Electrolytic capacitor

By using a combination of self-doped conductive polymers and specific solvents in electrolytic capacitors, and optimizing the anode foil and dielectric layer structures, the problem of initial value and long-term change of ESR in electrolytic capacitors is solved, achieving low ESR and high stability. of electrolytic capacitors.

CN118765428APending Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023914.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-28
Filing Date
2023-02-20
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing electrolytic capacitors perform poorly in terms of initial ESR (equivalent series resistance) and change in ESR over time (ΔESR), making it difficult to simultaneously suppress low initial ESR and long-term stability of ESR.

Method used

A liquid component containing a self-doping conductive polymer and a specific alkylene glycol or oxyalkylene glycol is used. By combining these solvents with the conductive polymer, the dissolution of the conductive polymer is suppressed and the conductive path is maintained. , combined with appropriate anode foil and dielectric layer structures, reduce the initial value and long-term changes of ESR.

Benefits of technology

It effectively suppresses the initial ESR and ESR changes over time of the electrolytic capacitor, improves the stability of the conductivity and capacity, and enhances the reliability of the electrolytic capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765428A_ABST
    Figure CN118765428A_ABST
Patent Text Reader

Abstract

The electrolytic capacitor includes a capacitor element and a liquid component. The capacitor element includes an anode foil having a dielectric layer on a surface thereof, and a conductive polymer component in contact with at least a portion of the dielectric layer. The conductive polymer component contains a self-doped conductive polymer. The liquid component contains at least one solvent selected from the group consisting of alkylene glycols having 4 or more carbon atoms and polyalkylene glycols having a repeating structure of oxyalkylene groups having 3 or more carbon atoms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to electrolytic capacitors. Background Art

[0002] The capacitor element contained in the electrolytic capacitor includes, for example, an anode body, a dielectric layer formed on the surface of the anode body, and a cathode portion covering at least a portion of the dielectric layer. The cathode portion includes a conductive polymer covering at least a portion of the dielectric layer. The conductive polymer is also called a solid electrolyte. For example, Patent Document 1 proposes using the following conductive polymer solution to form a solid electrolyte layer of a solid electrolytic capacitor, wherein the conductive polymer solution contains a conductive polymer, a polysulfonic acid or a salt thereof that functions as a dopant, a mixture of a polyacid and a carbon material, and a solvent.

[0003] As a small, large-capacity, and low-ESR (equivalent series resistance) capacitor, an electrolytic capacitor containing a capacitor element having a solid electrolyte layer and a liquid component such as an electrolyte in a shell is also considered promising. For example, Patent Document 2 proposes an electrolytic capacitor comprising a capacitor element, an electrolyte impregnated in the capacitor element, and an outer casing that seals the capacitor element and the electrolyte together, wherein the electrolyte contains a non-volatile solvent that is at least one of a polyalkylene glycol and a derivative of a polyalkylene glycol.

[0004] In addition, self-doping conductive polymers are sometimes used as solid electrolytes. For example, Patent Document 3 proposes a capacitor in which an anode body is at least partially coated with a solid electrolyte, wherein the solid electrolyte comprises a conductive polymer that has been heterogeneously doped, a counter ion that is not covalently bonded to the heterogeneously doped conductive polymer, and a self-doped conductive polymer.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2012 / 117994 (Claims 1, 13, and 16)

[0008] Patent Document 2: International Publication No. 2011 / 099261 (Claim 1)

[0009] Patent Document 3: Japanese Patent Application Publication No. 2021-36603 (Claim 14) Summary of the invention

[0010] Problems to be solved by the invention

[0011] Electrolytic capacitors are required to have a low initial ESR and a small change in ESR over time (ΔESR).

[0012] Means for solving problems

[0013] A first aspect of the present invention relates to an electrolytic capacitor comprising a capacitor element and a liquid component.

[0014] The capacitor element includes an anode foil having a dielectric layer on its surface and a conductive polymer component in contact with at least a portion of the dielectric layer.

[0015] The conductive polymer component includes a self-doping conductive polymer.

[0016] The liquid component contains at least one solvent selected from the group consisting of an alkylene glycol having 4 or more carbon atoms and a polyalkylene glycol containing a repeating structure of an oxyalkylene group having 3 or more carbon atoms.

[0017] Effects of the Invention

[0018] In an electrolytic capacitor, initial ESR and temporal change in ESR can be suppressed to be low. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a schematic cross-sectional view of an electrolytic capacitor according to one embodiment of the present invention.

[0020] Figure 2 Yes Figure 1 A schematic diagram of a portion of an expanded capacitor element of an electrolytic capacitor. DETAILED DESCRIPTION

[0021] The novel features of the present invention are described in the attached technical claims, but both the structure and content of the present invention, together with other objects and features of the present invention, can be better understood through the following detailed description with reference to the accompanying drawings.

[0022] In an electrolytic capacitor, for example, when a conductive polymer component (conjugated polymer and dopant, etc.) with high conductivity is used, it is advantageous in suppressing the initial ESR to be low. In addition, if the conductive polymer component is combined with an electrolyte, the degradation of the conductive polymer component is alleviated, so it is advantageous from the perspective of suppressing the increase of the ESR of the electrolytic capacitor. However, in the case where the conductive polymer component includes a conjugated polymer and a dopant, dedoping or decomposition of the conjugated polymer after dedoping occurs during repeated use of the electrolytic capacitor. Therefore, it is difficult to suppress the decrease in the conductivity of the conductive polymer component over time. Therefore, it is difficult to suppress the increase of ESR over time.

[0023] On the other hand, the self-doping conductive polymer has a conjugated polymer skeleton and a functional group (anionic group, etc.) that functions as a dopant and is directly or indirectly bonded to the skeleton by a covalent bond. Therefore, if a self-doping conductive polymer is used, high conductivity can be obtained, and it is difficult to use a conjugated polymer and a dopant, so it is also difficult to reduce the conductivity over time. Therefore, it is expected that the initial ESR and the time-varying ESR can be suppressed to be low. In a solid electrolytic capacitor, by using a self-doping conductive polymer, the initial ESR and the time-varying ESR can be suppressed to be low.

[0024] In this way, self-doping conductive polymer is a material with excellent performance. However, when the self-doping conductive polymer is combined with liquid components such as electrolyte, unlike the situation of solid electrolytic capacitors, the initial ESR cannot be suppressed to a low level sometimes, and the time-dependent change of ESR increases. Therefore, in the past, when using liquid components, even if self-doping conductive polymers are used, it is difficult to obtain an electrolytic capacitor with a performance of a practical level. It is believed that the initial increase and the increase over time of ESR when the self-doping conductive polymer is combined with the liquid component are caused by the dissolution of the self-doping conductive polymer in the liquid component. In the conductive polymer component comprising a conjugated polymer and a dopant, due to the presence of the dopant molecule, the orientation of the conjugated polymer is improved, and high crystallinity can be obtained, so the conductive polymer component becomes rigid. Even if such a rigid conductive polymer component contacts with the liquid component, it is not easy to dissolve. However, in the self-doping conductive polymer, the polymer chain is relatively soft, the positions of functional groups such as anionic groups are random, and the polymer chain has low orientation and low crystallinity. Therefore, it is believed that the self-doping conductive polymer is easily compatible with liquid components and easily eluted into the liquid components.

[0025] In view of the above, (1) an electrolytic capacitor comprises a capacitor element and a liquid component. The capacitor element comprises an anode foil having a dielectric layer on its surface and a conductive polymer component in contact with at least a portion of the dielectric layer. The conductive polymer component comprises a self-doped conductive polymer. The liquid component comprises at least one solvent selected from an alkylene glycol having 4 or more carbon atoms and a polyalkylene glycol having a repeating structure of an oxyalkylene having 3 or more carbon atoms.

[0026] Thus, in the electrolytic capacitor of the present invention, a conductive polymer component containing a self-doped conductive polymer and a liquid component containing at least one solvent (hereinafter referred to as the first solvent) selected from an alkylene glycol having a carbon number of 4 or more and a polyalkylene glycol having a repeating structure containing an oxyalkylene group having a carbon number of 3 or more are combined. By using a liquid component containing the first solvent, the dissolution of the self-doped conductive polymer into the liquid component can be suppressed despite the combination of the self-doped conductive polymer and the liquid component. Therefore, the conductive path in the conductive polymer component is maintained, and high conductivity can be obtained. In addition, the conductive polymer component can be fully swollen by using the first solvent, so that high conductivity can be ensured. As a result, the initial ESR and the time-dependent change of ESR (more specifically, the increase of ESR when the electrolytic capacitor is repeatedly used) can be suppressed to a low level.

[0027] (2) In the above (1), the mode value of the volume-based pore diameter of the anode foil having the dielectric layer may be 0.1 μm or more and 0.3 μm or less.

[0028] (3) In the above (1) or (2), the alkylene glycol may have 6 or less carbon atoms.

[0029] (4) In any one of the above (1) to (3), the alkylene glycol has a structure in which at least one carbon atom is interposed between carbon atoms to which two hydroxyl groups are respectively bonded.

[0030] (5) In any one of the above (1) to (4), the polyalkylene glycol may contain an oxy group C 3-4 Repeating structure of alkylene.

[0031] (6) In any one of the above (1) to (5), the weight average molecular weight of the polyalkylene glycol may be 400 or more.

[0032] (7) In any one of the above (1) to (6), the content of the solvent in the liquid component may be 30% by mass or more and 100% by mass or less.

[0033] (8) In any one of the above (1) to (7), the self-doping conductive polymer may have a conjugated polymer skeleton, and the conjugated polymer may have one or more and three or less anionic groups per molecule.

[0034] (9) In any one of the above (1) to (8), the self-doping conductive polymer may have a conjugated polymer skeleton including a monomer unit corresponding to the thiophene compound, and an anionic group introduced into the skeleton.

[0035] (10) In the above (9), the anionic group may be introduced into the skeleton via a linking group. The linking group may include an alkylene group having 2 or more carbon atoms.

[0036] (11) In any one of the above (1) to (10), the self-doping conductive polymer may contain at least a sulfone group.

[0037] (12) In any one of the above (1) to (11), the anode foil may include aluminum.

[0038] (13) In any one of (1) to (12) above, the capacitor element may include a cathode foil and a separator interposed between the anode foil and the cathode foil. The separator may be impregnated with the conductive polymer component.

[0039] The electrolytic capacitor of the present invention is described in more detail below, including the above (1) to (13).

[0040] At least one of (13) is combined with at least one of the following elements.

[0041] (Capacitor Components)

[0042] The capacitor element included in the electrolytic capacitor includes at least an anode foil having a dielectric layer on its surface and a conductive polymer component in contact with at least a portion of the dielectric layer.

[0043] (Anode Foil)

[0044] The anode foil may include valve metal, alloy containing valve metal, compound containing valve metal, etc. These materials may be used alone or in combination of two or more. As the valve metal, aluminum, tantalum, niobium, and titanium are preferably used, for example.

[0045] Among them, aluminum is cheap and lightweight, and can obtain high conductivity, so it is often used in the anode foil of capacitor elements. However, when using a liquid component, the anode foil containing aluminum is easily corroded by anionic groups contained in the conductive polymer component or acid components contained in the liquid component. In the present invention, even when using an anode foil containing aluminum, the dissolution of the anode foil can be suppressed and the corrosion can be suppressed. It is believed that this is because, by using a self-doping conductive polymer and the liquid component containing a first solvent, the dissolution of the self-doping conductive polymer in the liquid component is suppressed, the increase in the acidity of the liquid component is suppressed, and the excessive increase in the affinity of the liquid component to the anode foil is suppressed. The anode foil containing aluminum can contain aluminum metal, can contain aluminum alloy, or can contain both.

[0046] The anode foil may have a porous portion having pores on the surface. The anode foil having the porous portion is obtained by, for example, roughening the surface of a substrate (foil-shaped or plate-shaped substrate, etc.) containing a valve-acting metal by etching, etc. The roughening may be performed, for example, by electrolytic etching or chemical etching, etc.

[0047] (Dielectric layer)

[0048] The dielectric layer is formed by anodizing the valve action metal on the surface of the anode foil by chemical conversion treatment, etc. The dielectric layer may be formed so as to cover at least a portion of the anode foil.

[0049] The dielectric layer includes an oxide of a valve metal. For example, when tantalum is used as the valve metal, the dielectric layer includes Ta2O5, and when aluminum is used as the valve metal, the dielectric layer includes Al2O3. It should be noted that the dielectric layer is not limited to this, as long as it functions as a dielectric.

[0050] The dielectric layer is usually formed on the surface of the anode foil. When the dielectric layer is formed on the surface of the porous portion of the anode foil, the dielectric layer is formed along the inner wall surfaces of the pores of the porous portion or the depressions (pits) on the surface of the anode foil.

[0051] The mode value of the volume-based pore size of the anode foil having a dielectric layer can be, for example, greater than 0.1 μm and less than 0.5 μm. The mode value of the pore size can also be greater than 0.1 μm and less than 0.3 μm. In this case, the self-doped conductive polymer easily invades the pores formed in the anode foil having a dielectric layer, and a high capacity can be obtained. In addition, the self-doped conductive polymer becomes more difficult to dissolve, thereby reducing the time-dependent change in capacity. In addition, by maintaining the connection points between the particles of the self-doped conductive polymer, high conductivity is maintained, thereby further reducing the time-dependent change in ESR.

[0052] The mode value of the volume-based pore diameter of the anode foil having a dielectric layer is the mode value (modal diameter) when the pore diameter is measured for pores with a pore diameter of 10 μm or less in the volume-based pore diameter distribution measured using a mercury porosimeter. In the measurement of the pore diameter distribution using a mercury porosimeter, the anode foil is taken out from the capacitor element, the attached conductive polymer component is removed using a solvent (ethanol), and the anode foil thus obtained is cut into a predetermined size (5 mm in length × 5 mm in width), and the obtained sample is used.

[0053] (Conductive polymer component)

[0054] The conductive polymer component includes a self-doping conductive polymer. The conductive polymer component is in contact with at least a portion of the dielectric layer. The conductive polymer component in contact with the surface of the dielectric layer can constitute a layer (sometimes referred to as a conductive polymer layer). The conductive polymer component constitutes at least a portion of the cathode body in the electrolytic capacitor. The conductive polymer component can include at least one of other conjugated polymers (non-self-doping conjugated polymers, etc.) and dopants as needed. The conductive polymer component can include additives as needed.

[0055] Self-doping conductive polymers usually contain anionic groups. Examples of anionic groups include sulfonic groups, carboxyl groups, phosphoric acid groups, and phosphonic acid groups. In the conductive polymer component of the electrolytic capacitor, the anionic groups of the self-doping conductive polymer can be contained in any form such as anions, free groups, esters, and salts, and can also be contained in a form that interacts with or is complexed with the components contained in the conductive polymer component. In this specification, all forms thereof are referred to as anionic groups.

[0056] The self-doping conductive polymer may contain one anionic group or two or more. From the viewpoint of easily ensuring the higher conductivity of the self-doping conductive polymer, the self-doping conductive polymer may contain at least a sulfonic group. However, the self-doping conductive polymer containing a sulfonic group is easily dissolved in the liquid component due to the effect of the sulfonic group, and is easy to corrode the anode foil (anode foil containing aluminum, etc.). However, in the present invention, even in the case where the self-doping conductive polymer contains a sulfonic group, the dissolution of the self-doping conductive polymer in the liquid component can be suppressed by using a liquid component containing the first solvent. In addition, the corrosion of the anode foil can be suppressed.

[0057] The self-doping conductive polymer comprises a conjugated polymer skeleton and anionic groups introduced into the skeleton. It can be said that the skeleton of the self-doping conductive polymer is composed of a conjugated polymer. The number of anionic groups contained in the self-doping conductive polymer is, for example, 1 or more and 3 or less per molecule of the conjugated polymer constituting the skeleton of the self-doping conductive polymer, and can be 2 or 1.

[0058] As conjugated polymers constituting the skeleton of the self-doping conductive polymer, for example, polymers with polypyrrole, polythiophene, polyaniline, polyfuran, polyacetylene, polyphenylene, polyphenylene vinylene, polybenzone and polythiophene vinylene as the basic skeleton can be cited. The above-mentioned polymers only need to contain at least one monomer unit constituting the basic skeleton. The above-mentioned polymers also include homopolymers, copolymers of two or more monomers, and their derivatives (substitutents with substituents, etc.). For example, polythiophene includes poly (3,4-ethylenedioxythiophene) and the like. The self-doping conductive polymer has anionic groups in the skeletons of these conjugated polymers. The anionic groups can be directly introduced into the skeleton of the conjugated polymer, or they can be introduced via a connecting group. As the connecting group, it is preferred to include a multivalent group (divalent group) of an alkylene group, etc. As the connecting group, for example, aliphatic multivalent groups (divalent groups, etc.) such as an alkylene group, -R 1 -XR 2 - group (X is oxygen or sulfur, R 1 and R 2 The same or different, is an alkylene group.). The number of carbon atoms of each alkylene group contained in the linking group is, for example, 1 or more and 10 or less, or 1 or more and 6 or less. The alkylene group may be linear or branched. From the viewpoint of easily achieving a balance between high swelling properties brought by the liquid component and inhibiting dissolution into the liquid component, the linking group preferably contains at least an alkylene group with a carbon number of 2 or more. The number of carbon atoms of such an alkylene group may be 2 or more (or 3 or more) and 10 or less, or 2 or more (or 3 or more) and 6 or less. For example, R 1 It may be an alkylene group having 1 to 6 carbon atoms, R 2 The alkylene group may be an alkylene group having 2 or more (or 3 or more) and 10 or less carbon atoms. However, the linking group is not limited to these.

[0059] The conjugated polymer constituting the skeleton of the self-doping conductive polymer may be polypyrrole, polythiophene or polyaniline. From the viewpoint of easily obtaining high conductivity and stability, the self-doping conductive polymer preferably has a skeleton of a conjugated polymer containing monomer units corresponding to a thiophene compound and a polymer having an anionic group introduced into the skeleton.

[0060] Examples of the thiophene compound include compounds having a thiophene ring and capable of forming a repeating structure of a corresponding monomer unit. The thiophene compound may be linked at the 2-position and the 5-position of the thiophene ring to form a repeating structure of a monomer unit.

[0061] The thiophene compound may have a substituent at at least one of the 3-position and the 4-position of the thiophene ring. The substituent at the 3-position and the substituent at the 4-position may be linked to form a ring condensed with the thiophene ring. Examples of the thiophene compound include thiophene which may have a substituent at at least one of the 3-position and the 4-position, and alkylene dioxythiophene compounds (such as ethylene dioxythiophene compounds). 2-4 Alkylenedioxythiophene compounds, etc.) The alkylenedioxythiophene compounds also include compounds having a substituent in the alkylene moiety.

[0062] As the substituent, an alkyl group (such as a methyl group or an ethyl group) is preferred. 1-4 Alkyl, etc.), alkoxy (methoxy, ethoxy, etc. C 1-4 alkoxy, etc.), hydroxyl, hydroxyalkyl (hydroxymethyl, etc. hydroxy C 1-4 alkyl, etc.), but are not limited to these. When the thiophene compound has two or more substituents, each substituent may be the same or different. The thiophene ring (in the alkylenedioxythiophene ring, at least one of the thiophene ring and the alkylene group) may have the above-mentioned anionic group or a group containing anionic groups (for example, sulfoalkyl, etc.) as a substituent.

[0063] The self-doping conductive polymer may have a skeleton of a conjugated polymer (PEDOT, etc.) containing at least a monomer unit corresponding to a 3,4-ethylenedioxythiophene compound (3,4-ethylenedioxythiophene (EDOT), etc.). The skeleton of the conjugated polymer containing at least a monomer unit corresponding to EDOT may contain only a monomer unit corresponding to EDOT, or may contain a monomer unit corresponding to a thiophene compound other than EDOT in addition to the monomer unit.

[0064] The weight average molecular weight (Mw) of the self-doping conductive polymer is not particularly limited, and may be, for example, 1,000 to 1,000,000, 1,000 to 100,000, or 5,000 to 50,000. The type or mixing ratio of the first solvent may be adjusted according to the Mw of the self-doping conductive polymer to adjust the balance between the dissolution suppression and high conductivity of the self-doping conductive polymer.

[0065] In this specification, the weight average molecular weight (Mw) is a value in terms of polystyrene measured by gel permeation chromatography (GPC). In general, GPC is measured using a polystyrene gel column and water / methanol (volume ratio 8 / 2) as a mobile phase.

[0066] The ratio of the self-doped conductive polymer contained in the conductive polymer component is, for example, 50% by mass or more, 75% by mass or more, or 90% by mass or more. The ratio of the self-doped conductive polymer contained in the conductive polymer component is 100% by mass or less. When the ratio of the self-doped conductive polymer in the conductive polymer component is relatively high, it is easier to ensure the high conductivity and high stability of the conductive polymer component. The conductive polymer component may also be composed of only the self-doped conductive polymer.

[0067] As other conductive polymers (non-self-doping conductive polymers, etc.) contained in the conductive polymer component, for example, conjugated polymers (non-self-doping conjugated polymers (for example, conjugated polymers without anionic groups), etc.) and dopants can be cited. As conjugated polymers, conjugated polymers exemplified as conjugated polymers constituting the main skeleton of self-doping conductive polymers can be cited. In the case where the conjugated polymer has a similar skeleton to the conjugated polymer constituting the main skeleton of the self-doping conductive polymer, high affinity is easily obtained. For example, a non-self-doping conjugated polymer containing a monomer unit of a thiophene compound can be combined with a self-doping conductive polymer having a main skeleton containing a monomer unit of a thiophene compound. As a thiophene compound corresponding to the monomer unit of the non-self-doping conjugated polymer, the thiophene compound described for the self-doping conductive polymer can be cited.

[0068] As a dopant, at least one selected from anions and polyanions (polymer anions, etc.) can be cited. As anions, for example, sulfate ions, nitrate ions, phosphate ions, borate ions, organic sulfonate ions, carboxylate ions, etc. can be cited. As a dopant that generates sulfonate ions, for example, p-toluenesulfonic acid and naphthalenesulfonic acid can be cited. From the viewpoint of easily obtaining higher stability, polymer anions can be used. As a polymer anion having a sulfonic group, for example, a high-molecular polysulfonic acid can be cited. As a specific example of a polymer anion, polyvinyl sulfonic acid, polystyrene sulfonic acid (PSS (also including copolymers and substitutes with substituents, etc.)), polyallyl sulfonic acid, polyacrylic sulfonic acid, polymethacrylic sulfonic acid, poly (2-acrylamide-2-methylpropanesulfonic acid), polyisoprene sulfonic acid, polyester sulfonic acid (aromatic polyester sulfonic acid, etc.), phenolsulfonic acid phenolic resin can be cited. However, the dopant is not limited to these specific examples.

[0069] The conductive polymer component (conductive polymer layer) formed into a layer may be a single layer or may be composed of a plurality of layers. When the conductive polymer layer is composed of a plurality of layers, the composition of the conductive polymer component contained in each layer (the type and amount of the self-doped conductive polymer, the type and amount of the conjugated polymer, the type and amount of the dopant, the type and amount of the additive, etc.) may be the same or different.

[0070] The conductive polymer component (or conductive polymer layer) is formed, for example, using a treatment liquid (also referred to as a liquid composition) containing a self-doped conductive polymer. For example, an anode foil having a dielectric layer, or a precursor of a capacitor element including an anode foil having a dielectric layer and a cathode body (for example, a wound body formed by winding an anode foil having a dielectric layer and a cathode foil with a separator) is immersed in the liquid composition and then dried, thereby forming a conductive polymer component (or conductive polymer layer) in contact with the dielectric layer.

[0071] The self-doping conductive polymer may be dissolved in the liquid composition or dispersed in the form of particles. The liquid composition may further contain other components (eg, other conjugated polymers, dopants, additives, etc.).

[0072] The liquid composition can be obtained, for example, by polymerizing (e.g., oxidative polymerization) a precursor of a self-doping conductive polymer in a liquid medium. The precursor may be at least one selected from monomers constituting the self-doping conductive polymer, oligomers formed by connecting several monomers, and prepolymers. When preparing the liquid composition, at least one of other conjugated polymers and dopants may coexist as needed.

[0073] As the liquid medium, for example, water and an organic liquid medium can be cited. The liquid medium is, for example, a medium that is liquid at room temperature (temperature above 20°C and below 35°C). As the organic liquid medium, for example, monohydric alcohols (methanol, ethanol, propanol, etc.), polyhydric alcohols (ethylene glycol, glycerol, etc.), or aprotic polar solvents (N,N-dimethylformamide, dimethyl sulfoxide, acetonitrile, acetone, benzonitrile, etc.) can be cited. The liquid composition can contain one liquid medium or two or more liquid media.

[0074] In the case where the liquid composition includes a particle-shaped self-doping conductive polymer, from the viewpoint of being easily filled into the holes of the porous portion, the average particle size of the particles of the self-doping conductive polymer can be less than 100nm, or less than 50nm. The lower limit of the average particle size is not particularly limited, for example, more than 0.5nm or more than 5nm. It should be noted that the average particle size referred to herein refers to the median particle size (D50) in the particle size distribution based on the volume. The average particle size of the self-doping conductive polymer can be obtained, for example, based on the particle size distribution based on the dynamic light scattering method (DLS). Specifically, an aqueous dispersion (for example, a liquid dispersion) of particles containing self-doping conductive polymers is used, and a dynamic light scattering method particle size distribution measuring device (HORIBA, LB-550) is used to measure the particle size distribution of the particles based on the volume, and the median particle size (D50) is used as the average particle size.

[0075] (Cathode)

[0076] A metal foil (cathode foil) can be used as the cathode body. The type of metal is not particularly limited, and for example, valve metals such as aluminum, tantalum, and niobium or alloys containing valve metals can be used. The surface of the metal foil can be roughened as needed. A chemical conversion film can be provided on the surface of the metal foil, and a film of a metal (dissimilar metal) or a non-metallic film different from the metal constituting the metal foil can also be provided. Examples of dissimilar metals and non-metals include metals such as titanium and non-metals such as carbon.

[0077] (Diaphragm)

[0078] A separator may be disposed between the cathode foil and the anode foil. The separator is not particularly limited, and for example, nonwoven fabrics containing fibers of cellulose, polyethylene terephthalate, vinylon, or polyamide (for example, aliphatic polyamide, aromatic polyamide such as aramid) may be used.

[0079] In the case where the capacitor element includes a diaphragm, the conductive polymer component may be impregnated in the diaphragm. The conductive polymer component may be interposed between the anode foil and the cathode foil, and may contact at least a portion of the dielectric layer and at least a portion of the cathode foil. In the present invention, the high conductivity of the conductive polymer component can be obtained by combining the self-doped conductive polymer with the liquid component, and therefore, in these methods, the initial ESR and the change in ESR over time can also be suppressed to be low.

[0080] (other)

[0081] The electrolytic capacitor may be a wound type, a chip type or a stacked type. The electrolytic capacitor may have at least one capacitor element, or may have multiple capacitor elements. For example, the electrolytic capacitor may have a stack of two or more capacitor elements, or may have two or more wound capacitor elements. The composition or number of capacitor elements may be selected according to the type or purpose of the electrolytic capacitor.

[0082] (Liquid ingredients)

[0083] The liquid component usually contains a non-aqueous solvent. The liquid component contains: at least one solvent (first solvent) selected from alkylene glycols having 4 or more carbon atoms and polyalkylene glycols containing a repeating structure of oxyalkylene having 3 or more carbon atoms. By containing the first solvent in the liquid component, the effect of swelling the conductive polymer component by the liquid component can be obtained, and the dissolution of the self-doped conductive polymer in the liquid component can be suppressed. Since the high conductivity of the conductive polymer component can be ensured, the initial ESR and the change of ESR over time can be suppressed to be low.

[0084] Polyalkylene glycol also includes copolymers having two or more oxyalkylene units, adducts obtained by adding alkylene oxide having 3 or more carbon atoms to alkylene glycol (wherein the alkylene moiety of the alkylene glycol and the alkylene moiety of the alkylene oxide have different structures), etc. The alkylene moiety contained in the first solvent may be linear or branched.

[0085] Examples of the alkylene glycol having 4 or more carbon atoms include butanediol (1,2-butanediol, 1,3-butanediol, 2,3-butanediol, 1,4-butanediol, etc.), pentanediol (1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 1,5-pentanediol, etc.), hexanediol (3-methyl-2,4-pentanediol, 1,2-hexanediol, 1,3-hexanediol, 1,4-hexanediol, 1,6-hexanediol, etc.), dihydroxyoctane (2-ethyl-1,3-hexanediol, 1,2-dihydroxyoctane, 1,8-dihydroxyoctane, etc.), dihydroxynonane (2-methyl-1,8-dihydroxyoctane, 1,9-nonanediol, etc.), and dihydroxydecane. The alkylene glycol may have 4 or more and 10 or less carbon atoms, or 4 or more and 8 or less carbon atoms. From the viewpoint of being easy to adjust the affinity with the conductive polymer component, being easy to make the conductive polymer component swell, and being easy to obtain a higher capacity, the number of carbon atoms of the alkylene glycol can be 4 or more and 6 or less. Each of the two hydroxyl groups of the alkylene glycol can be bonded to any one of the primary carbon atom, the secondary carbon atom, and the tertiary carbon atom contained in the alkylene moiety. In the alkylene glycol, at least one carbon atom can be interposed between the carbon atoms bonded with each hydroxyl group. In this case, the dipole force term δp becomes larger, and the swelling effect of the conductive polymer component is further improved, thereby further improving the conductivity.

[0086] The polyalkylene glycol contains an oxyalkylene group having 3 or more carbon atoms (oxy C 3-4 alkylene, etc.), and may contain oxyalkylene (oxy C 3-4 The number of carbon atoms in the oxyalkylene group may be 6 or less, or 4 or less. The oxyalkylene unit having 3 or more carbon atoms (oxyC 3-4 The ratio of the monomer units (such as alkylene units) in the total monomer units constituting the polyalkylene glycol may be 50 mol% or more, 70 mol% or more, or 90 mol% or more. Examples of such polyalkylene glycols include PPG, polytetramethylene glycol, polybutylene glycol (polyC 3-4 alkylene glycol, etc.), polyoxyethylene-polyoxypropylene copolymers (for example, copolymers containing 50 mol% or more of oxypropylene units in the total monomer units), propylene oxide adducts of ethylene glycol, propylene oxide adducts of alkylene glycols having 4 or more carbon atoms, C 2-3The butylene oxide adduct of alkylene glycol, the butylene oxide adduct of alkylene glycol having 5 or more carbon atoms, etc. The number of carbon atoms of the alkylene glycol to which the alkylene oxide is added is, for example, 10 or less, 8 or less, or 6 or less. The number of repetitions of the oxyalkylene unit in the polyalkylene glycol is, for example, 2 or more and 600 or less, 2 or more and 10 or less, or greater than 10 and 600 or less (for example, 100 or more and 600 or less). The number of alkylene oxide units in the alkylene oxide adduct may be 1 or more, and the total number of alkylene oxide units may be 2 or more. The total number of repetitions of the alkylene oxide units in the alkylene oxide adduct may be 2 or more and 50 or less, or 2 or more and 20 or less.

[0087] The Mw of the polyalkylene glycol is, for example, 1000 or less, 150 or more (or 200 or more) and 1000 or less, or 150 or more (or 200 or more) and 700 or less. When the Mw of the polyalkylene glycol is within such a range, the effect of suppressing the dissolution of the self-doping conductive polymer in the liquid component is improved. In addition, the effect of swelling the conductive polymer component is improved, and the film repairability of the dielectric layer and the conductivity of the conductive polymer component can be further improved.

[0088] The liquid component may include the first solvent and a non-aqueous solvent other than the first solvent (hereinafter referred to as the second solvent). As the second solvent, at least one of an alcoholic solvent, a sulfone compound, a lactone compound and a carbonate compound other than the first solvent may be cited. From the viewpoint of suppressing the dissolution of the self-doped conductive polymer and improving the effect of swelling the conductive polymer component, the ratio of the first solvent to the non-aqueous solvent contained in the liquid component is preferably 50% by mass or more, more preferably 75% by mass or more or 90% by mass or more. The ratio of the first solvent to the non-aqueous solvent is less than 100% by mass. The non-aqueous solvent may also be constituted by only the first solvent.

[0089] The content of the first solvent in the liquid component is, for example, more than 30% by mass, and can be more than 50% by mass or more than 55% by mass. When the content of the first solvent is in such a range, the effect of suppressing the dissolution of the self-doped conductive polymer in the liquid component and the effect of swelling the conductive polymer component are further improved. The content of the first solvent in the liquid component can be less than 100% by mass, and considering the concentration of solutes and additives, it can be, for example, less than 85% by mass or less than 75% by mass. These lower limits and upper limits can be combined arbitrarily. The content of the first solvent in the liquid component can be, for example, more than 30% by mass and less than 100% by mass, or more than 50% by mass (or more than 55% by mass) and less than 100% by mass. Within these ranges, the upper limit can also be changed to the above range.

[0090] The alcohol solvent as the second solvent includes monohydric alcohol and polyhydric alcohol. From the viewpoint of easily obtaining high repairability of the dielectric layer, the alcohol solvent may include at least polyhydric alcohol. As the polyhydric alcohol, diol compounds other than the first solvent, glycerol compounds, sugar alcohol compounds, etc. may be cited.

[0091] As the diol compound, in addition to the first solvent, alkylene glycol, polyalkylene glycol, alkylene oxide adducts of polyols, etc. can be mentioned. As the alkylene glycol, ethylene glycol (EG), propylene glycol (PG), trimethylene glycol (C 2-3 Alkylene glycol, etc.) etc. Alkylene glycol may be either linear or branched. Examples of polyalkylene glycol include diethylene glycol, triethylene glycol, polyethylene glycol (PEG) etc. Examples of alkylene oxide adducts of polyols include C 2-4 Alkylene oxide adducts (ethylene oxide adducts, propylene oxide adducts, etc.), also including poly C 2-4 Alkylene oxide adducts (polyethylene oxide adducts, etc.). As polyols to which alkylene oxide is added, in addition to trimethylolpropane, sugar alcohols (glycerol, erythritol, mannitol, pentaerythritol, etc.) can also be mentioned. The number of repetitions of the oxyalkylene units in the polyalkylene glycol, the number of alkylene oxide units in the addition part in the alkylene oxide adduct, or the total number of repetitions of the alkylene oxide units in the addition part can be selected from the above ranges described for the first solvent.

[0092] Examples of the glycerol compound include glycerol and polyglycerol (diglycerol, triglycerol, etc.). The number of repetitions of the glycerol unit in the polyglycerol is, for example, 2 to 20, and may be 2 to 10. Examples of the sugar alcohol compound include sugar alcohols (erythritol, mannitol, pentaerythritol, etc.).

[0093] Examples of the sulfone compound include sulfolane (SL), dimethyl sulfoxide, and diethyl sulfoxide. Examples of the lactone compound include γ-butyrolactone (GBL), γ-valerolactone, and the like. Examples of the carbonate compound include dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, and fluoroethylene carbonate.

[0094] When the liquid component includes the first solvent and the second solvent, using the second solvent including at least one selected from sulfone compounds and lactone compounds is advantageous in suppressing the temporal change of ESR compared to using an alcohol-based second solvent.

[0095] The qualitative and quantitative analysis of each solvent in the non-aqueous solvent can be performed by GC-MS analysis using a liquid component. The GC-MS analysis can be performed under the following conditions.

[0096] Device: GCMS-QP2010 (manufactured by Shimadzu Corporation)

[0097] Sample volume: 1 μL

[0098] Column: DB-WAX (length 30m, inner diameter 0.25mm, adsorbent film thickness 0.25μm, heat resistance upper limit temperature 260℃)

[0099] Heating process: 50℃ for 1 minute → heating at 10℃ / min to 250℃ → 250℃ for 20 minutes

[0100] Ion beam source temperature setting: 200°C

[0101] Interface temperature: 250℃

[0102] (Solute)

[0103] The liquid component may contain a solute. Examples of the solute include an acid component and an alkali component.

[0104] Examples of the acid component include acids having a carbonyl oxygen bond (carboxylic acid, oxycarbonic acid, Michaelis acid, etc.), coordination compounds of acids or phenol compounds having a carbonyl oxygen bond, phenol compounds (picric acid, p-nitrophenol, pyrogallol, catechol, etc.), sulfur-containing acids (sulfuric acid, sulfonic acid (aromatic sulfonic acid, etc.), oxyaromatic sulfonic acid (phenol-2-sulfonic acid, etc.), compounds having a sulfonimide bond, boron-containing acids (boric acid, halogenated boric acid (tetrafluoroboric acid, etc.), or partial esters thereof), phosphorus-containing acids (phosphoric acid, halogenated phosphoric acid (hexafluorophosphoric acid, etc.), phosphonic acid, phosphinic acid, or partial esters thereof), nitrogen-containing acids (nitric acid, nitrous acid, etc.), and p-nitrobenzene. Examples of the above-mentioned carboxylic acids include aliphatic carboxylic acids, aromatic carboxylic acids (including sulfoaromatic carboxylic acids (p-sulfobenzoic acid, 3-sulfophthalic acid, 5-sulfosalicylic acid, etc.)), and the like. From the aspect of high stability, aromatic carboxylic acids (particularly aromatic hydroxy acids (benzoic acid, salicylic acid, etc.), aromatic polycarboxylic acids (phthalic acid, pyromellitic acid, etc.) are preferred. Examples of compounds having a sulfonyl imide bond include saccharin, 1,2-benzenedisulfonyl imide, cyclohexafluoropropane-1,3-bis(sulfonyl)imide, 4-methyl-N-[(4-methylphenyl)sulfonyl]benzenesulfonamide, dibenzenesulfonyl imide, trifluoromethanesulfonyl anilide, N-[(4-methylphenyl)sulfonyl]acetamide, benzenesulfonyl anilide, N,N'-diphenylsulfamide, etc. Examples of the above-mentioned coordination compound include coordination compounds formed by bonding at least one central atom selected from boron, aluminum, and silicon to an acid having a carbonyl oxygen bond on the central atom. As a specific example of the coordination compound, boron disalicylic acid, boron dioxalic acid, boron diglycolic acid, boron digallic acid, boron dicatechin, and boron dipyrogallol can be cited. The liquid component can contain one acid component, or it can contain two or more. Among the acid components, aromatic carboxylic acids (phthalic acid, salicylic acid, benzoic acid, etc.) and the above-mentioned coordination compounds (boron disalicylic acid, boron dioxalic acid, boron diglycolic acid, etc.) are preferred, among which phthalic acid, salicylic acid, boron disalicylic acid, etc. are preferred.

[0105] The acid component may be contained in the liquid component in a free form, in a form of anions, or in a form of salts. Sometimes, all of these forms are referred to as the acid component.

[0106] The liquid component may contain an alkali component together with the acid component. At least a portion of the acid component is neutralized by the alkali component. Therefore, the concentration of the acid component can be increased and corrosion of the electrode caused by the acid component can be suppressed.

[0107] Examples of the alkaline component include ammonia, amines (specifically, primary amines, secondary amines, and tertiary amines), quaternary ammonium compounds, and amidinium compounds. The liquid component may contain one type of alkaline component, or two or more types.

[0108] Amines may be any of aliphatic, aromatic and heterocyclic. Examples of amines include trimethylamine, diethylamine, ethyldimethylamine, triethylamine, ethylenediamine, aniline, pyrrolidine, imidazole (1,2,3,4-tetramethylimidazolinium, etc.), and 4-dimethylaminopyridine. Examples of quaternary ammonium compounds include amidine compounds (including imidazole compounds).

[0109] The liquid component may contain the alkali component in a free form, in a cationic form, or in a salt form. All of these forms may be referred to as the alkali component.

[0110] The molar ratio of the total amount of the acid component to the base component (=acid component / base component) may be, for example, 0.5 or more (or 1 or more) and 50 or less, or 1.1 or more (or 1.5 or more) and 20 or less.

[0111] From the viewpoint of further facilitating the suppression of dissolution of the self-doped conductive polymer, the pH of the liquid component may be 1 to 4, or 1 to 3.5.

[0112] From the viewpoint of ensuring the high dissociation of the solute in the liquid component and easily obtaining the high film repairability of the dielectric layer, the concentration of the solute in the liquid component can be 0.1 mass % or more and 25 mass % or less, or 0.5 mass % or more and 25 mass % or less (or 15 mass % or less). It should be noted that the concentration of the acid component is not converted into anions or salts, but is converted into free acids to obtain. Similarly, the concentration of the alkali component is not converted into cations or salts, but is converted into free bases to obtain.

[0113] (other)

[0114] In the capacitor element, one end of the cathode lead terminal is electrically connected to the cathode body. One end of the anode lead terminal is electrically connected to the anode body. Each lead terminal can be joined to an electrode (metal foil, etc.) by welding or by a conductive adhesive.

[0115] The electrolytic capacitor is made by accommodating the capacitor element and the liquid component in a shell or an outer body. For example, the capacitor element and the liquid component can be accommodated in a bottom shell, and the opening of the bottom shell is sealed with a sealant, thereby forming an electrolytic capacitor. At this time, the other end of the anode lead terminal and the other end of the cathode lead terminal are respectively led out from the shell or the outer body. The other end of each terminal exposed from the shell or the outer body is used for welding connection with the substrate on which the electrolytic capacitor should be mounted.

[0116] Hereinafter, the electrolytic capacitor of the present invention will be described in more detail based on the embodiments. However, the electrolytic capacitor of the present invention is not limited to the following embodiments.

[0117] Figure 1 is a schematic cross-sectional view of an electrolytic capacitor according to this embodiment, Figure 2 FIG. 1 is a schematic diagram showing a portion of a capacitor element of the electrolytic capacitor after expansion.

[0118] The electrolytic capacitor includes, for example, a capacitor element 10, a bottomed case 101 that accommodates the capacitor element 10 and a liquid component (not shown), a sealing member 102 that blocks an opening of the bottomed case 101, a seat plate 103 that covers the sealing member 102, leads 104A and 104B that are led out from the sealing member 102 and pass through the seat plate 103, and lead terminals 105A and 105B that connect the leads to electrodes of the capacitor element 10. The vicinity of the opening end of the bottomed case 101 is drawn inward, and the opening end is curled to be tightly pressed against the sealing member 102.

[0119] The capacitor element 10 is, for example, Figure 2 The winding body shown. The winding body includes an anode foil 11 connected to a lead connector 105A, a cathode foil 12 connected to a lead connector 105B, and a separator 13. The anode foil 11 and the cathode foil 12 are wound with the separator 13 interposed therebetween. The outermost periphery of the winding body is fixed by a stopper tape 14. It should be noted that Figure 2 The diagram shows a state where a part of the wound body is unwound before the outermost periphery of the wound body is fixed.

[0120] In the capacitor element 10, a dielectric layer (not shown) is formed on at least a portion of the surface of the anode foil 11. A separator 13 and a conductive polymer component (not shown) are interposed between the anode foil 11 and the cathode foil 12. The conductive polymer component is in contact with at least a portion of the dielectric layer. In addition, the conductive polymer component is in contact with at least a portion of the cathode foil 12. Furthermore, the conductive polymer component and the separator are impregnated with a liquid component.

[0121] [Example]

[0122] Hereinafter, the present invention will be specifically described based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0123] 《Production of Electrolytic Capacitors E1 to E10 and C1 to C4》

[0124] A wound electrolytic capacitor (diameter 8 mm×L (length) 10 mm) having a rated voltage of 35 V and a rated electrostatic capacitance of 150 μF was produced. A specific method for producing the electrolytic capacitor will be described below.

[0125] (Preparation of anode foil)

[0126] An aluminum foil having a thickness of 100 μm was etched to roughen the surface of the aluminum foil. Then, a dielectric layer was formed on the surface of the aluminum foil by chemical conversion treatment. The chemical conversion treatment was performed by immersing the aluminum foil in an ammonium adipate solution and applying a voltage of 60 V thereto. Then, the aluminum foil was cut to prepare an anode foil.

[0127] (Preparation of cathode foil)

[0128] An aluminum foil having a thickness of 50 μm was subjected to etching treatment to roughen the surface of the aluminum foil, and then the aluminum foil was cut to prepare a cathode foil.

[0129] (Production of wound body)

[0130] The anode lead connector and the cathode lead connector are connected to the anode foil and the cathode foil, and the anode foil and the cathode foil are wound through the diaphragm while the lead connector is wound in. The anode lead and the cathode lead are respectively connected to the ends of each lead connector protruding from the wound body. The prepared wound body is subjected to chemical conversion treatment again, and a dielectric layer is formed at the cut end of the anode foil. Next, the end of the outer surface of the wound body is fixed with a stop tape to prepare the wound body.

[0131] (Preparation of liquid composition)

[0132] An aqueous dispersion (liquid composition) containing a self-doping polythiophene polymer is prepared. The concentration of the polythiophene polymer in the liquid composition is 4% by mass. The particles of the polythiophene polymer are very small particles with a particle size of less than 1 nm. As the self-doping polythiophene polymer, PEDOT (Mw: about 10,000) having a sulfonic group bonded to the PEDOT skeleton via a linking group containing a butenyl group is used.

[0133] In addition, in Comparative Example 4, an aqueous dispersion containing PEDOT doped with PSS (concentration: 4 mass %) was used instead of an aqueous dispersion containing a self-doping polythiophene-based polymer.

[0134] (Formation of Solid Electrolyte)

[0135] In a reduced pressure atmosphere (40 kPa), the wound body is immersed in a liquid mixture contained in a predetermined container for 5 minutes, and then the wound body is lifted from the liquid mixture. Next, the wound body impregnated with the liquid mixture is dried in a drying furnace at 150°C for 20 minutes, thereby configuring a conductive polymer component (solid electrolyte) containing a self-doped polythiophene polymer between the anode foil and the cathode foil having a dielectric layer. The conductive polymer component contacts at least a portion of the dielectric layer and at least a portion of the cathode foil, and is impregnated in the diaphragm. Thus, a capacitor element is formed.

[0136] (Preparation of liquid component (electrolyte))

[0137] The solvent and solute shown in Table 1 were mixed so that the content of each component in the liquid component became the value shown in Table 1. As the solute, triethylamine phthalate (salt) was used. It should be noted that the total of the solvent and the solute was 100% by mass. In this way, a liquid component (electrolyte) was prepared.

[0138] (Assembly of electrolytic capacitors)

[0139] In a reduced pressure atmosphere (40 kPa), the above-mentioned winding body formed with a conductive polymer component (solid electrolyte) is immersed in a liquid component for 5 minutes. Thus, a capacitor element impregnated with a liquid component is obtained. The obtained capacitor element is accommodated in a housing, and the opening of the housing is sealed with a sealing body. Thus, the Figure 1 The electrolytic capacitor shown in FIG. 1 was then aged at 130° C. for 2 hours while a rated voltage was applied to the electrolytic capacitor. An elastic member made of butyl rubber was used as a sealing member.

[0140] [Evaluation: Measurement of ESR and electrostatic capacitance]

[0141] In an environment of 20°C, using a 4-terminal LCR meter, the ESR (mΩ) of each electrolytic capacitor at a frequency of 100kHz and the electrostatic capacitance (μF) at a frequency of 120Hz were measured. In addition, the average value of the ESR (initial ESR) and the average value of the electrostatic capacitance Cap (initial Cap) of the 20 electrolytic capacitors were obtained.

[0142] Next, the electrolytic capacitor is placed in a thermostatic chamber at 145°C and maintained for 500 hours with the rated voltage applied, thereby performing an accelerated test. Then, the ESR and Cap are measured at 20°C in the same steps as the initial ESR and Cap, and the average values ​​of 20 solid electrolytic capacitors (ESR and Cap after the accelerated test) are calculated. The ESR after the accelerated test is measured, and the difference in change relative to the initial ESR is calculated (ΔESR = ESR after the accelerated test - initial ESR). In addition, the ratio of the Cap after the accelerated test to the initial Cap (= Cap after the accelerated test / initial Cap × 100 (%)) is calculated as the Cap change rate. The Cap change rate is an indicator of the change of Cap over time. The initial ESR, the ESR after the accelerated test, and the Cap change rate are respectively expressed as ratios when the values ​​of Comparative Example 1 are set to 100.

[0143] [Evaluation: Mode of Pore Diameters of Anode Foil Having Dielectric Layer]

[0144] For the anode foil having a dielectric layer taken out from one arbitrarily selected capacitor element, the mode value of the volume-based pore diameters is determined according to the above-described procedure.

[0145] The evaluation results are shown in Table 1. In the table, E1 to E10 are Examples, and C1 to C4 are Comparative Examples.

[0146] [Table 1]

[0147]

[0148] As shown in Table 1, when ethylene glycol or diethylene glycol is used as the second solvent instead of the first solvent, the initial ESR and the ESR after the accelerated test (i.e., ΔESR) are both very large values ​​(C1, C2). It is believed that this is because the conductive polymer component dissolves into the liquid component from the initial stage, the conductivity of the conductive polymer component decreases, and the conductive polymer component continues to dissolve in the liquid component during the accelerated test, thereby reducing the conductivity. In addition, for C3 in which γ-butyrolactone is used as the second solvent instead of the first solvent, although ΔESR is suppressed to a low level, the initial ESR becomes higher. It is believed that this is because the conductive polymer component is not easily swelled by the liquid component, so that the conductivity of the conductive polymer component in the initial stage decreases.

[0149] In contrast, in the examples using the liquid component containing the first solvent, both the initial ESR and the ESR after the accelerated test (ΔESR) were suppressed to be low (E1 to E10). It is believed that this is because the conductive polymer component is fully swollen by the liquid component, high conductivity can be obtained, and the dissolution of the conductive polymer component into the liquid component during the accelerated test is suppressed. On the other hand, even in the case of using the liquid component containing the first solvent, in C4 where the conductive polymer component does not contain a self-doped conductive polymer, although the initial ESR and ΔESR are suppressed to be low compared to C1 and C2, the ΔESR and capacity change rate are insufficient compared to E1 to E10. It is believed that the reason why the ΔESR in C4 is large and the capacity change rate is low compared to E1 to E10 is that dedoping occurs due to the accelerated test, thereby deteriorating the conductive polymer and reducing the conductivity of the solid electrolyte layer.

[0150] In addition, in the examples, when the volume-based pore diameter mode of the anode foil having the dielectric layer is 0.1 μm or more and 0.3 μm or less, there is a tendency that a relatively high capacity can be obtained even after the accelerated test. This is believed to be because the conductive polymer component easily penetrates into the fine recessed portions on the surface of the dielectric layer, and the dissolution of the conductive polymer component during the accelerated test is suppressed.

[0151] The preferred embodiments of the present invention are described, but such disclosure is not interpreted restrictively. By reading the above disclosure, various deformations and changes are undoubtedly obvious to those skilled in the art of the technical field to which the present invention belongs. Therefore, the scope of the attached claims should be interpreted as including all deformations and changes without departing from the true spirit and scope of the present invention.

[0152] Industrial Applicability

[0153] The electrolytic capacitor of the present invention can be used as a hybrid electrolytic capacitor. The ESR of the electrolytic capacitor changes little over time and has excellent reliability. Therefore, it is particularly suitable for applications requiring high reliability. However, the applications of the electrolytic capacitor are not limited to these.

[0154] Description of Reference Numerals

[0155] 100: Electrolytic capacitor

[0156] 101: Shell with bottom

[0157] 102: Sealed body

[0158] 103: Seat plate

[0159] 104A, 104B: Lead wire

[0160] 10SA, 105B: Lead connector

[0161] 10: Capacitor components

[0162] 11: Anode foil

[0163] 12: Cathode foil

[0164] 13: Diaphragm

[0165] 14: Stop tape

Claims

1. An electrolytic capacitor comprising a capacitor element and a liquid component, The capacitor element includes an anode foil having a dielectric layer on its surface and a conductive polymer component in contact with at least a portion of the dielectric layer. The conductive polymer component includes a self-doping conductive polymer, The liquid component includes at least one solvent selected from the group consisting of an alkylene glycol having 4 or more carbon atoms and a polyalkylene glycol including a repeating structure of an oxyalkylene group having 3 or more carbon atoms.

2. The electrolytic capacitor according to claim 1, wherein: The volume-based pore diameter mode of the anode foil having the dielectric layer is 0.1 μm or more and 0.3 μm or less.

3. The electrolytic capacitor according to claim 1 or 2, wherein: The alkylene glycol has 6 or less carbon atoms.

4. The electrolytic capacitor according to any one of claims 1 to 3, wherein The alkylene glycol has a structure in which at least one carbon atom is interposed between carbon atoms to which two hydroxyl groups are respectively bonded.

5. The electrolytic capacitor according to any one of claims 1 to 4, wherein The polyalkylene glycol comprises an oxy group C 3-4 Repeating structure of alkylene.

6. The electrolytic capacitor according to any one of claims 1 to 5, wherein The weight average molecular weight of the polyalkylene glycol is 400 or more.

7. The electrolytic capacitor according to any one of claims 1 to 6, wherein: The content of the solvent in the liquid component is 30% by mass or more and 100% by mass or less.

8. The electrolytic capacitor according to any one of claims 1 to 7, wherein The self-doping conductive polymer has a conjugated polymer skeleton, and the conjugated polymer has one or more and three or less anionic groups per molecule.

9. The electrolytic capacitor according to any one of claims 1 to 8, wherein The self-doping conductive polymer has a conjugated polymer skeleton including a monomer unit corresponding to a thiophene compound, and an anionic group introduced into the skeleton.

10. The electrolytic capacitor according to claim 9, wherein: The anionic group is introduced into the skeleton via a linking group, The linking group includes an alkylene group having 2 or more carbon atoms.

11. The electrolytic capacitor according to any one of claims 1 to 10, wherein: The self-doping conductive polymer contains at least a sulfonic group.

12. The electrolytic capacitor according to any one of claims 1 to 11, wherein: The anode foil includes aluminum.

13. The electrolytic capacitor according to any one of claims 1 to 12, wherein: The capacitor element includes a cathode foil and a separator between the anode foil and the cathode foil. The conductive polymer component is impregnated into the separator.