Lithium ion battery
By using high-porosity anode plates and controlling the reaction capacity ratio in lithium-ion batteries, the mass energy density of lithium-ion batteries is increased and cycle performance is optimized, solving the problem of lithium precipitation on the anode surface and ensuring the safety of the battery. sex and longevity.
Patent Information
- Application Number
- CN202380022865.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2024-10-11
AI Technical Summary
While improving the mass energy density of existing lithium-ion batteries, it is difficult to balance the control of lithium deposition and cycle life, especially the safety issues caused by uncontrollable lithium deposition on the anode surface.
The anode plate with high porosity is used to induce the excess lithium on the cathode side to be controlled to precipitate in the form of lithium metal on the anode side during the charging process, and by controlling the reaction capacity of the anode plate to be lower than the reaction capacity of the cathode plate, reducing the anode The mass proportion of active materials in the pole piece increases the mass energy density while ensuring safety performance.
It effectively improves the mass energy density and cycle performance of lithium-ion batteries, avoids uncontrollable lithium precipitation on the anode surface, extends the cycle life of the battery and improves safety performance.
Smart Images

Figure CN118765443A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of lithium-ion batteries, and specifically relates to a lithium-ion battery. Background Art
[0002] The overall capacity of a lithium-ion battery is determined by the capacity per unit area of the cathode material configured inside the battery. In order to increase the mass energy density (i.e., mass specific capacity) of the battery, the battery's deadweight needs to be reduced as much as possible while keeping the battery charge constant. In the prior art, the main method of reducing the deadweight of a battery is to reduce the mass proportion of inactive components and structural parts inside the battery, such as using thinner electrode current collectors, using porous current collectors, reducing the amount of battery liquid injection, using thinner and lighter separators, using thinner and lighter battery packaging bags, etc.
[0003] During the charging process of lithium-ion batteries, lithium ions are extracted from the cathode material and then embedded in the anode material; during discharge, lithium ions are extracted from the inside of the anode material and embedded in the cathode material; this cycle repeats to achieve repeated charging and discharging of secondary batteries. In the actual design process of the battery, in order to prevent the uncontrollable lithium precipitation problem on the surface of the anode pole piece, which leads to safety problems such as reduced cycle life or even battery short circuit, it is necessary to ensure that the lithium capacity that can be embedded in the anode material is greater than the lithium capacity that can be extracted from the cathode material. This part of the anode material that is higher than the capacity of the cathode material is used to prevent lithium ions from precipitating outside the anode material. It does not participate in the embedding and extraction of lithium during the actual working process of the battery and is also an inactive component. The prior art also considers reducing the amount of this part of inactive components to improve the mass energy density of lithium-ion batteries. However, the mass compression space of inactive components inside the battery is limited. Improving the mass energy density of the battery by reducing the amount of inactive anode materials is gradually approaching the limit, and it is difficult to further improve the mass energy density of lithium-ion batteries. Therefore, the prior art cannot take into account both controlling the lithium precipitation problem (cycle performance) and further improving the energy density. Summary of the invention
[0004] In order to solve the above problems, and to take into account both further improving the energy density of lithium-ion batteries and controlling the lithium precipitation problem, this application proposes a lithium-ion battery that uses a high-porosity anode pole piece. During the battery charging process, when the anode material is fully embedded with lithium, it can induce the excess lithium on the cathode side to be controllably precipitated on the anode side in the form of lithium metal, thereby preventing uncontrollable lithium precipitation on the surface of the anode pole piece and ensuring the cycle life of the lithium-ion battery. On this basis, by controlling the reaction capacity of the anode pole piece to be lower than the reaction capacity of the cathode pole piece, the mass proportion of active materials in the anode pole piece in the lithium-ion battery is reduced while ensuring the battery capacity, effectively improving the mass energy density of the lithium-ion battery, while also taking into account higher cycle performance.
[0005] The lithium-ion battery provided in this application adopts the following scheme:
[0006] A lithium ion battery comprises a cathode plate and an anode plate, wherein the porosity of the anode plate is N, and the value range of N is N≥50%; the reaction capacity of the anode plate is C a , the reaction capacity of the cathode plate is C c , the reaction capacity of the anode plate C a and the reaction capacity C of the cathode plate c Satisfy the conditions: 0<C a / C c ≤0.95. The lithium-ion battery of the present application adopts an anode plate with a high porosity (N ≥ 50%). During the battery charging process, when the anode material is fully embedded with lithium, it can induce the excess lithium on the cathode side to be controlled to precipitate in the pores of the anode plate in the form of lithium metal, thereby preventing uncontrollable lithium precipitation on the surface of the anode plate. By controlling the porosity ≥ 50% to ensure safety, the anode reaction capacity C a Less than the cathode reaction capacity C c , both satisfy 0<C a / C c ≤0.95, breaking through the inertial thinking in this field that the lithium insertion capacity of the anode must be no less than the lithium removal capacity of the cathode. Under the premise of ensuring the battery capacity, the mass proportion of active materials in the anode electrode of the lithium-ion battery is reduced, and the mass energy density is improved by reducing the active materials, while also taking into account higher safety performance and cycle performance.
[0007] Different from the traditional anode plate, the capacity of the anode plate in the present application includes two parts: 1. The capacity exerted by the redox reaction between the anode material and lithium ions, that is, the capacity exerted by the lithium embedding of the anode material, which is defined as the reaction capacity (lithium embedding capacity) of the anode plate in the present application; 2. The capacity exerted by the lithium precipitated in the pores of the anode plate, which is defined as the controllable lithium deposition capacity of the anode plate in the present application. The reaction capacity and controllable lithium deposition capacity of the anode plate in the present application together constitute the anode plate capacity. Therefore, although the present application reduces the active material of the anode plate and reduces its reaction capacity, the lithium metal precipitated in the pores of the anode plate can still participate in the cycle and manifest as the lithium deposition capacity, so that the capacity of the anode plate is not reduced, and the mass of the anode active material is reduced while ensuring the capacity, so that the mass energy density of the lithium-ion battery is improved.
[0008] In addition, the reaction capacity (lithium removal capacity) of the cathode electrode in the present application is the capacity exerted by the cathode material undergoing redox reaction, that is, the capacity exerted by the cathode material delithiation.
[0009] Furthermore, in the above lithium-ion battery, the reaction capacity C of the anode electrode is a and the reaction capacity C of the cathode plate c Satisfy the conditions: 0.20≤Ca / C c ≤0.80. By controlling the relationship between the anode reaction capacity and the cathode reaction capacity, the active material in the anode electrode can be further reduced, thereby improving the mass energy density of the lithium-ion battery.
[0010] Furthermore, in the above lithium-ion battery, the reaction capacity C of the anode electrode is a and the reaction capacity C of the cathode plate c Satisfy the conditions: 0.40≤C a / C c ≤0.60.
[0011] Preferably, the porosity N of the anode pole piece is in the range of 50% ≤ N ≤ 90%. The present application controls the porosity to be between 50% and 90%, so that the excess lithium released can be controlled to precipitate at the anode, thereby improving the safety performance and cycle performance, and avoiding the anode pole piece from being too large due to the high porosity, so that the anode pole piece has a suitable volume for application. In some application scenarios where the volume requirement is not high, the porosity of the anode pole piece can satisfy N>90%, so that the pores of the anode pole piece can accommodate more lithium ions for controllable precipitation.
[0012] Furthermore, in order to take into account excellent safety, cycle performance and appropriate volume, the porosity N of the anode plate is in the range of 65%≤N≤76%.
[0013] Preferably, the porosity N of the anode plate and the reaction capacity C of the anode plate are a and the reaction capacity C of the cathode plate c Satisfy the relationship I: N ≥ [-0.9375 × (C a / C c )+1.0625]×100%. By controlling the relationship between the porosity of the anode plate, the reaction capacity of the anode plate, and the reaction capacity of the cathode plate, the excess lithium ions of the cathode material can be completely received by the pores of the anode plate after reducing the amount of positive electrode material, which can improve the energy density and avoid uncontrollable lithium precipitation on the surface of the anode plate, which helps to achieve the best energy density and cycle performance. Furthermore, when the porosity N of the anode plate and the reaction capacity C of the anode plate are a and the reaction capacity C of the cathode plate c Satisfy the relationship I: N>[-0.9375×(C a / C c )+1.0625]×100%, it is beneficial to further improve the cycle performance of lithium-ion batteries.
[0014] Preferably, the anode plate has a two-dimensional structure and / or a three-dimensional structure. The anode material may be a material having a two-dimensional structure, a material having a three-dimensional structure, or a mixed material having a two-dimensional structure and a three-dimensional structure, that is, the anode plate may have a composite structure including two-dimensional and three-dimensional structures.
[0015] Preferably, the anode electrode plate includes at least one of silicon oxide, silicon carbon, pure silicon, silver, tin, hard carbon, soft carbon, graphite, and lithium titanate. The use of lithium-embedded materials such as graphite, hard carbon, soft carbon, and silicon as anode materials has mature technology and a wide range of sources. In this application, pure silicon refers to silicon with a purity of more than 99%; soft carbon refers to amorphous carbon that can be graphitized at a high temperature of more than 2000°C; hard carbon refers to amorphous carbon that is difficult to graphitize even at a high temperature of more than 2500°C.
[0016] Preferably, the cathode electrode comprises at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide, lithium iron phosphate, lithium-rich manganese-based materials, and sulfur. In this application, the lithium-rich manganese-based material refers to a material composed of Li 2 MnO 3 and LiMO 2 (M=Ni 1 / 2 Mn 1 / 2 and / or Mn x Ni y Co (1-x-y) ) materials.
[0017] Based on the lithium-ion battery of the present application, by controlling the reaction capacity C of the anode electrode a and the reaction capacity C of the cathode plate c Satisfy the conditions: 0<C a / C c≤0.95. During the charging process of lithium-ion batteries, the cathode electrode provides lithium ions and the anode electrode receives lithium ions. The present application improves the energy density of lithium-ion batteries by controlling the reaction capacity relationship between the cathode and the anode, while the amount of lithium ions provided remains unchanged, by reducing the amount of anode active materials. The anode electrode cannot receive all the lithium ions with more lithium ions in the cathode electrode, so the present application controls the porosity N of the anode electrode to be ≥50%, so that the excess lithium ions are precipitated inside the pores of the anode electrode, avoiding the problem of lithium precipitation on the surface of the anode electrode, so that the lithium-ion battery has better cycle performance and safety performance. The lithium ions entering the pores of the anode electrode and the lithium ions embedded in the structure of the anode active material still participate in the cycle process, so the amount of active lithium in the battery has not decreased, but because the reaction capacity of the anode electrode is reduced, the corresponding anode material load per unit area is also low, so the mass of the active material in the anode electrode in the lithium-ion battery is reduced while ensuring the battery capacity, so the energy density can be effectively improved. Therefore, the present application controls the reaction capacity ratio between the anode electrode and the cathode electrode and the porosity of the anode electrode, so that the active lithium will not be reduced, the load of the anode electrode can be reduced, and lithium precipitation can be avoided, thereby improving the energy density, safety performance and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a surface photograph of the anode electrode piece obtained by disassembling the lithium-ion battery of Comparative Example 1 in a fully charged state;
[0019] Figure 2 This is a cross-sectional photograph of the anode electrode piece obtained by disassembling the lithium-ion battery of Comparative Example 1 in a fully charged state;
[0020] Figure 3 This is a surface photograph of the anode electrode piece obtained by disassembling the lithium-ion battery of Comparative Example 2 in a fully charged state;
[0021] Figure 4 This is a cross-sectional photograph of the anode electrode piece obtained by disassembling the lithium-ion battery of Comparative Example 2 in a fully charged state;
[0022] Figure 5 This is a surface photograph of the anode electrode piece obtained by disassembling the lithium-ion battery of Example 1 in a fully charged state;
[0023] Figure 6 This is a cross-sectional photograph of the anode electrode piece obtained by disassembling the lithium-ion battery of Example 1 in a fully charged state;
[0024] Figure 7 is the ratio of the porosity N to the capacity per unit area of the anode electrode sheet and the cathode electrode sheet in the lithium ion battery of Example 2 and Example 5 (C a / C c )’s corresponding relationship curve. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0026] In the lithium-ion battery of the present application, the reaction capacity of the anode electrode is reduced (i.e., 0<C a / C c ≤0.95), on the basis of keeping the amount of lithium ions that can be extracted from the cathode unchanged, the mass of the anode active material in the lithium-ion battery can be reduced, thereby improving the energy density of the battery. On this basis, since the capacity of the anode electrode that can embed lithium is less than the capacity of the cathode electrode that can extract lithium, during the battery charging process, when the anode material is completely embedded with lithium, some lithium ions will not be able to enter the anode active material, but at the same time, due to the use of anode electrodes with high porosity (N ≥ 50%), the lithium ions that cannot enter the anode active material will enter the pores in the form of metallic lithium, that is, part of the lithium ions on the cathode side are embedded in the active material on the anode side, and the rest will enter the pore structure on the anode side. Since the excess lithium ions enter the pores, lithium precipitation will not occur on the surface of the electrode, avoiding or reducing safety issues such as short circuits caused by uncontrollable lithium precipitation.
[0027] In the lithium-ion battery of the present application, the relevant materials and preparation methods thereof and the testing methods of the relevant performances are as follows:
[0028] Anode plate
[0029] In the present application, the conventional coating and cold pressing method can be used to prepare the anode pole piece, which specifically includes uniformly dispersing the raw materials such as lithium-embedded anode material, binder, conductive agent, solvent dispersant, etc. to form a slurry, coating the slurry on the anode current collector, drying, and cold pressing to obtain the anode pole piece.
[0030] In order to control the porosity of the anode electrode to be not less than 50%, a lithium-intercalated anode material with a three-dimensional porous structure can be used when preparing the slurry; a lithium-intercalated anode material with a large particle size can be used; the solid content of the anode slurry can be reduced; a pore-forming agent can be added to the anode slurry, and the pore-forming agent decomposes into gas and escapes during the drying process of the electrode to form holes inside the anode electrode; the cold pressing pressure of the electrode can be reduced; and the electrode cold pressing process can be omitted.
[0031] In the present application, the anode electrode can also be prepared by an electrospinning method, which specifically includes evenly dispersing the lithium-embedded anode material, the polymer main material, and the solvent dispersant into a spinning solution, and then using an electrospinning device to prepare an anode electrode with a three-dimensional porous structure constructed from a one-dimensional fiber structure.
[0032] Cathode Piece
[0033] In this application, the cathode electrode sheet can be prepared by a conventional coating cold pressing method. Taking the ternary positive electrode as an example, the ternary positive electrode material (NCM811), conductive carbon black and polyvinylidene fluoride (PVDF) are fully stirred and mixed in an N-methylpyrrolidone solvent system at a weight ratio of about 97.7%: 1.0%: 1.3% to prepare a positive electrode slurry. The prepared positive electrode slurry is coated on the positive electrode current collector aluminum foil, dried, and cold pressed to obtain the positive electrode, that is, the cathode electrode sheet of this application.
[0034] In the lithium-ion battery of the present application, the capacity per unit area of the anode pole piece can be reduced by reducing the anode material load in the anode pole piece, and the capacity per unit area of the cathode pole piece can be increased by increasing the cathode material load in the cathode pole piece. In the present application, the mass energy density of the lithium-ion battery is calculated by battery capacity / battery mass. When the anode material load in the anode pole piece is reduced, the amount of lithium ions that can be extracted from the cathode material remains unchanged, corresponding to the battery capacity of the lithium-ion battery remains unchanged, and the mass of the anode active material is reduced, corresponding to the total mass of the lithium-ion battery is reduced, and the mass energy density is improved; when the cathode material load in the cathode pole piece is increased, the amount of lithium ions that can be extracted from the cathode material increases, corresponding to the battery capacity of the lithium-ion battery increases, and the anode material in the anode pole piece is reduced compared with conventional lithium-ion batteries, which is equivalent to a reduction in the total mass of the lithium-ion battery, and the mass energy density of the lithium-ion battery is improved.
[0035] The lithium-ion battery of the present application also includes: an electrolyte and a separator.
[0036] Electrolyte
[0037] In the present application, conventional ether or carbonate electrolytes may be used. Taking conventional ether electrolytes as an example, in a dry argon atmosphere, dioxolane (DOL) and ethylene glycol dimethyl ether (DME) are first mixed in a volume ratio of 1:1, and then lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) is added to dissolve and mix evenly to obtain an ether electrolyte with a lithium salt concentration of 1M.
[0038] Lithium-ion battery full battery
[0039] In the present application, a lithium-ion battery full cell can be prepared by conventional methods, and a separator can be used to separate the cathode electrode piece and the anode electrode piece. The separator can be a conventional separator, which can include a substrate layer and a surface treatment layer. For example, a porous polyethylene film with a thickness of 9 μm can be selected and placed between the cathode electrode piece and the anode electrode piece as a separator, and assembled into a full battery together with the anode electrode piece, the cathode electrode piece and the electrolyte.
[0040] The lithium-ion battery of the present application can be a button battery, a soft-pack battery, a square battery, a special-shaped battery, etc.
[0041] The porosity of the anode electrode is tested by the gas replacement method. The test method is: cut anode electrode samples of appropriate quality, vacuum dry the samples and place them in the sample chamber of the true density tester, then seal the test system and completely evacuate. First, the sample chamber and expansion chamber are sealed independently, and then nitrogen is introduced respectively, and the gas pressures in the sample chamber and expansion chamber are recorded as P1 and Pa respectively; then the valve between the sample chamber and the expansion chamber is opened to connect the two, and after the pressure stabilizes, the pressure of the sample chamber and the expansion chamber is recorded as P2; then the true volume V of the sample can be calculated according to the following formula: Among them, V CELL is the volume of the sample chamber of the true density tester, V EXP is the volume of the expansion chamber of the true density tester; the apparent volume of the sample V 0 The following can be obtained by measuring the sample area S, the total thickness of the anode electrode H and the thickness of the anode current collector h: 0 =S×(Hh); the porosity of the electrode can be calculated
[0042] Calculation method of theoretical mass energy density of battery: In this application, in order to facilitate the comparison of the theoretical energy density of lithium-ion batteries of various embodiments and comparative examples, all embodiments and comparative examples use the same 10μm thick copper foil as the anode current collector; the same 12μm thick aluminum foil as the cathode current collector; the same 9μm thick porous polyethylene film as the separator; the injection volume is designed to be one-tenth of the cathode load. It should be noted that the use of this condition to assemble the full battery for measurement and comparison is only to unify the measurement scale of the theoretical energy density of lithium-ion batteries and facilitate the performance comparison of the embodiments and comparative examples, and does not limit the materials and sizes of the lithium-ion batteries of this application; the lithium-ion batteries of this application can select different types and sizes of anode current collectors, cathode current collectors and diaphragm materials according to different application requirements.
[0043] In order to more intuitively illustrate the improvement in energy density of the lithium-ion battery equipped with a lithium-poor anode material in this application, the theoretical mass energy density of the battery is calculated based on the total mass M (mg) of the four main materials of the battery, namely the cathode electrode, the anode electrode, the electrolyte and the isolation membrane. At 25°C, the battery is charged at a constant current of 0.2C to the charging cut-off voltage, and then charged at a constant voltage to a current of 0.025C. At this time, the battery is fully charged. The charging capacity at this time is recorded, which is the charging capacity of the first cycle; after the battery is allowed to stand for 5 minutes, it is discharged at a constant current of 0.5C to the discharge cut-off voltage. This is a cyclic charge and discharge process; the battery is subjected to 5 cycles of charge and discharge, and the discharge capacity A (mAh) of the 5th cycle is recorded; the discharge voltage U (V) of the 5th cycle is recorded. The theoretical mass energy density W (Wh / kg) of the battery can be calculated according to the following formula:
[0044] Cycle performance test method: At 25°C, charge the battery at a constant current of 0.2C to the charge cut-off voltage, then charge at a constant voltage to a current of 0.025C. At this time, the battery is fully charged. Record the charge capacity at this time, which is the charge capacity of the first cycle. After the battery is left to stand for 5 minutes, discharge it at a constant current of 0.5C to the discharge cut-off voltage. This is a cycle charge and discharge process. Record the discharge capacity at this time, which is the discharge capacity of the first cycle. Perform a cycle charge and discharge test on the battery according to the above method, record the discharge capacity after each cycle, until the discharge capacity of the battery decays to 80% of the discharge capacity of the first cycle, and use the number of cycles at this time to characterize the cycle performance of the battery. The higher the number of cycles, the better the cycle performance of the battery.
[0045] In the theoretical mass energy density and cycle performance test of lithium-ion batteries, the specific values of the charge cut-off voltage and the discharge cut-off voltage are not strictly limited in this application, and can be determined according to the lithium-ion battery system composed of different positive electrode materials and negative electrode materials in the field. For example, when the anode material of the lithium-ion battery is a ternary material, the charge cut-off voltage is 4.3V and the discharge cut-off voltage is 2.8V.
[0046] In the lithium-ion battery system of the present application, the anode electrode sheet and the cathode electrode sheet have the same area in the working state, so the unit area capacity C of the anode electrode sheet can be used. a1 (Anode surface capacity) represents the reaction capacity of the anode electrode, and the unit area capacity C of the cathode electrode is used. c1 (Cathode surface capacity) represents the reaction capacity of the cathode electrode, which is expressed by the unit area capacity of the anode electrode / the unit area capacity of the cathode electrode. a / C c .
[0047] The capacity per unit area of the anode electrode in this application is C a1 and the capacity per unit area of the cathode plate C c1 The reaction capacity (lithium insertion capacity) of the anode electrode can be measured by a method comprising the following steps: a , divided by the area of the anode plate to obtain the unit area capacity C of the anode plate a1 ; Test to obtain the reaction capacity (lithium removal capacity) of the cathode electrode C c , divided by the area of the cathode plate to obtain the unit area capacity C of the cathode plate c1 .
[0048] In some embodiments, the lithium insertion capacity C of the anode electrode is a Or the lithium removal capacity of the cathode electrode C c Follow this method to test:
[0049] The anode electrode or cathode electrode is used as the electrode to be tested, the electrode to be tested is used as the cathode and the pure lithium electrode is used as the anode to assemble a test battery. Then the test battery is first charged at a constant current of 0.1C to the charge termination voltage, and then discharged at a constant current of 0.1C to the discharge termination voltage. The discharge capacity of the test battery is obtained, which is the lithium insertion capacity C of the tested anode electrode. a Or the lithium removal capacity C of the tested cathode electrode c .
[0050] In some embodiments, the charge termination voltage and the discharge termination voltage are determined as follows:
[0051] When the anode electrode is the cathode, the charge termination voltage is 3V and the discharge termination voltage is 0.005V; or, when the cathode electrode is the cathode, the lithium removal capacity C of the cathode electrode is c The testing methods include:
[0052] When the cathode material of the cathode electrode is lithium cobalt oxide, the charge termination voltage is 4.5V and the discharge termination voltage is 3.2V; when the cathode material of the cathode electrode is one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium manganese oxide, or any combination and any proportion of the cathode material, the charge termination voltage is 4.3V and the discharge termination voltage is 2.8V; when the cathode material of the cathode electrode is lithium iron phosphate, the charge termination voltage is 4.0V and the discharge termination voltage is 2.5V; when the cathode material of the cathode electrode is lithium-rich manganese-based material, the charge termination voltage is 4.8V and the discharge termination voltage is 3.0V; when the cathode material of the cathode electrode is sulfur, the charge termination voltage is 3.0V and the discharge termination voltage is 1.7V.
[0053] In some embodiments, the capacity per unit area of the cathode electrode C c1 The value range is 2mAh≤C c1 ≤5mAh; and / or, the capacity per unit area of the anode electrode C a1 The value range is 1mAh≤C a1 ≤4mAh. In this application, increasing the surface capacity of the cathode electrode piece (corresponding to selecting a higher cathode material loading amount) is beneficial to increasing the total capacity of the lithium-ion battery; by controlling the lower surface capacity of the anode electrode piece (corresponding to selecting a lower anode material loading amount), the mass of the lithium-ion battery is reduced without affecting the total capacity of the lithium-ion battery. Therefore, controlling the optional range of the unit area capacity of the cathode electrode piece and the anode electrode piece can ensure that the lithium-ion battery has a higher mass energy density.
[0054] Example
[0055] The technical solution of the present application is described below in conjunction with specific embodiments and comparative examples. Unless otherwise specified, the raw materials used in the following embodiments are all from common commercially available products, and the devices or equipment used are all purchased from conventional market sales channels.
[0056] Example 1
[0057] In the lithium-ion battery of this embodiment, the cathode current collector is an aluminum foil with a thickness of 12 μm, the cathode material is lithium nickel cobalt manganese oxide NCM811, and the cathode loading is 18.37 mg / cm 2 The anode current collector is a copper foil with a thickness of 10 μm, the anode material is a silicon oxide material, and the obtained anode electrode has a three-dimensional structure. The anode load is 2.25 mg / cm 2 A porous polyethylene film with a thickness of 9 μm is used as a separator and placed between the cathode and anode plates. An ether electrolyte with a lithium salt concentration of 1 M is used, and the injection volume is one-tenth of the cathode load. The separator, anode plate, cathode plate and electrolyte are assembled into a full battery.
[0058] The performance of the anode and cathode plates was tested: the porosity of the anode plate was N=50% as determined by the gas replacement method.
[0059] The anode electrode is used as the electrode to be tested, the electrode to be tested is used as the positive electrode, and the pure lithium electrode is used as the negative electrode to assemble a test battery. Then the test battery is first charged at a constant current of 0.1C to a charge termination voltage of 3V, and then discharged at a constant current of 0.1C to a discharge termination voltage of 0.005V. The discharge capacity of the test battery is obtained, which is the reaction capacity C of the anode electrode tested. a The capacity per unit area of the anode plate is calculated by dividing the reaction capacity of the anode plate by the plate area. a1 =3.02mAh / cm 2 .
[0060] The cathode electrode is used as the electrode to be tested, the electrode to be tested is used as the positive electrode, and the pure lithium electrode is used as the negative electrode to assemble a test battery. Then the test battery is first charged at a constant current of 0.1C to a charge termination voltage of 4.5V, and then discharged at a constant current of 0.1C to a discharge termination voltage of 3.2V. The discharge capacity of the test battery is obtained, which is the reaction capacity C of the cathode electrode tested. c The cathode electrode capacity per unit area is calculated by dividing the cathode electrode reaction capacity by the electrode area. c1 =3.75mAh / cm 2 , the unit area capacity of the anode electrode / the unit area capacity of the cathode electrode = C a / C c =0.81≤0.95.
[0061] Embodiment a
[0062] The lithium ion battery of this embodiment is different from that of embodiment 1 only in that the porosity N of the anode plate is 30% as measured by the gas replacement method. The anode load is 2.65 mg / cm 2 The unit area capacity of the anode electrode is 3.56 mAh / cm 2 The unit area capacity of the cathode plate is 3.75 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.95.
[0063] Embodiment b
[0064] The lithium ion battery of this embodiment is different from that of embodiment 1 only in that the porosity N of the anode plate is 85% as measured by the gas replacement method. The anode load is 0.56 mg / cm 2 The unit area capacity of the anode electrode is 0.75 mAh / cm 2 The unit area capacity of the cathode plate is 3.75 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.20.
[0065] Example 2
[0066] The lithium ion battery of this embodiment is different from that of embodiment 1 only in that the anode load is 1.67 mg / cm 2 The unit area capacity of the anode electrode is 2.25 mAh / cm 2 The unit area capacity of the cathode plate is 3.75 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.60.
[0067] Example 3
[0068] The lithium ion battery of this embodiment is different from that of embodiment 1 only in that the porosity N of the anode plate is 65% as measured by the gas replacement method. The anode load is 1.40 mg / cm 2 The unit area capacity of the anode electrode is 1.88 mAh / cm 2 The unit area capacity of the cathode plate is 3.75 mAh / cm 2Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.50.
[0069] Example 4
[0070] The lithium ion battery of this embodiment is different from that of embodiment 3 only in that the anode load is 1.67 mg / cm 2 The unit area capacity of the anode electrode is 2.25 mAh / cm 2 The unit area capacity of the cathode plate is 3.75 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.60.
[0071] Example 5
[0072] The lithium ion battery of this embodiment is different from that of embodiment 3 only in that the anode load is 1.22 mg / cm 2 The unit area capacity of the anode electrode is 1.64 mAh / cm 2 The unit area capacity of the cathode plate is 3.75 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.60.
[0073] Example 6
[0074] The lithium ion battery of this embodiment is different from that of Embodiment 5 only in that the porosity N of the anode electrode plate obtained by gas replacement method is 76%.
[0075] Example 7
[0076] The lithium ion battery of this embodiment is different from that of embodiment 3 only in that the cathode load is 10.58 mg / cm 2 , the anode loading is 0.8 mg / cm 2 The test showed that the capacity per unit area of the anode electrode was 1.08 mAh / cm 2 The unit area capacity of the cathode electrode is 2.16 mAh / cm 2 , the unit area capacity of the anode electrode / the unit area capacity of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / Cc =0.50.
[0077] Example 8
[0078] The lithium ion battery of this embodiment is different from that of embodiment 3 only in that the cathode load is 13.18 mg / cm 2 , the anode loading is 1 mg / cm 2 The test showed that the capacity per unit area of the anode electrode was 1.35 mAh / cm 2 The unit area capacity of the cathode plate is 2.69 mAh / cm 2 , the unit area capacity of the anode electrode / the unit area capacity of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.50.
[0079] Example 9
[0080] The lithium ion battery of this embodiment is different from that of embodiment 3 only in that the cathode load is 15.78 mg / cm 2 , the anode loading is 1.21 mg / cm 2 The test showed that the unit area capacity of the anode electrode was 1.62 mAh / cm 2 The unit area capacity of the cathode plate is 3.22 mAh / cm 2 , the unit area capacity of the anode electrode / the unit area capacity of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.50.
[0081] Example 10
[0082] The lithium ion battery of this embodiment is different from that of embodiment 3 in that the anode material is silicon carbon material and the anode loading is 1.32 mg / cm 2 The anode plate has a three-dimensional structure. The porosity of the anode plate is N=65% as measured by the gas replacement method. The unit area capacity of the anode plate is 1.88 mAh / cm 2 The unit area capacity of the cathode plate is 3.75 mAh / cm 2 , the unit area capacity of the anode electrode / the unit area capacity of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.50.
[0083] Embodiment 11
[0084] The lithium ion battery of this embodiment is different from that of embodiment 3 in that the anode material is pure silicon material and the anode loading is 0.80 mg / cm 2 The anode plate has a three-dimensional structure. The porosity of the anode plate is N=65% as measured by the gas replacement method. The unit area capacity of the anode plate is 1.88 mAh / cm 2 The unit area capacity of the cathode plate is 3.75 mAh / cm 2 , the unit area capacity of the anode electrode / the unit area capacity of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.50.
[0085] Example 12
[0086] The lithium ion battery of this embodiment is different from that of embodiment 3 only in that the cathode material is lithium cobalt oxide LCO and the cathode loading is 16.56 mg / cm 2 ; The anode material is silicon oxide material, and the anode load is 1.09 mg / cm 2 The test showed that the unit area capacity of the anode electrode was 1.47 mAh / cm 2 The unit area capacity of the cathode plate is 2.93 mAh / cm 2 , the unit area capacity of the anode electrode / the unit area capacity of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.50.
[0087] Embodiment 13
[0088] The lithium ion battery of this embodiment is different from that of embodiment 3 only in that the cathode material is lithium manganese oxide LMO and the cathode loading is 19.02 mg / cm 2 ; The anode material is silicon oxide material, and the anode load is 1.09 mg / cm 2 The test showed that the unit area capacity of the anode electrode was 1.05 mAh / cm 2 The unit area capacity of the cathode plate is 2.08 mAh / cm 2 , the unit area capacity of the anode electrode / the unit area capacity of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.50.
[0089] Comparative Example 1
[0090] The lithium-ion battery of this comparative example is different from that of Example 1 only in that the porosity of the anode electrode piece measured by the gas replacement method is N=25%. The anode loading is 2.93 mg / cm 2 The unit area capacity of the anode electrode is 3.94 mAh / cm 2 The unit area capacity of the cathode plate is 3.75 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =1.05.
[0091] Comparative Example 2
[0092] The lithium-ion battery of this comparative example is different from that of Example 1 in that the porosity of the anode electrode piece measured by the gas replacement method is N=25%. The anode loading is 2.25 mg / cm 2 The unit area capacity of the anode electrode is 3.01 mAh / cm 2 The unit area capacity of the cathode plate is 3.75 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.80.
[0093] Comparative Example 3
[0094] The lithium-ion battery of this comparative example is different from that of Example 1 in that the porosity of the anode electrode piece measured by the gas replacement method is N=37%. The anode loading is 2.25 mg / cm 2 The unit area capacity of the anode electrode is 3.02 mAh / cm 2 The unit area capacity of the cathode plate is 3.75 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =0.81.
[0095] Comparative Example 4
[0096] The lithium-ion battery of this comparative example is different from that of Example 7 in that the porosity of the anode electrode piece measured by the gas replacement method is N=25%. The anode loading is 1.69 mg / cm 2 The unit area capacity of the anode electrode is 2.27 mAh / cm 2The unit area capacity of the cathode electrode is 2.16 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =1.05.
[0097] Comparative Example 5
[0098] The lithium-ion battery of this comparative example is different from that of Example 8 in that the porosity of the anode electrode piece measured by the gas replacement method is N=25%. The anode loading is 2.10 mg / cm 2 The unit area capacity of the anode electrode is 2.83 mAh / cm 2 The unit area capacity of the cathode plate is 2.69 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =1.05.
[0099] Comparative Example 6
[0100] The lithium-ion battery of this comparative example is different from that of Example 9 in that the porosity of the anode electrode piece measured by the gas replacement method is N=25%. The anode loading is 2.52 mg / cm 2 The unit area capacity of the anode electrode is 3.38 mAh / cm 2 The unit area capacity of the cathode plate is 3.22 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =1.05.
[0101] Comparative Example 7
[0102] The lithium-ion battery of this comparative example is different from that of Example 10 in that the porosity of the anode electrode piece measured by the gas replacement method is N=25%. The anode loading is 2.76 mg / cm 2 The unit area capacity of the anode electrode is 3.94 mAh / cm 2 The unit area capacity of the cathode plate is 3.75 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =1.05.
[0103] Comparative Example 8
[0104] The lithium-ion battery of this comparative example is different from that of Example 11 in that the porosity of the anode electrode piece measured by the gas replacement method is N=25%. The anode loading is 1.68 mg / cm 2 The unit area capacity of the anode electrode is 3.94 mAh / cm 2 The unit area capacity of the cathode plate is 3.75 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =1.05.
[0105] Comparative Example 9
[0106] The lithium-ion battery of this comparative example is different from that of Example 12 only in that the porosity of the anode electrode piece measured by the gas replacement method is N=25%. The anode loading is 2.29 mg / cm 2 The unit area capacity of the anode electrode is 3.08 mAh / cm 2 The unit area capacity of the cathode plate is 2.93 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =1.05.
[0107] Comparative Example 10
[0108] The lithium-ion battery of this comparative example is different from that of Example 13 in that the porosity of the anode electrode piece measured by the gas replacement method is N=25%. The anode loading is 1.62 mg / cm 2 The unit area capacity of the anode electrode is 2.18 mAh / cm 2 The unit area capacity of the cathode plate is 2.08 mAh / cm 2 Calculate the capacity per unit area of the anode electrode / the capacity per unit area of the cathode electrode = the reaction capacity of the anode electrode / the reaction capacity of the cathode electrode = C a / C c =1.05.
[0109] Test Example 1
[0110] The lithium ion batteries of Examples 1 to 13 (including Example a and Example b) and Comparative Examples 1 to 10 were respectively subjected to battery theoretical mass energy density tests and cycle performance tests. The test results of each Example and Comparative Example are shown in Table 1 below.
[0111] Table 1
[0112]
[0113]
[0114] In Comparative Examples 1 to 3 and Examples 1 to 6 (including Example a and Example b), the cathode plate adopts the same design: the cathode active material is NCM811 ternary material, the theoretical mass energy density is 209.1 mAh / g, and the cathode plate surface capacity (capacity per unit area) is 3.75 mAh / cm 2 ; The lithium-insertion anode material uses silicon oxide, and the theoretical mass energy density is 1600mAh / g. Comparative Example 1 uses a conventional battery design, and the anode surface capacity (i.e., the capacity per unit area) is 3.94mAh / cm 2 , which is 1.05 times the surface capacity of the cathode. The porosity of the anode electrode is 25%. The theoretical mass energy density of the full battery is calculated to be 361.49Wh / Kg. After the full battery is cycled 154 times in the voltage range of 2.8 to 4.3V, the battery capacity decays to 80%.
[0115] Comparative Example 2 reduces the amount of lithium-inserted anode material used, and the surface capacity of the anode electrode is reduced to 80% of the surface capacity of the cathode electrode, which is 3.01 mAh / cm 2 , the porosity of the anode plate is still designed to be 25%. Due to the reduction of the anode load, the theoretical mass energy density of the whole battery is increased to 379.04Wh / kg; however, after the lithium-embedded anode material on the anode side is completed, since there is not enough space inside the anode plate to accommodate the remaining lithium on the cathode side, lithium metal is easily precipitated on the surface of the anode plate and forms lithium dendrites, so the whole battery short-circuits after 47 cycles in the voltage range of 2.8 to 4.3V. Comparative Example 3 increases the porosity of the anode plate to 37% on the basis of Comparative Example 2. Since the battery mass remains unchanged, only the discharge voltage of the whole battery fluctuates slightly, so the theoretical mass energy density of the whole battery remains basically unchanged; although the battery life is slightly extended after the porosity of the anode plate is increased, a short circuit still occurs in the 73rd cycle, indicating that the 37% anode plate porosity is still not enough to prevent lithium precipitation on the surface of the anode plate.
[0116] In Example 1, the porosity of the anode plate is further increased to 50%. At this time, the capacity of the full battery decays to 80% after 182 cycles in the voltage range of 2.8 to 4.3 V. In Examples a to b and Examples 2 to 6, different designs are made for the surface capacity and porosity of the anode plate based on Example 1. By comparing Comparative Example 1 with Examples a to b and Examples 1 to 6, it can be found that when the porosity of the anode plate is not less than 50%, the battery design configured with a poor lithium-insertion anode material (i.e., controlling Ca / C c The ratio of the anode surface capacity to the cathode surface capacity is below 0.95) which can significantly improve the mass energy density of the battery under the premise of preventing the battery from short circuiting. According to the mass energy density and cycle performance test results, the theoretical mass energy density of the lithium ion battery of Examples 1 to 6 and Example b can reach 383.54 to 415.51Wh / kg, which is further improved than that of Example a. It can be seen that the ratio of the anode surface capacity to the cathode surface capacity of the present application is controlled to make C a / C c Satisfy 0.20≤C a / C c ≤0.80, reducing the loading of anode active materials while ensuring the total capacity of the lithium-ion battery can further improve the mass energy density of the lithium-ion battery while meeting better cycle performance.
[0117] Examples 7 to 9 and Comparative Examples 4 to 6 were verified for different cathode pole piece surface capacity designs. The cathode materials used in these six groups of experiments were all NCM811 ternary materials with a mass energy density of 209.1 mAh / g. The anode material uses silicon oxide material with a theoretical mass energy density of 1600 mAh / g. The results show that in batteries with different cathode designs, controlling the ratio of anode surface capacity to cathode surface capacity below 0.95 and constructing a porosity of ≥50% inside the anode pole piece can effectively improve the theoretical mass energy density of the battery and ensure high cycle performance.
[0118] Examples 10 to 13 and Comparative Examples 7 to 10 were verified for different battery systems. The cathode pole pieces in Examples 10 and 11 and Comparative Examples 7 and 8 adopt the same design: the cathode active material is NCM811 ternary material, with a theoretical mass energy density of 209.1 mAh / g and a surface capacity of 3.75 mAh / cm 2 . The lithium-intercalated anode material used in Example 10 and Comparative Example 7 is silicon-carbon material with a theoretical mass energy density of 1700mAh / g; the lithium-intercalated anode material used in Example 11 and Comparative Example 8 is pure silicon nanoparticles with an average particle size of 60nm, and a theoretical mass energy density of 3500mAh / g. The lithium-intercalated anode materials used in Examples 12, 13 and Comparative Examples 9 and 10 are all silicon-oxygen with a theoretical mass energy density of 1600mAh / g; the cathode active material used in Example 12 and Comparative Example 9 is lithium cobalt oxide material with a theoretical mass energy density of 185mAh / g and a surface capacity of 2.93mAh / cm 2 The cathode material used in Example 13 and Comparative Example 10 is lithium manganate material, with a theoretical mass energy density of 113.1 mAh / g and a surface capacity of 2.08 mAh / cm 2The results show that the strategy of improving the battery mass energy density by controlling the ratio of the anode surface capacity to the cathode surface capacity ≤ 0.95 and ensuring the anode electrode porosity ≥ 50% in the present application can be applied to different battery systems and battery designs.
[0119] Test Example 2
[0120] At 25°C, the lithium ion batteries of Comparative Example 1, Comparative Example 2 and Example 1 were charged at a constant current of 0.2C to the charging cut-off voltage, and then charged at a constant voltage to a current of 0.025C, at which time the battery was fully charged. The anode electrode piece of the lithium ion battery was removed in the fully charged state, and the surface and cross section of the anode electrode piece were observed using an optical microscope. Figure 1 This is a photo of the surface of the anode electrode piece disassembled from the lithium-ion battery of Comparative Example 1 in a fully charged state. Figure 2 This is a cross-sectional photo of the anode pole piece disassembled from the lithium-ion battery of Comparative Example 1 in a fully charged state. Since the anode pole piece of Comparative Example 1 is equipped with a sufficient amount of lithium-intercalated anode material, the lithium inside the cathode material is completely embedded in the lithium-intercalated anode material, so no obvious lithium precipitation phenomenon is observed on the surface of the anode pole piece. However, since Comparative Example 1 uses more anode material, its theoretical mass energy density is relatively low, only 361.49Wh / kg.
[0121] Figure 3 and Figure 4 They are the surface and cross-sectional photos of the anode electrode piece removed from the full battery in Comparative Example 2 when fully charged. It can be seen that very obvious lithium deposition has occurred at the edge of the electrode piece. This shows that lithium deposition on the surface of the anode electrode piece is the main reason for the premature short circuit of the battery in Comparative Example 2 and the number of cycles being only 47.
[0122] Figure 5 and Figure 6 They are surface and cross-sectional photographs of the anode electrode piece removed from the full battery in Example 1 when fully charged. It can be seen that the lithium metal is uniformly deposited inside the anode electrode piece, so no obvious local lithium deposition is observed on the electrode piece surface; and from the lithium-ion battery performance test results of Example 1, it can be seen that the lithium-ion battery of Example 1 has a theoretical mass energy density of 383.54Wh / kg based on 182 cycles, which takes into account both excellent mass energy density and cycle performance. Figures 1 to 6 The results show that the unit area capacity of the anode electrode and the unit area capacity of the cathode electrode of the present invention make C a / C c Satisfy the conditions: 0<C a / C c≤0.95, combined with the porosity N≥50% of the anode electrode, the excess lithium ions in the cathode are precipitated inside the pores of the anode electrode, avoiding the precipitation of lithium ions on the surface of the anode electrode and the occurrence of lithium dendrites, reducing the risk of premature short circuit, and being able to improve the energy density of lithium-ion batteries while improving the cycle performance and safety performance.
[0123] Test Example 3
[0124] The reaction capacity ratio (C a / C c ) and the anode plate porosity (N) are presented in the form of a scatter plot. Based on Examples 2 and 5, in which the cycle performance is relatively low, the relationship between N and C in Examples 2 and 5 is established. a / C c The corresponding relationship is y = -0.9375x + 1.0625, and the result is as follows Figure 7 As shown. Due to the reaction capacity ratio of the anode plate and the cathode plate (C a / C c ) is reduced, the difference between the amount of lithium ions that can be released from the cathode electrode and the amount of lithium ions that can be embedded in the anode electrode increases, so a higher porosity of the anode electrode is required to accommodate the lithium ions released from the cathode electrode to avoid the problem of lithium ion precipitation on the surface of the anode electrode. a / C c The corresponding relationship is determined by N≥[-0.9375×(C a / C c )+1.0625]×100%, and N≥50%. When the value of N is within this range, the lithium-ion battery can have excellent cycle performance. For example, the cycle performance test results of the ternary lithium-ion batteries of Examples 1 to 6 (the positive electrode material is NCM811 and the negative electrode material is silicon oxide) are more than 170 cycles. When N<[-0.9375×(C a / C c )+1.0625]×100%, its cycle performance is poor. In addition, when N>[-0.9375×(C a / C c )+1.0625]×100%(corresponding to Figure 7 y=-0.9375x+1.0625), and N≥50%, as in Example 1 [corresponding to Figure 7 midpoint (0.8, 0.5)], Example 3 [corresponding to Figure 7 midpoint (0.5, 0.65)], Example 4 [corresponding to Figure 7 midpoint (0.6, 0.65)], Example 6 [corresponding to Figure 7The cycle performance test result of the midpoint (0.44, 0.76)] can reach more than 180 cycles, which is higher than N = [-0.9375 × (C a / C c )+1.0625]×100%(corresponding to Figure 7 The point on the curve y=-0.9375x+1.0625) further improves the cycle performance of the lithium-ion battery.
[0125] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A lithium ion battery, characterized in that: The lithium-ion battery comprises a cathode electrode sheet and an anode electrode sheet; The porosity of the anode electrode sheet is N, and the value range of N is N≥50%; The reaction capacity of the anode electrode plate is Ca, and the reaction capacity of the cathode electrode plate is Cc. The reaction capacity Ca of the anode electrode plate and the reaction capacity Cc of the cathode electrode plate satisfy the condition: 0<Ca / Cc≤0.
95.
2. The lithium-ion battery according to claim 1, characterized in that The reaction capacity Ca of the anode electrode and the reaction capacity Cc of the cathode electrode satisfy the condition: 0.20≤Ca / Cc≤0.
80.
3. The lithium-ion battery according to claim 2, characterized in that: The reaction capacity Ca of the anode electrode and the reaction capacity Cc of the cathode electrode satisfy the condition: 0.40≤Ca / Cc≤0.
60.
4. The lithium-ion battery according to claim 1, characterized in that: The porosity N of the anode plate has a value range of 50%≤N≤90%.
5. The lithium-ion battery according to claim 4, characterized in that: The porosity N of the anode plate has a value range of 65%≤N≤76%.
6. The lithium-ion battery according to claim 1, characterized in that The anode plate has a two-dimensional structure and / or a three-dimensional structure.
7. The lithium-ion battery according to claim 1, characterized in that: The anode electrode plate includes at least one of silicon oxide, silicon carbon, pure silicon, silver, tin, hard carbon, soft carbon, graphite, and lithium titanate.
8. The lithium-ion battery according to claim 1, characterized in that The cathode electrode plate includes at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide, lithium iron phosphate, lithium-rich manganese-based material, and sulfur.