Self-repairing polyurethane elastomer with bicontinuous phase structure and preparation method of self-repairing polyurethane elastomer
By using specific molar ratios of amino-terminated polydimethylsiloxane, isophorone diisocyanate and 5-(2-hydroxyethyl)-6-methyl-2-aminouracil in flexible electronic devices The bicontinuous phase structure polyurethane elastomer solves the problems of performance degradation and insufficient thermodynamic stability in the existing technology, and achieves efficient self-healing and improved fatigue resistance.
Patent Information
- Application Number
- CN202310360373.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-04-06
AI Technical Summary
The performance of existing self-healing polyurethane elastomers in flexible electronic devices deteriorates during repeated use, and they lack thermodynamic stability and cannot effectively repair cracks during high-frequency bending and extension movements, leading to early material failure.
Amino-terminated polydimethylsiloxane, isophorone diisocyanate and 5-(2-hydroxyethyl)-6-methyl-2-amino are used in a molar ratio of 1:1.1~1.5:0.1~0.5 Uracil, synthesized in the next step catalyzed by dibutyltin dilaurate, forms a self-healing polyurethane elastomer with a bicontinuous phase structure.
The material's resilience, fatigue resistance and thermal stability are improved. It can return to its original length within 5 minutes under 500% strain and within 2 minutes after being stretched to 50% strain at 50°C. The fatigue threshold is significant. promote.
Smart Images

Figure CN118772369A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials and relates to a self-repairing polyurethane elastomer with a dual-continuous phase structure and a preparation method thereof. Background Art
[0002] From ancient times to the present, human beings have never stopped exploring and learning about natural organisms, and therefore invented many bionic materials, which have played a vital role in the progress of human society. For a huge biological system, the most attractive thing is its self-healing ability. In 2001, White published a report on self-healing epoxy resin in Nature magazine [Nature, 2001, 409, 794-797], which has set off a research boom in self-healing polymer materials. With the in-depth study of component dynamic chemistry (supramolecular chemistry and dynamic covalent bonds), in order to meet practical application scenarios, more and more self-healing materials with different moduli (different hardness) have been studied by scientific researchers.
[0003] Flexible (low modulus) polymer materials have been widely used in flexible electronic devices because of their excellent stretchability and bendability. However, flexible electronic devices are very prone to damage in daily use environments, so it is very necessary to develop flexible electronic devices with self-repairing functions. Based on the above report, Professor Bao Zhennan of Stanford University developed a self-repairing polyurethane elastomer through hierarchical hydrogen bonding [Adv. Mater., 2018, 30, 1706846]. The elastomer is synthesized from amino-terminated polydimethylsiloxane, 4,4′-methylenebis(phenyl isocyanate), and isophorone diisocyanate. It can be repaired at room temperature for 48 hours to restore 78% of the mechanical properties. In addition, the material also has high damage resistance and crack propagation ability, but the above performance will gradually decrease during repeated use. In addition, the elastomer does not have excellent thermodynamic stability. It is not enough to evaluate the crack propagation resistance only in a single stretch. As we all know, in actual use, flexible electronic devices often have to bend and stretch thousands of times. Cracks can easily expand or even penetrate the entire material during extremely high-frequency reciprocating motion, which makes the material completely ineffective before it can be repaired. Therefore, for flexible electronic devices, it is imperative to develop room temperature fatigue-resistant flexible self-healing materials with thermal stability. Summary of the invention
[0004] The object of the present invention is to provide a self-repairing polyurethane elastomer with a dual-continuous phase structure and a preparation method thereof.
[0005] The technical solution for achieving the purpose of the present invention is as follows:
[0006] The self-healing polyurethane elastomer with a dual continuous phase structure is synthesized in one step from amino-terminated polydimethylsiloxane (NH2-PDMS-NH2), isophorone diisocyanate (IPDI) and 5-(2-hydroxyethyl)-6-methyl-2-aminouracil in a molar ratio of 1:1.1-1.5:0.1-0.5 with dibutyltin dilaurate as a catalyst. The structural formula of the self-healing polyurethane elastomer is as follows:
[0007] n≥22.
[0008] The preparation method of a self-repairing polyurethane elastomer with a dual-continuous phase structure comprises the following specific steps:
[0009] According to the molar ratio of amino-terminated polydimethylsiloxane, isophorone diisocyanate and 5-(2-hydroxyethyl)-6-methyl-2-aminouracil of 1:1.1-1.5:0.1-0.5, 5-(2-hydroxyethyl)-6-methyl-2-aminouracil powder, amino-terminated polydimethylsiloxane, isophorone diisocyanate and dibutyltin dilaurate were dissolved in N,N-dimethylformamide, and refluxed at 70±10°C in a nitrogen atmosphere with stirring. After the reaction, the mixture was cooled to room temperature to obtain a self-healing polyurethane elastomer material.
[0010] Preferably, 5-(2-hydroxyethyl)-6-methyl-2-aminouracil is prepared by the following steps: 2-acetylbutyrolactone, triethylamine and guanidine carbonate are refluxed in ethanol for 4 to 6 hours. After the reaction, a yellow powder solid is obtained by suction filtration, which is further washed with ethanol and dried at 60° C. for 12 to 24 hours to obtain a white 5-(2-hydroxyethyl)-6-methyl-2-aminouracil powder.
[0011] Preferably, the number average molecular weight of the amino-terminated polydimethylsiloxane is 3,000.
[0012] Preferably, the molar ratio of amino-terminated polydimethylsiloxane, isophorone diisocyanate, and 5-(2-hydroxyethyl)-6-methyl-2-aminouracil is 1:1.3:0.3.
[0013] Preferably, the reflux reaction time is 12 to 18 hours.
[0014] Preferably, in the reaction system, the concentration of amino-terminated polydimethylsiloxane is 30 wt %.
[0015] Preferably, the mass of dibutyltin dilaurate is 1% of the mass of isophorone diisocyanate.
[0016] Compared with the prior art, the present invention has the following advantages:
[0017] The present invention uses 5-(2-hydroxyethyl)-6-methyl-2-aminouracil as a chain extender to adjust the phase structure of the self-repairing polyurethane elastomer, so that it has a phase structure in the shape of a bicontinuous network. The phase of the bicontinuous network structure effectively improves the resilience of the self-repairing polyurethane elastomer (it can recover to its original length within 5 minutes after being stretched to 500% strain), fatigue resistance (fatigue threshold of 1010J m -2 ) and thermal stability (stretched to 50% strain at 50°C and still able to recover to its original length within 2 minutes). BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is an atomic force microscope phase image of SHPU-SNS-0.3 in Example 2;
[0019] Figure 2 The infrared images of SHPU-SNS-0.1, SHPU-SNS-0.3, SHPU-SNS-0.5 and SHPU-WNS in Examples 1, 2, 3 and Comparative Example 1 are shown;
[0020] Figure 3 The mechanical repair curves of SHPU-SNS-0.3 and SHPU-WNS in Example 2 and Comparative Example 1;
[0021] Figure 4 The actual display diagram of the samples obtained in Example 2 and Comparative Example 1 after being broken;
[0022] Figure 5 The tensile stress-strain curves of SHPU-SNS-0.1, SHPU-SNS-0.3, SHPU-SNS-0.5 and SHPU-WNS in Examples 1, 2, 3 and Comparative Example 1 are shown;
[0023] Figure 6 Fatigue threshold diagrams of SHPU-SNS-0.3 and SHPU-WNS in Example 2 and Comparative Example 1;
[0024] Figure 7 It is a comparison diagram of the elasticity of SHPU-SNS-0.3 and SHPU-WNS in Example 2 and Comparative Example 1;
[0025] Figure 8 It is the strain recovery curve of SHPU-SNS-0.3 and SHPU-WNS at 50°C in Example 2 and Comparative Example 1. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below in conjunction with the embodiments and drawings.
[0027] 5-(2-Hydroxyethyl)-6-methyl-2-aminouracil was prepared according to the reference [J.Am.Chem.Soc., 2018, 140, 5280], and the specific steps are as follows:
[0028] Weigh 2-acetylbutyrolactone (5.12 g), triethylamine (11 ml) and guanidine carbonate (3.60 g), stir in 40 ml ethanol at 60°C, and reflux for 4 hours. After the reaction, a yellow powder solid is obtained by suction filtration, which is further washed with ethanol, and the product is placed in an oven at 60°C for 12 hours to obtain a white 5-(2-hydroxyethyl)-6-methyl-2-aminouracil powder.
[0029] Example 1
[0030] White 5-(2-hydroxyethyl)-6-methyl-2-aminouracil powder (0.0169 g) was placed in a three-necked flask containing 10 ml of N,N-dimethylformamide solvent, and refluxed at 70°C for 12 hours. After the solution was cooled to room temperature, the obtained solid was dissolved in chloroform solution and then poured into a polytetrafluoroethylene mold to evaporate the solvent at room temperature for 12 hours to obtain a self-healing polyurethane elastomer SHPU-SNS-0.1 with a dual-continuous phase structure.
[0031] Example 2
[0032] White 5-(2-hydroxyethyl)-6-methyl-2-aminouracil powder (0.0507 g) was placed in a three-necked flask containing 10 ml of N,N-dimethylformamide solvent, and refluxed at 70°C for 12 hours. After the solution was cooled to room temperature, the obtained solid was dissolved in chloroform solution and then poured into a polytetrafluoroethylene mold to evaporate the solvent at room temperature for 12 hours to obtain a self-healing polyurethane elastomer SHPU-SNS-0.3 with a dual-continuous phase structure.
[0033] Example 3
[0034] White 5-(2-hydroxyethyl)-6-methyl-2-aminouracil powder (0.0845 g) was placed in a three-necked flask containing 10 ml of N,N-dimethylformamide solvent, and refluxed at 70°C for 12 hours. After the solution was cooled to room temperature, the obtained solid was dissolved in chloroform solution and then poured into a polytetrafluoroethylene mold to evaporate the solvent at room temperature for 12 hours to obtain a self-healing polyurethane elastomer SHPU-SNS-0.5 with a dual-continuous phase structure.
[0035] Comparative Example 1
[0036] Amino-terminated polydimethylsiloxane (3 g) and isophorone diisocyanate (0.222 g) were placed in a three-necked flask filled with 10 ml of N,N-dimethylformamide solvent, and refluxed at 70°C for 12 hours. After the solution was cooled to room temperature, the obtained solid was dissolved in chloroform solution and then poured into a polytetrafluoroethylene mold to evaporate the solvent at room temperature for 12 hours to obtain a self-healing polyurethane elastomer SHPU-WNS without a dual-continuous phase structure.
[0037] Figure 1 This is an atomic force microscope phase image of SHPU-SNS-0.3 in Example 2. It can be seen from the image that the material has a phase with a double continuous network structure.
[0038] Figure 2 These are the infrared images of SHPU-SNS-0.1, SHPU-SNS-0.3, SHPU-SNS-0.5 and SHPU-WNS in Examples 1, 2, 3 and Comparative Example 1, wherein Peak 1 is the carbonyl peak in carbamate, SHPU-WNS does not have Peak 1, while SHPU-SNS-0.1, SHPU-SNS-0.3 and SHPU-SNS-0.5 have Peak 1.
[0039] Figure 3 The mechanical repair curves of SHPU-SNS-0.3 of Example 2 and SHPU-WNS of Comparative Example 1 are shown.
[0040] Figure 4 This is a physical display picture of SHPU-SNS-0.3 of Example 2 and SHPU-WNS of Comparative Example 1 after being broken.
[0041] Figure 5The tensile stress-strain curves of SHPU-SNS-0.1, SHPU-SNS-0.3, SHPU-SNS-0.5 and SHPU-WNS in Examples 1, 2, 3 and Comparative Example 1 are shown. The stress and strain of SHPU-SNS-0.1 are 0.95 MPa and 1135%, respectively, and the stress and strain of SHPU-SNS-0.5 are 3.4 MPa and 1650%, respectively. Compared with SHPU-WNS (stress of 0.6 MPa and strain of 970%), the stress and strain of SHPU-SNS-0.3 are increased by 4.1 and 1.7 times, reaching 2.60 MPa and 1680%, respectively.
[0042] Figure 6 The fatigue threshold values of SHPU-SNS-0.3 of Example 2 and SHPU-WNS of Comparative Example 1 are shown in FIG. The fatigue threshold values of SHPU-SNS-0.3 and SHPU-WNS are 1010 J m -2 With 29J m -2 , the fatigue threshold of SHPU-SNS-0.3 is 34.8 times higher than that of SHPU-WNS.
[0043] Figure 7 This is a comparison diagram of the elasticity of SHPU-SNS-0.3 of Example 2 and SHPU-WNS of Comparative Example 1. Under a tensile strain of 500%, SHPU-SNS-0.3 can return to its original length within 5 minutes, while SHPU-WNS cannot.
[0044] Figure 8 The strain recovery curves of SHPU-SNS-0.3 of Example 2 and SHPU-WNS of Comparative Example 1 at 50°C are as follows. SHPU-SNS-0.3 is stretched to 50% at 50°C and can return to its original length within 2 minutes, but SHPU-WNS cannot return to its original length after being stretched to 50% at 50°C.
Claims
1. Self-healing polyurethane elastomer with dual continuous phase structure, It is characterized in that Its structural formula is as follows:
2. The method for preparing the self-repairing polyurethane elastomer having a dual-continuous phase structure according to claim 1, It is characterized in that The specific steps are as follows: According to the molar ratio of amino-terminated polydimethylsiloxane, isophorone diisocyanate and 5-(2-hydroxyethyl)-6-methyl-2-aminouracil of 1:1.1-1.5:0.1-0.5, 5-(2-hydroxyethyl)-6-methyl-2-aminouracil powder, amino-terminated polydimethylsiloxane, isophorone diisocyanate and dibutyltin dilaurate were dissolved in N,N-dimethylformamide, and refluxed at 70±10°C under nitrogen atmosphere with stirring. After the reaction, the mixture was cooled to room temperature to obtain a self-healing polyurethane elastomer material.
3. The preparation method according to claim 1, It is characterized in that 5-(2-Hydroxyethyl)-6-methyl-2-aminouracil is prepared by the following steps: 2-acetylbutyrolactone, triethylamine and guanidine carbonate are refluxed in ethanol for 4 to 6 hours. After the reaction, a yellow powder solid is obtained by suction filtration, which is further washed with ethanol and dried at 60°C for 12 to 24 hours to obtain a white 5-(2-hydroxyethyl)-6-methyl-2-aminouracil powder.
4. The preparation method according to claim 1, It is characterized in that The number average molecular weight of amino-terminated polydimethylsiloxane was 3,000.
5. The preparation method according to claim 1, It is characterized in that The molar ratio of amino-terminated polydimethylsiloxane, isophorone diisocyanate, and 5-(2-hydroxyethyl)-6-methyl-2-aminouracil is 1:1.3:0.
3.
6. The preparation method according to claim 1, It is characterized in that The reflux reaction time is 12 to 18 hours.
7. The preparation method according to claim 1, It is characterized in that In the reaction system, the concentration of amino-terminated polydimethylsiloxane was 30 wt %.
8. The preparation method according to claim 1, It is characterized in that The mass of dibutyltin dilaurate is 1% of the mass of isophorone diisocyanate.
Citation Information
Patent Citations
Supramolecular polyurethane impact-resistant material containing multiple hydrogen bonds and preparation method of supramolecular polyurethane impact-resistant material
CN111848907A
Supramolecular hot melt adhesive and preparation method thereof
CN114806485A
High-performance self-repairing polyurethane elastomer and preparation method thereof
CN115109225A
Self-repair oligomers and uses thereof
CN115362189A
Double dynamic polymers
US20220153907A1