Fe / Pt doped carbon nano-enzyme particles, preparation method, uric acid test paper and application
By preparing iron/platinum-doped carbon nanoparticles and paper-based microfluidic chips with peroxidase-like activity, a uric acid detection system was constructed, which solved the problems of complexity and low efficiency of existing uric acid detection methods, and achieved rapid and sensitive uric acid detection to meet clinical diagnostic needs.
Patent Information
- Application Number
- CN202410763409.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-15
AI Technical Summary
Existing uric acid detection methods are complex to operate and are not suitable for immediate testing. Natural peroxidase is easily inactivated, difficult to purify, and expensive. The catalytic efficiency is easily affected by temperature and pH conditions, making it difficult to meet the needs of rapid and sensitive clinical diagnosis.
A one-step hydrothermal method was used to prepare iron/platinum-doped carbon nanoparticles (Fe/Pt-CNPs) with peroxidase-like activity, and combined with a paper-based microfluidic chip (P-3DμPAD) to construct a uric acid detection system, through uric acid oxidation The cascade reaction of enzymes and chromogenic reagents with Fe/Pt-CNPs uses smartphone software to analyze the chromogenic photos to achieve rapid and portable uric acid detection.
It achieves fast, sensitive and reliable uric acid detection results, with a linear range of 25-1000 μM and a detection limit of 10 μM, which meets clinical needs and has broad clinical application prospects, with low cost and simple operation.
Smart Images

Figure CN118767943A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nanomaterials and medical chemical analysis, and in particular to iron / platinum-doped carbon nanoparticles with peroxidase-like activity, and a method and application thereof for instantly detecting uric acid content. Background Art
[0002] The level of uric acid (UA) in the human body is an important biomarker for many diseases.
[0003] At present, the main methods for detecting UA include high performance liquid chromatography, capillary electrophoresis-amperometry, fluorescence, colorimetry, and chemiluminescence analysis. The clinical test of UA is to oxidize UA to generate allantoin and H2O2 by urate oxidase (UOX). H2O2 and color developer generate colored substances under the catalysis of peroxidase (POD), and the UA content is determined by UV-vis method. Natural POD has the disadvantages of easy inactivation, difficult purification, high price, and catalytic efficiency is easily affected by sensing conditions such as temperature and pH.
[0004] Peroxidase mimics (POD-like) have both the unique properties of nanomaterials and catalytic functions, and have higher catalytic efficiency, more stable properties, scalable preparation, and low price. Nanomaterials such as Fe3O4 / Au / Pt / Pd nanoparticles and CeO2 / MnO2 / GO nanosheets all have POD-like capabilities. POD-like has gradually shown its advantages in the fields of anti-oxidation, antibacterial, biosensing, bioimaging, and disease treatment.
[0005] At present, a variety of POD-like (CDs, MOFs, AuCNs, etc.) have been developed to replace natural POD in the analysis and detection of H2O2 and substances that produce H2O2 during the reaction process, such as UA, glucose, cholesterol, etc.
[0006] At present, it has been reported that the introduction of heteroatoms leads to changes in the distribution of carbon electron density, causing charge transfer between carbon atoms and heteroatoms, reducing the reaction energy barrier and accelerating the reaction. 3+ , Cu 2 +、Au 3+ , Pt 4+The transition metal ion doping of carbon nanomaterials is an effective strategy to enhance POD-like activity and provide an alternative nanozyme material for the detection of UA based on the UOX-POD-like cascade reaction.
[0007] At present, there have been reports on the detection of UA content based on materials such as carbon dot nanozymes, gold nanoclusters, and FeOOH nanorods. These methods are sensitive and accurate, but the operation is complicated and not suitable for POCT (point-of-care testing) of UA.
[0008] Microfluidics is a technology that manipulates microfluids at the micro-nano scale, also known as Lab-on-a-Chip. The main feature of microfluidic chips is the use of structures such as microchannels to control microfluids so that the fluid flows along the designed path. Paper-based microfluidic chips (μPAD) are very attractive in the field of biosensing due to their low cost, easy operation, and diverse design. They are potential candidates for POCT. In order to achieve high-sensitivity detection of the target content, new analytical methods, μPAD engineering design, intelligent detection methods, and data analysis methods have been developed.
[0009] Therefore, the development of sensitive and rapid detection of UA content based on μPAD is of great significance to improve the efficiency of clinical diagnosis of gout and related diseases, reduce acute gout attacks and alleviate the severity of attacks. Summary of the invention
[0010] The main purpose of the present invention is to provide iron / platinum-doped carbon nanoparticles with peroxidase-like activity and a preparation method thereof, and a method and application thereof for real-time detection of uric acid content, a uric acid test strip and a system for real-time detection of uric acid content, so as to realize rapid detection of UA content.
[0011] To achieve the above object, the present invention provides a method for preparing Fe / Pt-doped carbon nanozyme particles, characterized in that it comprises the steps of:
[0012] S1, dissolving neutral red, chloroplatinic acid and ferric chloride in pure water at a mass-to-liquid ratio of 2:1 according to a weight ratio of 0.8-1.2:0.8-1.2:1.8-2.2;
[0013] S2, reacting the uniformly dispersed mixed solution in step S1 in a high-pressure reactor lined with polytetrafluoroethylene at 120° C. to 150° C. for 2-4 hours and then cooling naturally;
[0014] S3, dialyzing the solution after the reaction in step S2 for 36-60 hours, and centrifuging to remove large solid particles to obtain a supernatant;
[0015] S4, freeze-drying the supernatant obtained in step S3 to obtain a brown-black powder, which is the Fe / Pt-doped carbon nanozyme particles.
[0016] Furthermore, the step S4 comprises filtering the supernatant obtained in step S3 through a filter membrane, and freeze-drying the filtered solution to obtain a brown-black powder, which is the Fe / Pt-doped carbon nanozyme particles.
[0017] Furthermore, the pore size of the filter membrane is 0.2-0.24 μm.
[0018] Furthermore, the mass ratio of neutral red, chloroplatinic acid and ferric chloride in step S1 is 1:1:2.
[0019] Furthermore, the reaction temperature in step S2 is 138° C. to 142° C., and the reaction time is 2.5-3.5 h; and the dialysis time in step S3 is 45-55 h.
[0020] The present invention also provides a Fe / Pt-doped carbon nanozyme particle, which is prepared by any of the preparation methods described above.
[0021] The present invention also provides an application of the Fe / Pt-doped carbon nanozyme particles as described above to catalyze H2O2 to generate ·OH free radicals in real-time detection of uric acid content.
[0022] The present invention also provides a uric acid detection test paper, comprising a uric acid decomposition layer located at the top and a catalytic layer located at the bottom; the uric acid decomposition layer comprises a first hydrophilic paper base region having a hydrophobic boundary and loaded with urate oxidase and a color developer, and the catalytic layer comprises a second hydrophilic paper base region having a hydrophobic boundary and loaded with Fe / Pt-doped carbon nanozyme particles prepared by any of the preparation methods described above; the uric acid decomposition layer is provided with a hole for dripping a test sample, the hole is connected to the first hydrophilic paper base region, and the first hydrophilic paper base region and the second hydrophilic paper base region are arranged to be connected.
[0023] Furthermore, the developer is 3,3',5,5'-tetramethylbenzidine.
[0024] The present invention also provides a system for real-time detection of uric acid content, comprising a uric acid test strip as described in any of the above items, a dark box and an electronic device, wherein the dark box is provided with a lighting device, a placement area for placing the uric acid test strip and a shooting hole arranged corresponding to the placement area, the electronic device is used to take a photo of the uric acid test strip after color development through the shooting hole, and the electronic device is used to analyze and compare the photo of the uric acid test strip after color development through software to obtain a corresponding uric acid content value.
[0025] In the present invention, Fe / Pt-doped carbon nanozyme particles (also known as: iron / platinum-doped carbon nanoparticles with peroxidase-like activity, Fe / Pt-CNPs) are prepared by a one-step hydrothermal method. Urate oxidase catalyzes UA to generate allantoin and H2O2, Fe / Pt-CNPs catalyze H2O2 to generate ·OH free radicals, and 3,3',5,5'-tetramethylbenzidine (TMB) is oxidized by ·OH to generate oxTMB, thereby changing the color from colorless to blue. The uric acid test strip is formed by pasting PVC label paper on the top of the hydrophilic paper base to form a pasting-3D microfluidic paper-based analytical devices (P-3DμPAD). Based on the reaction of Fe / Pt-CNPs catalyzing the oxidation of TMB, the UA level is quantified along with the color intensity of TMB on P-3DμPAD, and a colorimetric method is established to detect the UA content, and the analysis is performed with the help of a smartphone application software. The linear range and detection limit of UA detection based on P-3DμPAD are 25-1000μM and 10μM, respectively, which can fully meet the needs of clinical detection of UA. Based on the high peroxidase-like activity of Fe / Pt-CNPs nanozymes, the present invention combines portable P-3DμPAD to construct a POCT platform for UA, which provides a sensitive, rapid and reliable tool for the detection of UA in serum, and has broad application prospects in the clinical diagnosis of diseases related to UA levels. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0027] Figure 1 A is a TEM image of Fe / Pt-CNPs prepared in Example 1 (inset: particle size distribution of Fe / Pt-CNPs); Figure 1 B is the XRD spectrum of Fe / Pt-CNPs prepared in Example 1; Figure 1 C is the UV-vis absorption spectrum of Fe / Pt-CNPs prepared in Example 1; Figure 1 D is the FT-IR image of Fe / Pt-CNPs prepared in Example 1.
[0028] Figure 2 A is the full scan XPS spectrum of Fe / Pt-CNPs prepared in Example 1; Figure 2 B is the HR-XPS spectrum of Fe 2p of Fe / Pt-CNPs prepared in Example 1; Figure 2 C is the HR-XPS spectrum of O1s of Fe / Pt-CNPs prepared in Example 1; Figure 2 D is the HR-XPS spectrum of N 1s of Fe / Pt-CNPs prepared in Example 1; Figure 2 E is the HR-XPS spectrum of C1s of Fe / Pt-CNPs prepared in Example 1; Figure 2 F is the HR-XPS spectrum of Pt 4f of Fe / Pt-CNPs prepared in Example 1.
[0029] Figure 3 A is the UV-vis absorption spectrum of TMB under different reaction conditions (the inset is the corresponding solution image); Figure 3 B is the UV-vis absorption spectrum of ABTS under different reaction conditions (the inset is the corresponding solution image); Figure 3 C is the UV-vis absorption spectrum of OPD under different reaction conditions (the inset is the corresponding solution image); Figure 3 D is the absorbance variation reaction curve of TMB / H2O2 reaction system catalyzed by different concentrations of Fe / Pt-CNPs; Figure 3 E is the relative POD-like activity of Fe / Pt-CNPs under different pH conditions; Figure 3 F is the relative POD-like activity of Fe / Pt-CNPs at different temperatures.
[0030] Figure 4 This is a steady-state kinetic analysis of the POD-like activity of Fe / Pt-CNPs; wherein, (A) is a reaction curve of the absorbance variation with time of the Fe / Pt-CNPs reaction system catalyzing different concentrations of TMB; (D) is a reaction curve of the absorbance variation with time of the Fe / Pt-CNPs reaction system catalyzing different concentrations of H2O2; (B) is a curve of the relationship between the catalytic reaction rate of Fe / Pt-CNPs and the concentration of substrate TMB; (E) is a curve of the relationship between the catalytic reaction rate of Fe / Pt-CNPs and the concentration of H2O2; (C) is a Lineweaver-Burk curve kinetic diagram of TMB; (F) is a Lineweaver-Burk curve kinetic diagram of H2O2.
[0031] Figure 5 A is a schematic diagram of the principle of UA detection based on UOX-POD-like cascade reaction. Figure 5 B is the UV-vis absorption spectra of Fe / Pt-CNPs+TMB, Fe / Pt-CNPs+UA+TMB and Fe / Pt-CNPs+UOX+UA+TMB (Inset: corresponding solution image)
[0032] Figure 6 A shows the experimental data for optimizing the pH conditions for detecting UA concentration by P-3DμPAD, 6B shows the experimental data for optimizing the incubation time conditions for detecting UA concentration by P-3DμPAD, 6C shows the experimental data for optimizing the reaction temperature conditions for detecting UA concentration by P-3DμPAD, 6D shows the experimental data for optimizing the TMB concentration conditions for detecting UA concentration by P-3DμPAD, and 6E shows the experimental data for optimizing the Fe / Pt-CNPs concentration conditions for detecting UA concentration by P-3DμPAD.
[0033] Figure 7 A is a calibration curve of the Fe / Pt-doped carbon nanozyme particles obtained in Example 1 applied to the P-3DμPAD uric acid test strip to detect UA concentration B / (R+B) value and UA concentration (25-1000μM);
[0034] Figure 7 B is the B / (R+B) value and corresponding picture of the P-3DμPAD uric acid test strip detection system after adding different interfering substances and UA; Figure 7 C is the B / (R+B) value and corresponding picture of the P-3DμPAD uric acid test strip detection system in which interfering substances and UA are added together.
[0035] Figure 8 A is the schematic diagram of the structure of P-3DμPAD. Figure 8 B is a schematic diagram of a portable visible light detection device. Figure 8 C is a schematic diagram of the UA concentration analysis process using the “UASensor” software. DETAILED DESCRIPTION
[0036] The technical solution in this embodiment will be described clearly and completely below in conjunction with the drawings in this embodiment. Obviously, the described embodiment is only a part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] In addition, the technical solutions between the various embodiments of the present invention can be combined with each other, but it must be based on the fact that ordinary technicians in the field can implement it. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0038] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.
[0039] Example 1
[0040] The preparation method of Fe / Pt-doped carbon nanozyme particles in this embodiment is as follows:
[0041] Weigh 5 mg of neutral red (NR, 3-amino-7-methylamino-2-methylphenazine hydrochloride), 5 mg of chloroplatinic acid (H2PtCl6), and 10 mg of ferric chloride (FeCl3), dissolve them in 10 mL of ultrapure water, stir for 10 min until completely dispersed, transfer the solution to a high-pressure reactor lined with polytetrafluoroethylene, react at 140°C for 3 h, and then cool naturally. The reaction solution is dialyzed (MW=500) for 48 h, centrifuged to remove large particles of solid, and the supernatant is passed through a membrane (0.22 μm). The brown-black powder obtained by freeze-drying the resulting solution is Fe / Pt-CNPs.
[0042] Example 2
[0043] The preparation method of Fe / Pt-doped carbon nanozyme particles in this embodiment is as follows:
[0044] Weigh 5 mg of neutral red (NR, 3-amino-7-methylamino-2-methylphenazine hydrochloride), 5 mg of chloroplatinic acid (H2PtCl6), and 5 mg of ferric chloride (FeCl3), dissolve them in 10 mL of ultrapure water, stir for 10 min until completely dispersed, transfer the solution to a high-pressure reactor lined with polytetrafluoroethylene, react at 135 ° C for 3 h, and then cool naturally. The reaction solution is dialyzed (MW = 500) for 48 h, centrifuged to remove large particles of solid, and the supernatant is passed through a membrane (0.22 μm). The obtained solution is freeze-dried to obtain a brown-black powder, which is Fe / Pt-CNPs.
[0045] Example 3
[0046] The preparation method of Fe / Pt-doped carbon nanozyme particles in this embodiment is as follows:
[0047] Weigh 5 mg of neutral red (NR, 3-amino-7-methylamino-2-methylphenazine hydrochloride), 10 mg of chloroplatinic acid (H2PtCl6), and 10 mg of ferric chloride (FeCl3), dissolve them in 10 mL of ultrapure water, stir for 10 min until completely dispersed, transfer the solution to a high-pressure reactor lined with polytetrafluoroethylene, react at 145 ° C for 3 h, and then cool naturally. The reaction solution is dialyzed (MW = 500) for 48 h, centrifuged to remove large particles of solid, and the supernatant is passed through a membrane (0.22 μm). The obtained solution is freeze-dried to obtain a brown-black powder, which is Fe / Pt-CNPs.
[0048] Please combine Figure 1 and Figure 2 , Figure 1 A is a TEM image of Fe / Pt-CNPs prepared in Example 1 (inset: particle size distribution of Fe / Pt-CNPs); Figure 1 B is the XRD spectrum of Fe / Pt-CNPs prepared in Example 1;
[0049] Figure 1 C is the UV-vis absorption spectrum of Fe / Pt-CNPs prepared in Example 1; Figure 1 D is the FT-IR image of Fe / Pt-CNPs prepared in Example 1.
[0050] Figure 2 A is the full scan XPS spectrum of Fe / Pt-CNPs prepared in Example 1; Figure 2 B is the HR-XPS spectrum of Fe 2p of Fe / Pt-CNPs prepared in Example 1; Figure 2 C is the HR-XPS spectrum of O1s of Fe / Pt-CNPs prepared in Example 1; Figure 2 D is the HR-XPS spectrum of N1s of Fe / Pt-CNPs prepared in Example 1;
[0051] Figure 2 E is the HR-XPS spectrum of C1s of Fe / Pt-CNPs prepared in Example 1; Figure 2 F is the HR-XPS spectrum of Pt 4f of Fe / Pt-CNPs prepared in Example 1.
[0052] exist Figure 1 In A, the morphology and size of Fe / Pt-CNPs were characterized by TEM. RCDs were uniformly spherical, well dispersed, and had an average particle size of 5.5 nm. XRD spectrum of Fe / Pt-CNPs ( Figure 1 B) There is a broad and low diffraction peak at 2θ = 21.4°, which may be due to the doping of Fe and Pt, which destroys the crystal phase of graphite carbon. Figure 1As shown in C, the UV-vis spectrum of Fe / Pt-CNPs has absorption peaks at 262, 303, 340 and 540 nm. The absorption peak at 262 nm is the π→π* transition of the C=C bond in the aromatic carbon of Fe / Pt-CNPs, and the absorption peaks at 303, 340 and 540 nm are the n→π* transitions of the C=O and C=N bonds on the surface of Fe / Pt-CNPs. By FT-IR ( Figure 1 D) and XPS ( Figure 2 A) Characterization of the functional groups and elemental composition of Fe / Pt-CNPs. In the FT-IR spectrum of Fe / Pt-CNPs, there are vibration absorption peaks of OH / NH, CH, C=O / C=N, COC / CNC, and Fe-N / Fe-O bonds, indicating the presence of -OH, -COOH, -NH2, and Fe-containing functional groups.
[0053] like Figure 2 As shown in A, the full spectrum XPS of Fe / Pt-CNPs has peaks at binding energies of 710.74, 531.87, 399.01, 284.59 and 72.12 eV, indicating the presence of Fe (2.7%), O (12.21%), N (15.41%), C (65.62%) and Pt (4.07%) elements. Figure 2 B), there are four characteristic peaks at 728.6, 724.4, 714.8 and 710.8 eV, corresponding to Fe 3+ 2p 1 / 2 , Fe 2+ 2p 1 / 2 , Fe 3+ 2p 3 / 2 and Fe 2+ 2p 3 / 2 The binding energy of Fe 2+ The appearance of Fe 3+ During the hydrothermal reaction, some reduction occurred, and Fe 3+ and Fe 2+ The presence of is very beneficial to enhance the POD-like activity of Fe / Pt-CNPs and the Fenton reaction. In the high-resolution spectrum of O1s ( Figure 2 C), there are two peaks at binding energies of 532.3 and 530.8 eV, corresponding to CO and C=O, respectively. Figure 2 In D, the deconvolution results of the N 1s spectrum show two peaks at 399.6eV (graphitic N) and 398.8eV (pyridinic-N / Pyrrolic-N). The HR-XPS spectrum of C 1s is fitted with four peaks ( Figure 2E), corresponding to the binding energies of C=O (286.6 eV), CO (285.4 eV), CN (284.8 eV) and CC / C=C (284.1 eV). High-resolution spectrum of Pt 4f ( Figure 2 F) There are two peaks at 75.5eV and 72.1eV, corresponding to Pt 2+ 4f 5 / 2 and Pt 2+ 4f 7 / 2 The above results verify that Fe and Pt are successfully doped into CNPs, and metal atom doping as active sites plays a very important role in the catalytic performance of Fe / Pt-CNPs.
[0054] The POD-like activity of Fe / Pt-CNPs prepared in Example 1 was evaluated. Figure 3 As shown in (AC), through three typical color change reactions in POD-like catalysis, Fe / Pt-CNPs catalyze the oxidation of TMB, ABTS, and OPD in the presence of H2O2 to generate the oxidation products blue oxTMB (652nm), blue-green ABTS ·+ (417nm), yellow oxOPD (452nm), indicating that Fe / Pt-CNPs have POD-like activity. Similarly, as the concentration of Fe / Pt-CNPs increases, the absorbance of the TMB / H2O2 reaction system increases with the increase of reaction time ( Figure 3 D). The POD-like activity of Fe / Pt-CNPs was tested in NaAc-HAc buffer with different pH values (2.2-7.0). Figure 3 E), when pH is 4.0, Fe / Pt-CNPs reach the highest POD-like catalytic activity. As the pH increases, the POD-like activity of Fe / Pt-CNPs decreases sharply, and when it reaches 7.0, the catalytic activity is close to 0. As the temperature changes from 10℃ to 50℃, the POD-like activity gradually increases, and after 30℃, the POD-like activity tends to remain stable ( Figure 3 F).
[0055] Using 5,5-dimethyl-1-pyrroline-N-oxide (DMPO) as a free radical scavenger, the types of free radicals were verified by electron spin resonance (ESR). Figure 3In G, no obvious peaks appeared when Fe / Pt-CNPs and DMPO coexisted. In the Fe / Pt-CNPs / H2O2 / DMPO system, an obvious quartet signal with an intensity ratio of 1:2:2:1 appeared, corresponding to DMPO capture · DMPO- formed by OH · The above results prove that Fe / Pt-CNPs have POD-like activity and catalyze H2O2 to generate strong oxidizing · OH oxidizes TMB to generate oxTMB.
[0056] Please combine Figure 4 , using TMB and H2O2 as substrates, the POD-like activity of the Fe / Pt-CNPs prepared in Example 1 was systematically evaluated. Figure 4 This is a steady-state kinetic analysis of the POD-like activity of Fe / Pt-CNPs; (A) is a reaction curve of the absorbance variation over time of the Fe / Pt-CNPs reaction system catalyzing different concentrations of TMB; (D) is a reaction curve of the absorbance variation over time of the Fe / Pt-CNPs reaction system catalyzing different concentrations of H2O2; (B) is a curve of the relationship between the reaction rate of Fe / Pt-CNPs catalysis and the concentration of substrate TMB; (E) is a curve of the relationship between the reaction rate of Fe / Pt-CNPs catalysis and the concentration of H2O2; (C) is a Lineweaver-Burk curve kinetic diagram of TMB; (F) is a Lineweaver-Burk curve kinetic diagram of H2O2. In the experiment, the H2O2 concentration was first maintained at 100μM, and the TMB concentration ranged from 1-5mM. The absorbance of the reaction system at 652nm increased with time and the increase of TMB concentration ( Figure 4 A); The concentration of TMB was fixed at 3 mM, the concentration of H2O2 varied from 50 to 250 μM, and the absorbance at 652 nm of the reaction system increased with time and the increase of H2O2 concentration ( Figure 4 D) Figure 4 As shown in Figures B and 4E, with the increase of the concentration of substrates TMB and H2O2, the catalytic rate of Fe / Pt-CNPs gradually increased and finally reached a plateau. The enzyme-like catalysis of Fe / Pt-CNPs conforms to the Michaelis-Menten kinetic equation. Figure 4 C and 4F, the double inverse of the kinetic curve was taken and fitted with the Lineweaver-Burk equation. When TMB was used as the substrate, the K m 0.97mM, V max 3.8×10 -8 Ms -1 ; With H2O2 as substrate, the Km 2.3mM, V max 7.41×10 -7 Ms -1 As shown in Table 1, compared with the kinetic parameters of other nanozymes, Fe / Pt-CNPs have good POD-like activity.
[0057] Table 1. Comparison of kinetic parameters of Fe / Pt-CNPs with reported nanozymes
[0058]
[0059] Please combine Figure 5 , Figure 5 A is a schematic diagram of the principle of UA detection based on UOX-POD-like cascade reaction. Figure 5 B is the UV-vis absorption spectra of Fe / Pt-CNPs+TMB, Fe / Pt-CNPs+UOX+TMB and Fe / Pt-CNPs+UOX+UA+TMB (inset: corresponding solution image).
[0060] The present invention is based on the UOX-Fe / Pt-CNPs cascade reaction system, and the UA colorimetric sensing mechanism is as follows: Figure 5 A): When UA is present in the reaction system, UOX catalyzes the oxidation of UA to generate allantoin and H2O2; Fe / Pt-CNPs have POD-like activity, catalyzing H2O2 to oxidize colorless TMB to generate blue oxTMB. The UA concentration is calculated based on the amount of oxTMB generated. Figure 5 As shown in Figure B, when Fe / Pt-CNPs and TMB are added to the reaction solution of UOX and UA, the characteristic absorption peak of the UV-vis absorption spectrum of the reaction system at 652 nm increases significantly. This is because the H2O2 generated by the reaction of UOX and UA undergoes a cascade reaction with Fe / Pt-CNPs and TMB, oxidizing TMB to generate oxTMB, and the maximum absorption wavelength of oxTMB is at 652 nm.
[0061] Please refer to Figure 8 A, by pasting a hydrophobic substrate layer (e.g., a PVC hydrophobic barrier) onto a hydrophilic paper substrate, a pasting-3D microfluidic paper-based analytical device (P-3DμPAD) uric acid test strip is constructed; the P-3DμPAD uric acid test strip includes a uric acid (UA) decomposition layer (1 st ) and the catalytic layer (2 nd); the uric acid decomposition layer comprises a first hydrophilic paper-based region having a hydrophobic boundary and loaded with urate oxidase and a color developer, and the catalytic layer comprises a second hydrophilic paper-based region having a hydrophobic boundary and loaded with Fe / Pt-doped carbon nanozyme particles prepared by any of the preparation methods described above; the uric acid decomposition layer is provided with a hole for dripping a test sample, the hole is connected to the first hydrophilic paper-based region, and the first hydrophilic paper-based region and the second hydrophilic paper-based region can be connected (for example, by overlapping and bonding).
[0062] Specifically, when preparing the first hydrophilic paper base area, Tris-HCl (0.01M, pH=8.0) buffer solution, urate oxidase and a color developer can be dropped on the first hydrophilic paper base area with a hydrophobic boundary, and then dried at room temperature for about 10 minutes; similarly, when preparing the second hydrophilic paper base area, NaAc-HAc (0.01M, pH=4.0) buffer solution and Fe / Pt-doped carbon nanozyme particles can be dropped on the second hydrophilic paper base area with a hydrophobic boundary; then the two are bonded to obtain the P-3DμPAD uric acid test strip.
[0063] Specifically, the first hydrophilic paper base area and the second hydrophilic paper base area can be directly bonded together, or they can be connected and bonded during the detection process (a tearable protective film can be attached to the first hydrophilic paper base area and the second hydrophilic paper base area, and the protective film can be torn off during use before bonding on site).
[0064] Please refer to Figure 8 B and 8C, in order to obtain the colorimetric image of the detection layer more conveniently and accurately, the system design for real-time detection of uric acid content includes a portable visible light detection device (dark box + portable UV lamp) and the "UA Sensor" application. The P-3DμPAD is placed in the portable detection device, and the smartphone "UA Sensor" application is opened. The image is collected through the smartphone, and the RGB value is analyzed to obtain the UA content value directly and in real time.
[0065] Please refer to Figure 6 By conducting experiments on different conditions for the P-3DμPAD uric acid test strip to detect UA concentration, the following results were obtained: Figure 6 A shows the experimental data for optimizing the pH conditions for detecting UA concentration by P-3DμPAD, 6B shows the experimental data for optimizing the incubation time conditions for detecting UA concentration by P-3DμPAD, 6C shows the experimental data for optimizing the reaction temperature conditions for detecting UA concentration by P-3DμPAD, 6D shows the experimental data for optimizing the TMB concentration conditions for detecting UA concentration by P-3DμPAD, and 6E shows the experimental data for optimizing the Fe / Pt-CNPs concentration conditions for detecting UA concentration by P-3DμPAD.
[0066] The optimal UA detection conditions for P-3DμPAD to detect UA concentration are: 1 st UA decomposition layer: Tris-HCl (0.01M, pH=8.0) buffer, UOX activity is 10000U L -1 , incubate at 37°C for 15 min; 2 nd Catalytic layer NaAc-HAc (0.01 M, pH = 4.0) buffer, TMB concentration of 50 mM, Fe / Pt-CNPs concentration of 9 μg L -1 .
[0067] Please combine Figure 7 ,like Figure 7 As shown in A, when the UA concentration increases, the color of the detection layer changes significantly from light blue to dark blue. The B / (R+B) value is linearly related to the UA concentration (25-1000 μM), and the linear fitting equation is y=0.00045x+0.4942(R 2 0.9889), and the LOD is 10μM (S / N 3). Here we use the UA concentration of 420μM as the dividing line. When the UA concentration is 190-420μM, it belongs to the normal UA range, and the paper base is light blue; when the UA concentration is greater than 420μM, it is in the high-risk range, and the color of the paper base is dark blue. As shown in Table 2, although the LOD of UA detection based on P-3DμPAD is not as good as the detection results based on large instruments, the linear range and minimum detection limit of UA detection based on P-3DμPAD can meet the detection of healthy / high uric acid populations, and it has the advantages of portability, rapidity, low cost and easy operation, so that it can realize on-site monitoring of UA in daily life applications.
[0068] Table 2. Comparison of the present method with reported ALP detection methods
[0069]
[0070] Select common metal ions (Na + Mg 2+ , K + ,Ca 2+ ), small molecules (L-Gly, L-Glu, Cre, Glu) and biomacromolecules (ALP, GOX) as interferences to explore the selectivity and anti-interference ability of P-3DμPAD in detecting UA. Figure 7 As shown in B, when P-3DμPAD detects UA, the paper base turns blue and the B / (R+B) ratio increases. After reacting with other interfering substances, the color of the detection layer remains basically unchanged. Figure 7As shown in Figure C, after the interfering substances were added to the reaction system together with UA, the B / (R+B) ratio of the detection system remained basically unchanged. Therefore, the P-3DμPAD system has excellent selectivity and strong anti-interference ability in detecting UA content, indicating that P-3DμPAD is practical in detecting UA content in actual samples.
[0071] Similarly, the Fe / Pt-CNPs prepared in Example 2 and Example 3 were used to construct P-3DμPAD uric acid detection test strips, and also a good color development effect was obtained.
[0072] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing Fe / Pt-doped carbon nanozyme particles, characterized in that: Includes steps: S1, dissolving neutral red, chloroplatinic acid and ferric chloride in pure water at a weight ratio of 0.8-1.2:0.8-1.2:1.8-2.2 and a mass-to-liquid ratio of 1.8-2.2:1; S2, reacting the uniformly dispersed mixed solution in step S1 in a high-pressure reactor lined with polytetrafluoroethylene at 120° C. to 150° C. for 2-4 hours and then cooling naturally; S3, dialyzing the solution after the reaction in step S2 for 36-60 hours, and centrifuging to remove large solid particles to obtain a supernatant; S4, freeze-drying the supernatant obtained in step S3 to obtain a brown-black powder, which is the Fe / Pt-doped carbon nanozyme particles.
2. The method according to claim 1, characterized in that The step S4 comprises filtering the supernatant obtained in step S3 through a filter membrane, and freeze-drying the filtered solution to obtain a brown-black powder, which is the Fe / Pt-doped carbon nanozyme particles.
3. The method according to claim 2, characterized in that The membrane pore size of the filter membrane is 0.2-0.24 μm.
4. The method according to claim 1, characterized in that: The mass ratio of neutral red, chloroplatinic acid and ferric chloride in step S1 is 1:1:
2.
5. The method according to claim 1, characterized in that The reaction temperature in step S2 is 138° C. to 142° C., and the reaction time is 2.5-3.5 h; the dialysis time in step S3 is 45-55 h.
6. A Fe / Pt-doped carbon nanozyme particle, characterized in that: The method is prepared according to any one of claims 1 to 5.
7. A use of the Fe / Pt-doped carbon nanozyme particles as claimed in claim 6 for catalyzing H2O2 to generate ·OH free radicals in real-time detection of uric acid content.
8. A uric acid test strip, characterized in that: The invention comprises a uric acid decomposition layer located at the top and a catalytic layer located at the bottom; the uric acid decomposition layer comprises a first hydrophilic paper base region having a hydrophobic boundary and loaded with urate oxidase and a color developer, and the catalytic layer comprises a second hydrophilic paper base region having a hydrophobic boundary and loaded with Fe / Pt-doped carbon nanozyme particles prepared by the preparation method described in any one of claims 1 to 5; the uric acid decomposition layer is provided with a hole for dripping a test sample, the hole is connected to the first hydrophilic paper base region, and the first hydrophilic paper base region and the second hydrophilic paper base region are arranged to be connectable.
9. The uric acid test strip according to claim 8, characterized in that: The color developer is 3,3',5,5'-tetramethylbenzidine.
10. A system for real-time detection of uric acid content, characterized in that: The invention comprises a uric acid test strip as described in any one of claims 8 to 9, a dark box and an electronic device, wherein the dark box is provided with a lighting device, a placement area for placing the uric acid test strip and a shooting hole arranged corresponding to the placement area, the electronic device is used to take a photo of the uric acid test strip after color development through the shooting hole, and the electronic device is used to analyze and compare the photo of the uric acid test strip after color development through software to obtain a corresponding uric acid content value.
Citation Information
Patent Citations
Nitrogen-doped graphene quantum dot-iron ion composite nano-enzyme and preparation and application thereof
CN113289654A
Preparation method and application of uricase mimic enzyme
CN113447453A
Preparation method and application of multi-enzyme active nano-enzyme fluorescent hydrogel
CN115386105A
Preparation method of iron monatomic doped fluorescent carbon dot nano-enzyme
CN115920890A
Novel uric acid test paper
CN116482090A