Inhibitor for ore flotation and preparation method and application thereof
Through the combined inhibitor of acidified water glass and naphthalene sulfonate polymer surfactant, the problems of high inhibitor toxicity and complicated process in fluorite ore flotation in the existing technology are solved, and the synthesis of calcite and barite is realized. Effective separation and efficient utilization of resources simplify the flotation process, and the inhibitor is green, environmentally friendly and highly safe.
Patent Information
- Application Number
- CN202411100614.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing fluorite ore flotation process, the inhibitors used, such as iron chromium lignosulfonate and potassium dichromate, are highly toxic agents, and cannot effectively separate barite and calcite when used alone. The common combined inhibitor process is complex and requires It is difficult to achieve a green, environmentally friendly and simple flotation process by adjusting the pH value multiple times.
A combined inhibitor of acidified water glass and naphthalene sulfonate polymer surfactant is used, prepared by ultrasonic mixing to form an inhibitor with a mass ratio of 3:2, and mixed with deionized water for use in fluorite ore flotation. , simplifying the process and replacing traditional highly toxic agents.
It achieves the effective separation of calcite and barite in fluorite ore, simplifies the flotation process, reduces the need for pH adjustment, improves the comprehensive utilization level of resources, and the inhibitor is green, environmentally friendly and highly safe.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of mineral processing, and in particular to an inhibitor for ore flotation, a preparation method thereof and an application thereof. Background Art
[0002] At present, my country's fluorite resources are seriously lacking and difficult to mine. Therefore, the development and utilization of associated (symbiotic) fluorite resources have received widespread attention. Associated minerals include barite, calcite, and a small amount of celestite and dolomite. Common fluorite collectors include oleic acid and sodium oleate. When sodium oleate is used as a collector, since the surface properties of fluorite, barite and calcite are similar and their floatability is similar, a good inhibitor is needed to effectively separate barite and calcite from fluorite.
[0003] At present, when sodium oleate is used as a collector, common inhibitors include fulvic acid, tannin extract, xanthan gum, acidified water glass, lignin sulfonate ferrochromium, potassium dichromate, etc. Among them, lignin sulfonate ferrochromium and potassium dichromate are highly toxic agents, which are extremely harmful to the human body and the environment. When the above inhibitors are used alone, barite and calcite cannot be inhibited at the same time. Therefore, in common flotation operations, combined inhibitors are usually used, and the current common combined inhibitor flotation process is complicated. For example, before adding each inhibitor, it is necessary to gradually adjust the inhibition conditions such as pH value. Therefore, there is an urgent need for a green and environmentally friendly fluorite flotation inhibitor with a simple flotation process. Summary of the invention
[0004] In view of the deficiencies of the prior art, the present invention provides an inhibitor for ore flotation, a preparation method thereof and an application thereof. The inhibitor is green and environmentally friendly, has a simple preparation method and is easy to use.
[0005] A first aspect of the present invention provides an inhibitor for ore flotation, the inhibitor comprising acidified water glass, naphthalenesulfonate polymer surfactant and deionized water, wherein the mass ratio of the acidified water glass to the naphthalenesulfonate polymer surfactant is 3:2.
[0006] Preferably, the naphthalenesulfonate polymer surfactant is an amino-terminated polyether silicone surfactant modified with naphthalenesulfonate.
[0007] According to a second aspect of the present invention, there is provided a method for preparing an inhibitor for ore flotation, the method comprising the following steps:
[0008] Step S1, weighing acidified water glass and naphthalenesulfonate polymer surfactant according to proportion;
[0009] Step S2, adding deionized water to the acidified water glass, wherein the volume ratio of the acidified water glass to the deionized water is 1:1;
[0010] Step S3, adding deionized water to the naphthalenesulfonate polymer surfactant, wherein the volume ratio of the naphthalenesulfonate polymer surfactant to the deionized water is 1:1;
[0011] Step S4: mixing the acidified water glass solution prepared in the above steps S2 and S3 and the naphthalenesulfonate polymer surfactant aqueous solution under ultrasonic conditions for 30 minutes to obtain an inhibitor for ore flotation.
[0012] Furthermore, the preparation method of the naphthalenesulfonate polymer surfactant comprises the following steps:
[0013] Step a, adding 30-40 parts of deionized water into a three-necked flask, starting reflux, heating to 80° C. under nitrogen protection, successively adding 0.1-0.5 parts of sodium dodecylbenzene sulfonate, 2-6 parts of n-butanol and 2-4 parts of amino-terminated polyether silicone into the three-necked flask, and stirring for 30 minutes;
[0014] Step b, continue to add 1-2 parts of concentrated sulfuric acid into the three-necked flask and continue the reaction for 30 minutes;
[0015] Step c, mixing 2 to 5 parts of naphthalenesulfonate with 3 to 10 parts of ethanol under ultrasonic conditions for 30 minutes to obtain a mixed solution;
[0016] Step d: adding the mixed solution in step c into a three-necked flask, reacting for 2 to 6 hours, and cooling to room temperature to obtain a naphthalenesulfonate polymer surfactant.
[0017] Furthermore, the acidified water glass is prepared by the following method: adding water glass into a sulfuric acid solution, wherein the mass ratio of water glass to sulfuric acid solution is 5:1.
[0018] Furthermore, the concentration of the sulfuric acid solution is 50% to 70%.
[0019] According to a third aspect of the present invention, there is provided a depressant prepared by the depressant for ore flotation according to the first aspect of the present invention or the method for preparing the depressant for ore flotation according to the second aspect of the present invention, for use in fluorite ore flotation.
[0020] Furthermore, the application is:
[0021] 1) crushing and grinding the ore, then adding a collector to mix, so that the collector is dispersed in the material and adding water to slurry to form a slurry with a concentration of 30-50wt%;
[0022] 2) adding a pH adjuster to the slurry to adjust the pH of the slurry to 7.0;
[0023] 3) adding the inhibitor to the ore pulp with adjusted pH value, wherein the inhibitor is added in an amount of 50 to 100 g per ton of ore pulp;
[0024] 4) Bubbles are formed by mechanical stirring, and the foam layer is collected and dried to obtain fluorite ore.
[0025] Furthermore, the collector is sodium oleate, and the amount of sodium oleate used is 200 to 600 g.
[0026] Furthermore, the pH regulator is sodium hydroxide.
[0027] The present invention provides an inhibitor for ore flotation, a preparation method and an application thereof. The inhibitor for ore flotation uses acidified water glass and naphthalene sulfonate polymer surfactant as main components, has simple components, is green and environmentally friendly, and replaces traditional highly toxic agents such as lignin sulfonate iron chromium and potassium dichromate. The inhibitor for ore flotation provided by the present invention has good inhibitory ability for calcite and barite in minerals such as phosphate ore and fluorite ore.
[0028] The inhibitor for ore flotation prepared by the method of the present invention has a simple preparation process and does not require multiple additions of the inhibitor during use, thereby eliminating the step of adjusting the pH value of the system required for each addition of the inhibitor, shortening the flotation process, reducing the difficulty of flotation, and thus improving the level of comprehensive resource utilization. DETAILED DESCRIPTION
[0029] Now will refer to various embodiments of the present invention in detail, and its embodiment is described below.Although the present invention will be described together with exemplary embodiments of the present invention, it should be understood that this description is not intended to limit the present invention to those exemplary embodiments.On the other hand, the present invention is intended to not only cover the exemplary embodiments of the present invention, but also to cover various substitutes, modifiers, equivalents and other embodiments, which can be included in the spirit and scope of the present invention defined by the appended claims.
[0030] Hereinafter, exemplary embodiments of the present invention will be described in detail. The specific structures and functions described in the exemplary embodiments of the present invention are for illustrative purposes only. Embodiments according to the concepts of the present invention can be implemented in various forms, and it should be understood that they should not be interpreted as being limited to the exemplary embodiments described in the exemplary embodiments, but include all modifications, equivalents or substitutes included in the spirit and scope of the present invention.
[0031] It should be understood that although the terms "first", "second", etc. may be used herein to describe various elements, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. For example, the first element discussed below may be referred to as the second element without departing from the teachings of the present invention. Similarly, the second element may also be referred to as the first element.
[0032] Throughout the specification, the professional terms used herein are only for describing various exemplary embodiments and are not intended to be limiting. It will be further understood that the terms "include", "comprising", "having", etc., when used in the exemplary embodiments, specifically refer to the presence of the stated parts, steps, operations or elements, but do not exclude the presence or addition of one or more other parts, steps, operations or elements.
[0033] The first aspect of the present invention provides an inhibitor for ore flotation, the inhibitor comprising acidified water glass, naphthalenesulfonate polymer surfactant and deionized water, wherein the mass ratio of the acidified water glass to the naphthalenesulfonate polymer surfactant is 3:2. The naphthalenesulfonate polymer surfactant is an amino-terminated polyether silicone surfactant modified with naphthalenesulfonate.
[0034] In the ore flotation inhibitor provided by the present invention, the naphthalene ring of the naphthalenesulfonate polymer surfactant and the S=O group in the sulfonate can produce a complex reaction on the surface of barite, strongly hindering the adsorption of the collector sodium oleate on its surface, acidifying SiO3 in the water glass, and 2- The Si-O functional groups of the ions strongly act on the surface of calcite to form fine H2SiO3 colloid particles, which strongly hinder the adsorption of sodium oleate on the surface of calcite, thereby producing a good inhibitory effect on calcite. Therefore, the inhibitor for ore flotation provided by the present invention has good inhibitory ability for both calcite and barite.
[0035] According to a second aspect of the present invention, there is provided a method for preparing an inhibitor for ore flotation, the method comprising the following steps:
[0036] Step S1, weighing acidified water glass and naphthalenesulfonate polymer surfactant in proportion; wherein the mass ratio of acidified water to naphthalenesulfonate polymer surfactant is 3:2. Step S2, adding deionized water to the acidified water glass, wherein the volume ratio of the acidified water glass to the deionized water is 1:1; Step S3, adding deionized water to the naphthalenesulfonate polymer surfactant, wherein the volume ratio of the naphthalenesulfonate polymer surfactant to the deionized water is 1:1; Step S4, mixing the acidified water glass solution prepared in the above steps S2 and S3 and the naphthalenesulfonate polymer surfactant aqueous solution under ultrasonic conditions for 30 minutes. Using ultrasonic mixing can promote the dissolution of the acidified water glass and the naphthalenesulfonate polymer surfactant in water, thereby improving their activity.
[0037] In addition, the acidified water glass used in the present invention is prepared by the following method: adding water glass to a sulfuric acid solution, wherein the mass ratio of water glass to sulfuric acid solution is 5:1, and the concentration of the sulfuric acid solution is 50% to 70%.
[0038] Further, in some embodiments, the preparation method of the naphthalenesulfonate polymer surfactant of the present invention comprises the following steps: step a, adding 30 to 40 parts of deionized water into a three-necked flask, starting reflux, heating to 80°C under nitrogen protection, successively adding 0.1 to 0.5 parts of sodium dodecylbenzene sulfonate, 2 to 6 parts of n-butanol and 2 to 4 parts of amino-terminated polyether silicone into the three-necked flask, and stirring for 30 minutes; step b, continuing to add 1 to 2 parts of concentrated sulfuric acid into the three-necked flask, and continuing to react for 30 minutes; step c, mixing 2 to 5 parts of naphthalenesulfonate with 3 to 10 parts of ethanol under ultrasonic conditions for 30 minutes to obtain a mixed solution; step d, adding the mixed solution in step c into the three-necked flask, reacting for 2 to 6 hours, and cooling to room temperature, thereby obtaining a naphthalenesulfonate polymer surfactant.
[0039] The method of the present invention uses naphthalenesulfonate to modify the surface of amino-terminated polyether organosilicon. Before use, naphthalenesulfonate polymer surfactant can be prepared in batches, and its properties are stable and not easy to deteriorate. Then, in the process of ore flotation, it is directly ultrasonically mixed with acidified water glass, and it is ready for use, and the preparation process is simple. The above method is described in detail through specific examples.
[0040] Example 1
[0041] Preparation of depressants for ore flotation:
[0042] Preparation of naphthalenesulfonate polymer surfactant: add 30 parts of deionized water into a three-necked flask, start reflux, heat to 80°C under nitrogen protection, then add 0.3 parts of sodium dodecylbenzenesulfonate (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.), 5 parts of n-butanol (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) and 3 parts of amino-terminated polyether silicone (purchased from Yangzhou Chenhua New Materials Co., Ltd.) into the three-necked flask successively, and stir for 30 minutes; continue to add 1 part of concentrated sulfuric acid into the three-necked flask, and continue to react for 30 minutes; mix 3 parts of naphthalenesulfonate with 5 parts of ethanol under ultrasonic conditions for 30 minutes to obtain a mixed solution; add the above mixed solution into the three-necked flask, react for 2 hours, and cool to room temperature to obtain a naphthalenesulfonate polymer surfactant.
[0043] The invention discloses a method for preparing an inhibitor for ore flotation: adding water glass to a sulfuric acid solution with a concentration of 50%, wherein the mass ratio of the water glass to the sulfuric acid solution is 5:1, and then weighing acidified water glass and a naphthalenesulfonate polymer surfactant in proportion; adding deionized water to the acidified water glass, wherein the volume ratio of the acidified water glass to the deionized water is 1:1; adding deionized water to the naphthalenesulfonate polymer surfactant, wherein the volume ratio of the naphthalenesulfonate polymer surfactant to the deionized water is 1:1; and mixing the acidified water glass solution and the naphthalenesulfonate polymer surfactant aqueous solution for 30 minutes under ultrasonic conditions to obtain an inhibitor for ore flotation.
[0044] Example 2
[0045] Preparation of depressants for ore flotation:
[0046] Preparation of naphthalenesulfonate polymer surfactant: add 40 parts of deionized water into a three-necked flask, start reflux, heat to 80°C under nitrogen protection, then add 0.5 parts of sodium dodecylbenzenesulfonate, 6 parts of n-butanol and 4 parts of amino-terminated polyether silicone into the three-necked flask successively, and stir for 30 minutes; continue to add 2 parts of concentrated sulfuric acid into the three-necked flask, and continue to react for 30 minutes; mix 5 parts of naphthalenesulfonate with 10 parts of ethanol under ultrasonic conditions for 30 minutes to obtain a mixed solution; add the above mixed solution into the three-necked flask, react for 3 hours, and cool to room temperature, thereby obtaining a naphthalenesulfonate polymer surfactant.
[0047] The invention discloses a method for preparing an inhibitor for ore flotation: adding water glass to a sulfuric acid solution with a concentration of 70%, wherein the mass ratio of the water glass to the sulfuric acid solution is 5:1, and then weighing acidified water glass and a naphthalenesulfonate polymer surfactant in proportion; adding deionized water to the acidified water glass, wherein the volume ratio of the acidified water glass to the deionized water is 1:1; adding deionized water to the naphthalenesulfonate polymer surfactant, wherein the volume ratio of the naphthalenesulfonate polymer surfactant to the deionized water is 1:1; and mixing the acidified water glass solution and the naphthalenesulfonate polymer surfactant aqueous solution for 30 minutes under ultrasonic conditions to obtain an inhibitor for ore flotation.
[0048] Example 3
[0049] Preparation of depressants for ore flotation:
[0050] Preparation of naphthalenesulfonate polymer surfactant: add 35 parts of deionized water into a three-necked flask, start reflux, heat to 80°C under nitrogen protection, then add 0.1 parts of sodium dodecylbenzenesulfonate, 2 parts of n-butanol and 2 parts of amino-terminated polyether silicone into the three-necked flask successively, and stir for 30 minutes; continue to add 1.5 parts of concentrated sulfuric acid into the three-necked flask, and continue to react for 30 minutes; mix 2 parts of naphthalenesulfonate with 3 parts of ethanol under ultrasonic conditions for 30 minutes to obtain a mixed solution; add the above mixed solution into the three-necked flask, react for 6 hours, and cool to room temperature, thereby obtaining a naphthalenesulfonate polymer surfactant.
[0051] The invention discloses a method for preparing an inhibitor for ore flotation: adding water glass to a sulfuric acid solution with a concentration of 60%, wherein the mass ratio of the water glass to the sulfuric acid solution is 5:1, and then weighing acidified water glass and a naphthalenesulfonate polymer surfactant in proportion; adding deionized water to the acidified water glass, wherein the volume ratio of the acidified water glass to the deionized water is 1:1; adding deionized water to the naphthalenesulfonate polymer surfactant, wherein the volume ratio of the naphthalenesulfonate polymer surfactant to the deionized water is 1:1; and mixing the acidified water glass solution and the naphthalenesulfonate polymer surfactant aqueous solution for 30 minutes under ultrasonic conditions to obtain an inhibitor for ore flotation.
[0052] The third aspect of the present invention provides an application of an inhibitor prepared by the method for preparing the inhibitor for ore flotation according to the first aspect or the second aspect in the flotation of fluorite ore. The application is as follows: 1) crushing and grinding the ore, then adding a collector to mix, so that the collector is dispersed in the material and adding water to adjust the slurry to form a slurry with a concentration of 30-50wt%, preferably 30-45wt%, and more preferably 35-40wt%; 2) adding a pH adjuster to the slurry to make the pH of the slurry 7.0; 3) adding the inhibitor to the slurry with adjusted pH value, the amount of the inhibitor added is 50-100g of the inhibitor per ton of slurry, preferably 50-80g, and more preferably 60-70g; 4) forming bubbles by mechanical stirring, collecting and drying the foam layer to obtain fluorite ore.
[0053] In some embodiments, the collector is sodium oleate, and the amount of sodium oleate added per ton of pulp is 200-600g, preferably 200-500g, and more preferably 200g-300g. In fact, the collector can also be oleic acid, and the amount of oleic acid can be adjusted according to the specific use. Further, the pH adjuster of the present invention uses sodium hydroxide. When the adjusted pH value exceeds 7.0, dilute sulfuric acid (concentration of 50%-70%, preferably 50%) can also be added to further adjust the pH.
[0054] In the application process of the inhibitor for ore flotation of the present invention, there is no need to add different inhibitors in batches. The combined inhibitor of the present invention can be directly used to inhibit calcite and barite in fluorite, and in the subsequent bubbling process, the fluorite can be floated to obtain fluorite ore.
[0055] The inhibitory effects of the inhibitors of Examples 1 to 3 of the present invention on calcite and barite are verified by test examples below.
[0056] Test example
[0057] The test example uses a single-head ore grinder to grind the ore. Before grinding, the ore is first crushed, and then a sodium oleate collector is added for mixing, so that the sodium oleate is dispersed in the material and water is added for slurry adjustment, thereby forming a slurry with a concentration of 45wt% (in fact, the slurry concentration only needs to be guaranteed to be 30-45wt% in actual applications, and the concentration within this range will not have any effect on the use of the inhibitor), and then the pH value of the solution is adjusted to 7.0 using sodium hydroxide, and the inhibitor in the embodiment of the present invention is added to the slurry with the adjusted pH value. The amount of the inhibitor added is 100g of the inhibitor per ton of slurry (similarly, the inhibitor can achieve the inhibitory effect as long as 80-100g is added per ton of slurry during actual use, and the inhibitor will not have a special effect on the inhibitory effect as long as it is within this range); then mechanical stirring is used to form bubbles, the foam layer is collected, and the grade of CaFe2 (fluorite ore) and the flotation rate of barite and calcite are tested.
[0058] Table 1 below shows the grade of CaFe2 (fluorite ore) obtained by applying the flotation depressants of Examples 1 to 3 to the flotation of fluorite ore.
[0059] Table 1
[0060] Example <![CDATA[Grade (%) of CaFe2 (fluorite ore)]]> 1 90.23 2 91.57 3 90.21
[0061] Table 2 below shows the flotation rates of barite and calcite in the flotation of fluorite ore according to the flotation depressants of Examples 1 to 3.
[0062] Table 2
[0063] Example Barite floating rate (%) Calcite floating rate (%) 1 2.3 0.3 2 2.1 0.5 3 2.7 0.7
[0064] It can be seen from the above data that the ore flotation inhibitor prepared by the method of the present invention has a good inhibitory effect on barite and calcite, and the fluorite ore floated out has a high grade.
[0065] The foregoing description of specific exemplary embodiments of the present invention has been presented for the purpose of illustration and description. It is not intended to exclude or limit the present invention to the precise form disclosed, and it is obvious that many modifications and changes are feasible in view of the above teachings. Exemplary embodiments are selected and described to explain certain principles of the present invention and their practical application, so that other technicians in the field can make or use various exemplary embodiments of the present invention, and various alternatives and modifications thereof. It is intended that the scope of the present invention will be defined by the claims attached hereto and their equivalents.
[0066] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A depressant for ore flotation, characterized in that: The inhibitor comprises acidified water glass, naphthalenesulfonate polymer surfactant and deionized water, and the mass ratio of the acidified water glass to the naphthalenesulfonate polymer surfactant is 3:
2.
2. The depressant for ore flotation according to claim 1, characterized in that: The naphthalenesulfonate polymer surfactant is an amino-terminated polyether silicone surfactant modified with naphthalenesulfonate.
3. A method for preparing an inhibitor for ore flotation, characterized in that: The method comprises the following steps: Step S1, weighing acidified water glass and naphthalenesulfonate polymer surfactant according to proportion; Step S2, adding deionized water to the acidified water glass, wherein the volume ratio of the acidified water glass to the deionized water is 1:1; Step S3, adding deionized water to the naphthalenesulfonate polymer surfactant, wherein the volume ratio of the naphthalenesulfonate polymer surfactant to the deionized water is 1:1; Step S4: mixing the acidified water glass solution prepared in the above steps S2 and S3 and the naphthalenesulfonate polymer surfactant aqueous solution under ultrasonic conditions for 30 minutes to obtain an inhibitor for ore flotation.
4. The method for preparing an inhibitor for ore flotation according to claim 3, characterized in that: The preparation method of the naphthalenesulfonate polymer surfactant comprises the following steps: Step a, adding 30-40 parts of deionized water into a three-necked flask, starting reflux, heating to 80° C. under nitrogen protection, successively adding 0.1-0.5 parts of sodium dodecylbenzene sulfonate, 2-6 parts of n-butanol and 2-4 parts of amino-terminated polyether silicone into the three-necked flask, and stirring for 30 minutes; Step b, continue to add 1-2 parts of concentrated sulfuric acid into the three-necked flask and continue the reaction for 30 minutes; Step c, mixing 2 to 5 parts of naphthalenesulfonate with 3 to 10 parts of ethanol under ultrasonic conditions for 30 minutes to obtain a mixed solution; Step d: adding the mixed solution in step c into a three-necked flask, reacting for 2 to 6 hours, and cooling to room temperature to obtain a naphthalenesulfonate polymer surfactant.
5. The method for preparing an inhibitor for ore flotation according to claim 3 or 4, characterized in that: The acidified water glass is prepared by the following method: adding water glass into a sulfuric acid solution, wherein the mass ratio of water glass to sulfuric acid solution is 5:
1.
6. The method for preparing an inhibitor for ore flotation according to claim 5, characterized in that: The concentration of the sulfuric acid solution is 50% to 70%.
7. Use of the inhibitor for ore flotation according to claim 1 or 2 or the inhibitor prepared by the method for preparing the inhibitor for ore flotation according to any one of claims 3 to 6 in fluorite ore flotation.
8. The use according to claim 7, characterized in that: The application is: 1) crushing and grinding the ore, then adding a collector to mix, so that the collector is dispersed in the material and adding water to slurry to form a slurry with a concentration of 30-50wt%; 2) adding a pH adjuster to the slurry to adjust the pH of the slurry to 7.0; 3) adding the inhibitor to the ore pulp with adjusted pH value, wherein the inhibitor is added in an amount of 50 to 100 g per ton of ore pulp; 4) Bubbles are formed by mechanical stirring, and the foam layer is collected and dried to obtain fluorite ore.
9. The use according to claim 8, characterized in that: The collector is sodium oleate, and the dosage of the sodium oleate is 200-600g.
10. The use according to claim 8, characterized in that: The pH regulator is sodium hydroxide.
Citation Information
Cited By
Beneficiation method for magnesium-containing carbonate type low-grade fluorite mine
CN119237164A
Composite collecting agent, composite reagent and application of composite collecting agent and composite reagent in scheelite flotation
CN119565780A