, isoamyl acrylate, isooctyl acrylate, methyl methacrylate, ethyl methacrylate, hydroxyethyl acrylate, and hydroxypropyl acrylate.

7. A method for preparing a fluorine-containing polymer, characterized in that: The following steps are involved: Under polymerizable conditions, at least one monomer represented by formula I and at least one monomer represented by formula II are polymerized, wherein the molar content of the monomer represented by formula I is 70% to 90%, based on the total moles of the monomer represented by formula I and the monomer represented by formula II. wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or fluorine-substituted C 1-3 Alkyl, R4, R5, R6 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 Alkyl, R7 is selected from substituted or unsubstituted C 1-9 alkyl.

8. The preparation method according to claim 7, characterized in that R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine, and trifluoromethyl, and R5 and R6 are each independently selected from one or two of hydrogen and methyl.

9. The preparation method according to claim 7 or 8, characterized in that The molar content of the monomer represented by formula II is 10% to 30%, based on the total molar number of the monomer represented by formula I and the monomer represented by formula II.

10. The preparation method according to any one of claims 7 to 9, characterized in that The polymerization reaction includes a first stage polymerization and a second stage polymerization, First stage polymerization: adding an initiator, a first emulsifier, at least one monomer represented by formula I and an aqueous medium into a reaction vessel to carry out first stage polymerization, and continuously feeding the monomer represented by formula I into the first stage polymerization; Second stage polymerization: After a period of reaction, an initiator, a second emulsifier, at least one monomer represented by formula II and an aqueous medium are added to the reaction vessel to carry out a second stage polymerization, in which the monomer represented by formula I is continuously fed.

11. The preparation method according to claim 10, characterized in that: The mass of the monomer of formula I introduced into the first stage polymerization is 90% to 95% of the total mass of the monomer of formula I supplied in the polymerization reaction, and the mass of the monomer of formula I introduced into the second stage polymerization reaction is 5% to 10% of the total mass of the monomer of formula I supplied in the polymerization reaction.

12. The preparation method according to claim 10 or 11, characterized in that: The initiator provided in the first stage polymerization and the initiator provided in the second stage polymerization are both persulfates. The mass percentage of the initiator provided in the first stage polymerization is 0.05% to 0.1%, based on the total mass of the monomer represented by formula I and the monomer represented by formula II; the mass percentage of the initiator provided in the second stage polymerization is 0.05% to 0.1%, based on the mass of the monomer represented by formula II.

13. The preparation method according to any one of claims 10 to 12, characterized in that The mass percentage of the first emulsifier is 0.2% to 0.7%, based on the total mass of the monomer represented by formula I and the monomer represented by formula II.

14. The preparation method according to any one of claims 10 to 13, characterized in that The mass percentage of the second emulsifier is 0.5% to 1.5%, based on the mass of the monomer represented by formula II.

15. The preparation method according to any one of claims 10 to 14, characterized in that The mass percentage of the aqueous medium provided in the first stage polymerization is 200% to 500%, and the mass percentage of the aqueous medium provided in the second stage polymerization is 100% to 200%, based on the total mass of the monomer represented by formula I and the monomer represented by formula II.

16. The preparation method according to any one of claims 10 to 15, characterized in that The reaction pressure of the first stage polymerization is 5.5-7.5 MPa, and the reaction temperature is 75°C-85°C.

17. The preparation method according to any one of claims 10 to 16, characterized in that The reaction pressure of the second stage polymerization is 4.5-6.5 MPa, and the reaction temperature is 86° C.-95° C.

18. The preparation method according to any one of claims 10 to 17, characterized in that After the reaction has proceeded for a period of time, providing an initiator, a second emulsifier, at least one monomer represented by Formula II, and an aqueous medium into the reaction container for a second stage polymerization, comprising: After adding the initiator into the reaction container, a premixed solution comprising the initiator, a second emulsifier, at least one monomer represented by formula II and an aqueous medium is added.

19. The preparation method according to any one of claims 10 to 18, characterized in that The first emulsifier is an alkali metal perfluorooctanoate.

20. The preparation method according to any one of claims 10 to 19, characterized in that The second emulsifier is one or both of polyoxyethylene-4-phenol ether ammonium sulfate and nonylphenol polyoxyethylene ether ammonium sulfate.

21. Use of the fluorine-containing polymer according to any one of claims 1 to 6 in a secondary battery.

22. A primer slurry comprising a binder, a conductive agent and a solvent, characterized in that: The binder comprises the fluorine-containing polymer according to any one of claims 1 to 6.

23. The primer slurry according to claim 22, characterized in that: The mass fraction of the binder is 0.5% to 5%, based on the mass of the conductive agent.

24. The primer slurry according to claim 22 or 23, characterized in that: The solid content of the primer slurry is 15% to 30%, and the viscosity of the primer slurry is 100 mPa·s to 1000 mPa·s.

25. The primer slurry according to any one of claims 22 to 24, characterized in that The solvent is an organic solvent.

26. The primer slurry according to any one of claims 22 to 25, characterized in that The solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylpropionamide, N,N-diethylpropionamide, N,N-dipropylpropionamide, N,N-dibutylpropionamide, N,N-dimethylethylpropionamide and 3-butoxy-N-methylpropionamide.

27. A method for preparing a primer layer, characterized in that: The following steps are involved: The primer slurry according to any one of claims 22 to 26 is gravure coated on the surface of the current collector; and the primer slurry is dried to obtain a primer layer.

28. A secondary battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, and the negative electrode sheet comprises a primer layer prepared by the preparation method according to claim 27.

29. The secondary battery according to claim 28, characterized in that The secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.

30. A battery module, characterized in that: Includes the secondary battery according to claim 28 or 29.

31. A battery pack, characterized in that: The invention comprises at least one of the secondary battery according to claim 28 or 29 and the battery module according to claim 30.

32. An electrical device, characterized in that: The battery comprises at least one selected from the secondary battery according to claim 28 or 29, the battery module according to claim 30, or the battery pack according to claim 31.