Inductor sintering material with high magnetic conductivity

By introducing LiMn6Sn6 single crystal material into the inductor sintered material and using secondary ball milling and secondary sintering processes, combined with PVA glue, sodium bismuthate, and sodium molybdate, the problems of insufficient magnetic permeability and high porosity of the inductor sintered material are solved. problem, achieving higher magnetic permeability and density, improving the overall performance of the inductor.

CN118771872AActive Publication Date: 2024-10-15INNER MONGOLIA ERDOS ELECTRONIC CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410753178.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-15
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

Existing inductor sintered materials have insufficient magnetic permeability, high porosity and uneven grain growth, which limits the performance improvement and application scope expansion of inductors.

Method used

LiMn6Sn6 single crystal material is introduced and through secondary ball milling and secondary sintering, the magnetic permeability and density of the sintered material are improved, and the porosity is reduced. PVA glue is used for granulation and pressing, and sodium bismuthate and sodium molybdate are added to Enhance the mixing uniformity and density of materials.

Benefits of technology

The magnetic permeability of the sintered material is significantly improved, the porosity and coercive force are reduced, the resistance to magnetic domain movement and domain wall displacement is reduced, eddy current loss and energy loss are reduced, and the overall performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771872A_ABST
    Figure CN118771872A_ABST
Patent Text Reader

Abstract

The invention discloses an inductor sintering material with high magnetic conductivity in the technical field of inductor sintering materials. A preparation process of the inductor sintering material comprises the following steps: S1, preparing a LiMn6Sn6 single crystal material; s2, primary ball milling; s3, pre-sintering is carried out; s4, secondary ball milling; s5, performing granulation; and S6, secondary sintering. The LiMn6Sn6 single crystal material is introduced, ferromagnetic coupling between Mn3 layers and magnetic coupling between Sn2Li and Mn3 layers are promoted through super-exchange interaction, the long-range ferromagnetic ordered state of the sintered material is enhanced, and the magnetic conductivity of the material is remarkably improved; the doping of the LiMn6Sn6 single crystal material promotes the growth of crystal grains in the sintered material through a grain boundary phase, so that the crystal structure is more compact, the overall density is improved, the microstructure of the material is optimized, and the eddy current loss is reduced; possible agglomerates are effectively scattered through secondary ball milling, the specific surface area of the powder is increased, sodium bismuthate and sodium molybdate with low melting points are added, the compactness of the sintered material is improved, and the overall performance of the material is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inductor sintered materials, and in particular relates to an inductor sintered material with high magnetic permeability. Background Art

[0002] In the context of the rapid development of modern electronic technology, inductors, as key passive electronic components, play a vital role in many electronic fields such as electronic communication equipment, power management, and radio frequency identification (RFID) systems. Inductors are mainly responsible for filtering, energy storage, signal transmission, and maintaining electromagnetic compatibility. As electronic equipment develops towards miniaturization, integration, and high performance, the performance requirements of inductors are also increasing.

[0003] In order to meet the demand for miniaturization of integrated circuits, large inductance devices must be implemented in a limited space, which makes the volume of the inductor a major factor restricting circuit integration and miniaturization. Therefore, the development of planar thin-film inductors that can operate at high frequencies and have high magnetic permeability has become a key technical path to promote the further development of electronic devices. However, existing inductor sintered materials generally have problems such as insufficient magnetic permeability, high porosity, and uneven grain growth, which seriously limit the improvement of inductor performance and the expansion of application scope. Summary of the invention

[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention aims to provide a high magnetic permeability inductor sintered material, which not only has high magnetic permeability, but also can effectively reduce the porosity, improve the density and overall performance of the material. The present invention proposes to introduce single crystal materials and improve the magnetic permeability of the sintered material through secondary ball milling and secondary sintering.

[0005] In order to achieve the above object, the following technical solution is adopted: The present invention provides a sintered inductor material with high magnetic permeability, and the sintered inductor material is prepared by the following steps:

[0006] S1. Preparation of LiMn6Sn6 single crystal material: lithium, manganese and tin are weighed in a corresponding molar ratio under an argon atmosphere, and then added into a quartz tube, and then a flux is added at 5% of the total mass of the metal single substances, and then the quartz tube is placed in a high-temperature furnace, and the temperature is gradually increased to form a uniform melt, and the flux is separated by a centrifuge, and then the cooling rate is controlled to cool to obtain a LiMn6Sn6 single crystal material;

[0007] S2, primary ball milling: after weighing iron oxide, zinc oxide, nickel oxide, copper oxide, aluminum oxide, cobalt oxide, silicon dioxide and LiMn6Sn6 single crystal material in proportion, the raw materials are fully mixed by a ball mill, and then dried;

[0008] S3, pre-sintering: pre-sintering the mixed powder after the first ball milling and drying in a nitrogen atmosphere;

[0009] S4, secondary ball milling: adding the pre-sintered material together with sodium bismuthate and sodium molybdate into a ball mill for secondary ball milling to promote uniform mixing of the materials;

[0010] S5, granulation: add PVA glue and mix with the secondary ball-milled material, then grind, and then pour into a mold for pressing;

[0011] S6. Secondary sintering: placing the pressed material into a sintering furnace and sintering it in a protective atmosphere. After sintering, the material is naturally cooled to obtain the inductor sintered material.

[0012] Furthermore, the inductor sintered material includes the following raw material components in percentage by mass: 55-65% iron oxide, 12-22% zinc oxide, 10-25% nickel oxide, 1-8% copper oxide, 1-5% aluminum oxide, 0.5-5% cobalt oxide, 0.5-3% silicon dioxide, 1-10% LiMn6Sn6 single crystal material, 1.5-3% sodium bismuthate and 1.5-3% sodium molybdate.

[0013] Furthermore, the molar ratio of lithium, manganese and tin is 0.85-1.15:6-8.5:7-9.

[0014] Furthermore, the flux is one of magnesium oxide, bismuth oxide and calcium oxide.

[0015] Furthermore, the heating rate in step S1 is 20-50°C / min, the highest temperature is 1100-1300°C, and the cooling rate is 40-80°C / min.

[0016] Furthermore, the ball milling time in step S2 is 3-6 hours, the ball milling speed is 200-500 r / min, and the temperature is room temperature.

[0017] Furthermore, the pre-sintering temperature of step S3 is 850-1000° C. and the time is 2-5 hours.

[0018] Furthermore, the secondary ball milling time of step S4 is 1-3h, the ball milling speed is 100-300r / min, and the temperature is 50-100°C.

[0019] Furthermore, the added amount of the PVA glue is 10%-20% of the total mass of the raw materials.

[0020] Furthermore, the sintering temperature of step S6 is 750-1000° C. and the sintering time is 3-6 hours.

[0021] The beneficial effects of the present invention are:

[0022] (1) The present invention improves the magnetic permeability of the sintered material by introducing LiMn6Sn6 single crystal material into the raw material of the sintered material. The two Sn2 honeycomb layers sandwiched between two Mn3 layers in the LiMn6Sn6 single crystal material promote the ferromagnetic coupling between the Mn3-Mn3 layers through superexchange interaction. At the same time, the magnetic coupling between the Sn2Li and Mn3 layers enhances the long-range ferromagnetic ordered state of the sintered material, thereby increasing the magnetic permeability of the sintered material.

[0023] (2) The doping of LiMn6Sn6 single crystal material not only improves the magnetic permeability, but also promotes the growth of grains in the sintered material through the generated grain boundary phase, making the crystal structure denser, reducing the porosity, and improving the overall density. This structural optimization reduces the resistance to magnetic domain movement and domain wall displacement, reduces the coercive force, further increases the magnetic permeability, and effectively reduces eddy current loss and energy loss;

[0024] (3) The present invention adopts a secondary ball milling process to effectively break up possible agglomerates, increase the specific surface area of ​​the powder, and thus improve the mixing uniformity of the material. In the secondary ball milling process, sodium bismuthate and sodium molybdate with lower melting points are added. These substances penetrate into the voids of the material during the secondary sintering process, which helps to increase the density of the sintered material and further improve the overall performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Magnetic permeability curves of various embodiments and comparative examples of a high magnetic permeability inductor sintered material of the present invention;

[0026] Figure 2 The magnetic loss test results of various embodiments and comparative examples of a high magnetic permeability inductor sintered material of the present invention are shown;

[0027] Figure 3 The density test results of various embodiments and comparative examples of a high magnetic permeability inductor sintered material of the present invention are shown;

[0028] Figure 4 The current value measurement results of the embodiments and comparative examples of the high magnetic permeability inductor sintered material of the present invention with the inductance reduced by 30% are shown.

[0029] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0031] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0032] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.

[0033] Example 1

[0034] A sintered inductor material with high magnetic permeability

[0035] The inductor sintered material is prepared by the following steps:

[0036] S1. Preparation of LiMn6Sn6 single crystal material: lithium, manganese and tin are weighed in a corresponding molar ratio under an argon atmosphere, and then added into a quartz tube, and then a flux is added at 5% of the total mass of the metal single substances, and then the quartz tube is placed in a high-temperature furnace, and the temperature is gradually increased to form a uniform melt, and the flux is separated by a centrifuge, and then the cooling rate is controlled to cool to obtain a LiMn6Sn6 single crystal material;

[0037] S2, primary ball milling: after weighing iron oxide, zinc oxide, nickel oxide, copper oxide, aluminum oxide, cobalt oxide, silicon dioxide and LiMn6Sn6 single crystal material in proportion, the raw materials are fully mixed by a ball mill, and then dried;

[0038] S3, pre-sintering: pre-sintering the mixed powder after the first ball milling and drying in a nitrogen atmosphere;

[0039] S4, secondary ball milling: adding the pre-sintered material together with sodium bismuthate and sodium molybdate into a ball mill for secondary ball milling to promote uniform mixing of the materials;

[0040] S5, granulation: add PVA glue and mix with the secondary ball-milled material, then grind, and then pour into a mold for pressing;

[0041] S6. Secondary sintering: placing the pressed material into a sintering furnace and sintering it in a protective atmosphere. After sintering, the material is naturally cooled to obtain the inductor sintered material.

[0042] The inductor sintered material includes the following raw material components in percentage by mass: 55% iron oxide, 20% zinc oxide, 10% nickel oxide, 4% copper oxide, 5% aluminum oxide, 1% cobalt oxide, 1% silicon dioxide, 1% LiMn6Sn6 single crystal material, 1.5% sodium bismuthate and 1.5% sodium molybdate.

[0043] The molar ratio of lithium, manganese and tin is 0.85:6:7.

[0044] The flux is magnesium oxide.

[0045] The heating rate in step S1 is 20°C / min, the highest temperature is 1100°C, and the cooling rate is 40°C / min.

[0046] The ball milling time in step S2 is 3 h, the ball milling speed is 200 r / min, and the temperature is room temperature.

[0047] The pre-sintering temperature of step S3 is 850° C. and the time is 2 hours.

[0048] The secondary ball milling time of step S4 is 1 hour, the ball milling speed is 100 r / min, and the temperature is 50° C.

[0049] The added amount of the PVA glue is 10% of the total mass of the raw materials.

[0050] The sintering temperature of step S6 is 750° C. and the sintering time is 3 hours.

[0051] Example 2

[0052] A sintered inductor material with high magnetic permeability

[0053] The preparation steps of the inductor sintered material are the same as those in Example 1.

[0054] The inductor sintered material includes the following raw material components in percentage by mass: 65% iron oxide, 15% zinc oxide, 12% nickel oxide, 1.5% copper oxide, 1.5% aluminum oxide, 0.5% cobalt oxide, 0.5% silicon dioxide, 1% LiMn6Sn6 single crystal material, 1.5% sodium bismuthate and 1.5% sodium molybdate.

[0055] The molar ratio of lithium, manganese and tin is 1.15:8.5:9.

[0056] The flux is bismuth oxide.

[0057] The heating rate in step S1 is 50°C / min, the highest temperature is 1300°C, and the cooling rate is 80°C / min.

[0058] The ball milling time in step S2 is 6 hours, the ball milling speed is 500 r / min, and the temperature is room temperature.

[0059] The pre-sintering temperature of step S3 is 1000° C. and the time is 5 hours.

[0060] The secondary ball milling time of step S4 is 3 hours, the ball milling speed is 300 r / min, and the temperature is 100° C.

[0061] The added amount of the PVA glue is 20% of the total mass of the raw materials.

[0062] The sintering temperature of step S6 is 1000° C. and the sintering time is 6 hours.

[0063] Example 3

[0064] A sintered inductor material with high magnetic permeability

[0065] The preparation steps of the inductor sintered material are the same as those in Example 1.

[0066] The inductor sintered material includes the following raw material components in percentage by mass: 60% iron oxide, 12% zinc oxide, 12% nickel oxide, 3% copper oxide, 3% aluminum oxide, 1% cobalt oxide, 1% silicon dioxide, 4% LiMn6Sn6 single crystal material, 2% sodium bismuthate and 2% sodium molybdate.

[0067] The molar ratio of lithium, manganese and tin is 1.05:7.5:8.

[0068] The flux is calcium oxide.

[0069] The heating rate in step S1 is 30°C / min, the highest temperature is 1200°C, and the cooling rate is 50°C / min.

[0070] The ball milling time in step S2 is 5 h, the ball milling speed is 300 r / min, and the temperature is room temperature.

[0071] The pre-sintering temperature of step S3 is 900° C. and the time is 3.5 hours.

[0072] The secondary ball milling time of step S4 is 2 hours, the ball milling speed is 200 r / min, and the temperature is 80°C.

[0073] The added amount of the PVA glue is 15% of the total mass of the raw materials.

[0074] The sintering temperature of step S6 is 850° C. and the sintering time is 4.5 hours.

[0075] Comparative Example 1

[0076] The difference between this comparative example and Example 3 is that the raw material components of the inductor sintered material do not contain LiMn6Sn6 single crystal material, but are replaced by the remaining components in the raw material components in equal amounts, and the remaining components, component contents, and preparation process are the same as those in Example 3.

[0077] Comparative Example 2

[0078] The difference between this comparative example and Example 3 is that sodium bismuthate and sodium molybdate are not added during the secondary ball milling, and the remaining components, component contents, and preparation process are the same as those in Example 3.

[0079] Results Analysis

[0080] Copper wire was selected, and the number of winding turns N=26Ts turns. The inductance and the inductance value under superimposed current of each embodiment and comparative example were measured using a YG107A magnetic ring turn tester. The test frequency was 0-100MHz. The magnetic permeability at different test frequencies was calculated using the magnetic permeability calculation formula. The magnetic permeability curve is shown in FIG. Figure 1 .

[0081] pass Figure 1 It can be seen that the magnetic permeability of the inductor sintered material introduced with LiMn6Sn6 single crystal material and the inductor sintered material added with sodium bismuthate and sodium molybdate in the secondary ball milling are improved.

[0082] The magnetic loss of each embodiment and comparative example was measured by the AC power method of TCPSS1009-2020, and the sample was wound with double windings. The test results are shown in Figure 2 .

[0083] The density of each embodiment and comparative example was measured by the measurement method in GB / T 3850-2015. The measurement results are shown in Figure 3 .

[0084] The current value of each embodiment and comparative example with a 30% reduction in inductance was measured using an E4980A LCR meter. The results are shown in Figure 4 .

[0085] pass Figure 2-4 In summary, the sintered materials of each embodiment have fewer voids and higher density, and each embodiment has lower magnetic loss under a high-frequency excitation source, and the current value of the inductance is higher when the inductance decreases by 30%. This proves that the addition of LiMn6Sn6 single crystal material, sodium bismuthate and sodium molybdate helps to improve the density of the inductor sintered material, thereby reducing the coercive force, reducing the magnetic loss and power consumption.

[0086] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0087] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A sintered inductor material with high magnetic permeability, characterized in that: The inductor sintered material is prepared by the following steps: S1. Preparation of LiMn6Sn6 single crystal material: lithium, manganese and tin are weighed in a corresponding molar ratio under an argon atmosphere, and then added into a quartz tube, and then a flux is added at 5% of the total mass of the metal single substances, and then the quartz tube is placed in a high-temperature furnace, and the temperature is gradually increased to form a uniform melt, and the flux is separated by a centrifuge, and then the cooling rate is controlled to cool to obtain a LiMn6Sn6 single crystal material; S2, primary ball milling: after weighing iron oxide, zinc oxide, nickel oxide, copper oxide, aluminum oxide, cobalt oxide, silicon dioxide and LiMn6Sn6 single crystal material in proportion, the raw materials are fully mixed by a ball mill, and then dried; S3, pre-sintering: pre-sintering the mixed powder after the first ball milling and drying in a nitrogen atmosphere; S4, secondary ball milling: adding the pre-sintered material together with sodium bismuthate and sodium molybdate into a ball mill for secondary ball milling to promote uniform mixing of the materials; S5, granulation: add PVA glue and mix with the secondary ball-milled material, then grind, and then pour into a mold for pressing; S6. Secondary sintering: placing the pressed material into a sintering furnace and sintering it in a protective atmosphere. After sintering, the material is naturally cooled to obtain the inductor sintered material.

2. The high magnetic permeability inductor sintered material according to claim 1, characterized in that: The invention comprises the following raw material components in percentage by weight: 55-65% iron oxide, 12-22% zinc oxide, 10-25% nickel oxide, 1-8% copper oxide, 1-5% aluminum oxide, 0.5-5% cobalt oxide, 0.5-3% silicon dioxide, 1-10% LiMn6Sn6 single crystal material, 1.5-3% sodium bismuthate and 1.5-3% sodium molybdate.

3. The high magnetic permeability inductor sintered material according to claim 2, characterized in that: The molar ratio of lithium, manganese and tin is 0.85-1.15:6-8.5:7-9.

4. The high magnetic permeability inductor sintered material according to claim 3, characterized in that: The flux is one of magnesium oxide, bismuth oxide and calcium oxide.

5. The high magnetic permeability inductor sintered material according to claim 4, characterized in that: The heating rate in step S1 is 20-50°C / min, the maximum temperature is 1100-1300°C, and the cooling rate is 40-80°C / min.

6. The high magnetic permeability inductor sintered material according to claim 5, characterized in that: The ball milling time of step S2 is 3-6 hours, the ball milling speed is 200-500 r / min, and the temperature is room temperature.

7. The high magnetic permeability inductor sintered material according to claim 6, characterized in that: The pre-sintering temperature of step S3 is 850-1000° C. and the time is 2-5 hours.

8. The high magnetic permeability inductor sintered material according to claim 7, characterized in that: The secondary ball milling time of step S4 is 1-3 hours, the ball milling speed is 100-300 r / min, and the temperature is 50-100° C.

9. The high magnetic permeability inductor sintered material according to claim 8, characterized in that: The added amount of the PVA glue is 10%-20% of the total mass of the raw materials.

10. The high magnetic permeability inductor sintered material according to claim 9, characterized in that: The sintering temperature of step S6 is 750-1000° C. and the sintering time is 3-6 hours.

Citation Information

Patent Citations

  • Preparation method of manganese zinc MnZn soft magnetic ferrite material containing modified nanocarbon

    CN102976741A

  • High-reliability ferrite material and preparation method thereof

    CN110156449A

  • Composite ferrite substrate material for LTCF transformer and preparation method of composite ferrite substrate material

    CN114605142A

  • Magnetic powder material, magnetic device and electronic equipment

    CN115691933A

  • Ferrite material, preparation method and magnetic core

    CN116178003A