Polyisoprene polyurethane and preparation method thereof
By using liquid double-ended hydroxyl isoprene as the soft segment, the glass transition temperature of polyisoprene-based polyurethane is lowered, which solves the problem of high glass transition temperature of existing polyolefin-based polyurethane and enables wider applications. and excellent performance.
Patent Information
- Application Number
- CN202410958578.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The glass transition temperature of existing polyolefin-based polyurethanes is usually high, which limits their application range.
Liquid double-terminated hydroxyl isoprene is used as the soft segment, and polyisoprene-based polyurethane is generated by polymerizing with isocyanate to reduce the glass transition temperature of the material. By regulating the molecular weight of the soft segment, the content of the hard segment and the chain extender and The proportion of cross-linking agent controls the microscopic morphology and macroscopic properties of the material.
The low glass transition temperature of polyurethane material is achieved, its low temperature resistance and dynamic mechanical properties are enhanced, the loss factor and energy dissipation are reduced, and the scope of application is expanded.
Smart Images

Figure CN118772371A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to polyurethane, and more particularly to a polyisoprene-based polyurethane and a preparation method thereof. Background Art
[0002] Polyurethane, an important class of polymer materials, is widely used in various fields due to its excellent mechanical properties, wear resistance, and high damping performance. Polyurethanes can be divided into two categories: polyether and polyester, depending on whether the polymer backbone contains ether or ester bonds. Polyurethane elastomers typically use flexible polyether or polyester polyols as soft segments and rigid diisocyanates as hard segments. The ratio of soft and hard segments and their chemical structure significantly influence the microstructure and macroscopic properties of polyurethane.
[0003] With the rapid development of the polyurethane industry, the demand for high-performance, multifunctional polyurethane products is growing. Modulating the chemical structure of polyurethane's soft and hard segments is a research hotspot in the field. Many researchers use silicone rubber or polyolefin rubber as the soft segment in the synthesis of polyurethane to achieve high performance and functionalization of polyurethane.
[0004] Many researchers have used dihydroxyl-functionalized polyolefins as soft segments in the synthesis of polyurethanes, resulting in high-performance polyurethane materials such as hydroxyl-terminated butadiene, butadiene-acrylonitrile copolymers, butadiene-styrene copolymers, and isoprene-based olefin polymers. However, existing polyurethanes synthesized using dihydroxyl-functionalized polyolefins as soft segments typically exhibit high glass transition temperatures. Summary of the Invention
[0005] In order to solve the problem that the glass transition temperature of existing polyolefin-based polyurethanes is generally high, the present invention provides a polyisoprene-based polyurethane with a lower glass transition temperature.
[0006] The present invention introduces liquid dihydroxylated isoprene as a soft segment into a polyurethane system. Liquid dihydroxylated isoprene has a high degree of unsaturation. Its use as a soft segment can improve the flexibility and low-temperature performance of polyurethane materials, resulting in a lower glass transition temperature (Tg). This lower Tg leads to a wider range of applications. Furthermore, the unsaturated double bonds in the liquid dihydroxylated isoprene molecular chain can provide chemical modification sites, thereby enabling the regulation of polyurethane material properties.
[0007] One of the objects of the present invention is to provide a polyisoprene-based polyurethane.
[0008] The polyisoprene polyurethane comprises repeating structural units represented by formula A, formula B, and formula C;
[0009]
[0010] In formula A, R0 is -CH2, -CH2CH2 or -CH(CH3), preferably -CH2;
[0011] X=15~50, Y=1~3, Z=1~4; Preferably, X=18~19, Y=1~2, Z=1~2, X=21~22, Y=1~2, Z=1~2,
[0012] X is 88-92% of the sum of X, Y, and Z, for example, 88-89%, 89-90%, preferably 88-90%;
[0013] Formula B is a structural unit derived from isocyanate, and R1 is preferably selected from
[0014] Formula C is a structural unit derived from a small molecule diol, and R2 is preferably selected from -CH2CH2CH2CH2-.
[0015] The molar ratio of the repeating structural units represented by Formula A, Formula B, and Formula C is 0.25-0.52:1:0.37-0.6, preferably 0.39-0.45:1:0.43-0.48.
[0016] The polyisoprene-based polyurethane further comprises a repeating structural unit represented by formula D;
[0017]
[0018] Formula D is a structural unit derived from a small molecule triol, and R3 is preferably selected from -CH2CR3(CH3)-CH2-.
[0019] The molar ratio of the repeating structural unit represented by formula D to the repeating structural unit represented by formula B is 0.042-0.068:1, preferably 0.047-0.054:1.
[0020] In the polyisoprene-based polyurethane, the repeating structural unit represented by formula A is derived from dihydroxy-terminated polyisoprene.
[0021] A second object of the present invention is to provide a method for preparing the polyisoprene-based polyurethane described in one of the objects of the invention.
[0022] The preparation method of the polyisoprene-based polyurethane comprises: dissolving the dihydroxy-terminated polyisoprene after dehydration in solvent A, adding isocyanate dissolved in solvent A, and pre-reacting for 2-5 hours; adding a chain extender-catalyst solution dropwise, and reacting for 1-3 hours; and curing the reaction solution to obtain the polyisoprene-based polyurethane;
[0023] The pre-reaction and reaction were carried out under nitrogen atmosphere at 75-85°C;
[0024] The chain extender-catalyst solution comprises a chain extender, a catalyst and a solvent A;
[0025] When the polyisoprene-based polyurethane comprises the repeating structural unit represented by Formula D, the chain extender-catalyst solution further comprises a cross-linking agent.
[0026] The dehydration operation of the dihydroxy-terminated polyisoprene is conventional, for example, heating the dihydroxy-terminated polyisoprene to 110° C. and vacuuming for 2 hours to remove water.
[0027] The reaction mechanism is as follows: Bis-hydroxyl-terminated polyisoprene polymerizes with isocyanate to form a polyurethane prepolymer. Upon addition of a chain extender, the two ends of the chain extender connect to the polyurethane prepolymer and / or the isocyanate, while the prepolymer and / or the isocyanate continue to polymerize, ultimately forming a linear polyurethane linked by the chain extender. In the presence of a crosslinker, the three hydroxyl ends of the crosslinker connect to one or more of the polyurethane prepolymer, isocyanate, and the linear polyurethane, while the prepolymer and / or the isocyanate continue to polymerize, ultimately forming a crosslinked polyurethane linked by the crosslinker.
[0028] The isocyanate is selected from at least one of 4,4-diphenylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, and dicyclohexylmethane diisocyanate.
[0029] The chain extender is selected from small molecule diols, preferably 1,4-butanediol.
[0030] The cross-linking agent is selected from small molecule triols, preferably trimethylolpropane or glycerol.
[0031] The solvent A is selected from at least one of tetrahydrofuran, dioxane, dichloromethane, and dimethylformamide (DMF).
[0032] The catalyst is selected from organotin or tertiary amine catalysts; preferably dibutyltin dilaurate (T-12) of the organotin type.
[0033] A method for preparing polyisoprene-based polyurethane includes heating dihydroxy-terminated polyisoprene to 105-115°C, vacuuming for 2-3 hours to remove water, then lowering the temperature to 75-85°C, adding tetrahydrofuran to dissolve the dihydroxy-terminated polyisoprene, and then adding 4,4-diphenylmethane diisocyanate dissolved in tetrahydrofuran to react for 2-5 hours to prepare a prepolymer. The reaction is carried out under a nitrogen atmosphere. A chain extender, 1,4-butanediol, and a catalyst, dibutyltin dilaurate, dissolved in tetrahydrofuran, are then dropwise added to the reaction solution. If a cross-linked polyurethane is to be prepared, a crosslinker, trimethylolpropane, is also added. After continuing the reaction for 1-3 hours, the reaction solution is poured into a tetrafluoroethylene mold, allowed to stand at room temperature for 10-14 hours, and then cured in a vacuum oven at 75-85°C. The reaction process is schematically shown below:
[0034]
[0035] in represent
[0036] The structural formula of the dihydroxy-terminated polyisoprene is shown in formula (I);
[0037]
[0038] In formula (I),
[0039] R is -CH2OH, -CH2CH2OH, -CH(CH3)OH, preferably -CH2OH;
[0040] X=15~50, Y=1~3, Z=1~4; Preferably, X=18~19, Y=1~2, Z=1~2, X=21~22, Y=1~2, Z=1~2,
[0041] X is 88-92% of the total of X, Y, and Z, preferably 88-90%.
[0042] In formula (I), X is 88-92% of the total of X, Y, and Z; that is, in the homopolyisoprene unsaturated segment containing three types of polyisoprenes, the molar ratio of 1,4-polyisoprene is 88-92%.
[0043] Preferably, the structural formula of the double-terminated hydroxyl polyisoprene is:
[0044] in,
[0045] X=15~50, Y=1~3, Z=1~4; for example, X=18~19, Y=1~2, Z=1~2, X=21~22, Y=1~2, Z=1~2, X=33~34, Y=1~2, Z=2~3 or
[0046] X is 88-90% of the sum of X, Y, and Z, for example, 88-89%, 89-90%;
[0047] X, Y, and Z in the structural formula of the dihydroxy-terminated polyisoprene are the same as X, Y, and Z in the repeating structural unit shown in Formula A.
[0048] The number average molecular weight of the bihydroxyl-terminated polyisoprene liquid rubber is 1,000 to 50,000; the molecular weight distribution of the bihydroxyl-terminated polyisoprene liquid rubber is less than 1.7, preferably less than 1.4.
[0049] The preparation method of the dihydroxy-terminated polyisoprene comprises:
[0050] Isoprene, a chain transfer agent, an initiator, and a solvent B are mixed and reacted under heating and pressure to obtain the dihydroxy-terminated polyisoprene liquid rubber; the reaction temperature is 65 to 130° C.; the reaction pressure is 0.5 to 1 MPa; and the reaction time is 2 to 24 hours;
[0051] The molar ratio of the isoprene, the chain transfer agent, the initiator, and the solvent is 100-2000:1:0.2-0.5:100-500; preferably 500-1000:1:0.3-0.5:200-400.
[0052] The structure of the chain transfer agent is shown in formula (II),
[0053]
[0054] In formula (II), R is -CH2OH, -CH2CH2OH, -CH(CH3)OH; or / and,
[0055] The initiator includes an azo initiator and / or an organic peroxide initiator, preferably at least one selected from azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, acetophenone peroxide, and di-tert-butyl peroxide; or / and,
[0056] The solvent B is selected from at least one of dioxane, tetrahydrofuran, n-hexane, and cyclohexane
[0057] In the present invention, the double-terminal hydroxyl polyisoprene adopts the double-terminal hydroxyl polyisoprene liquid rubber in patent application 2023112670982.
[0058] The structure of double-terminated hydroxyl polyisoprene liquid rubber is shown in formula (I)
[0059]
[0060] In formula (I), R is -CH2OH, -CH2CH2OH or -CH(CH3)OH; X=1-700, Y=1-100, and Z=1-100.
[0061] The structural formula of the dihydroxylated polyisoprene liquid rubber indicates that the molecular chain of the dihydroxylated polyisoprene liquid rubber consists of a p-xylylene group in the middle, flanked by homoisoprene unsaturated segments, and terminated by trithioester groups on the outer sides of the trithioester groups (i.e., both ends of the molecular chain) with hydroxyl groups. The homoisoprene unsaturated segments consist of three types of polyisoprenes: 3,4-polyisoprene, 1,2-polyisoprene, and 1,4-polyisoprene, in that order, from the middle to the outer ends of the chain.
[0062] The number average molecular weight of the bihydroxyl-terminated polyisoprene liquid rubber is 1,000 to 50,000; and the molecular weight distribution of the bihydroxyl-terminated polyisoprene liquid rubber is less than 1.7.
[0063] The preparation method of the dihydroxy-terminated polyisoprene liquid rubber comprises:
[0064] Isoprene, a chain transfer agent, an initiator, and a solvent are mixed and reacted under heating and pressure to produce the dihydroxy-terminated polyisoprene liquid rubber; wherein the chain transfer agent is a dihydroxy-terminated trithioester chain transfer agent. Specifically, the following technical solutions can be adopted:
[0065] A dihydroxy-terminated polyisoprene liquid rubber is obtained by reversible addition-fragmentation chain transfer polymerization of isoprene using a dihydroxy-terminated trithioester compound as a chain transfer agent. In the preparation method of the dihydroxy-terminated polyisoprene liquid rubber of the present invention, the polymerization process is carried out in a stainless steel high-temperature and high-pressure reactor equipped with a magnetic stirrer. Isoprene, a chain transfer agent, an initiator, and a solvent are added to the reactor. After cryogenic pumping, the reactor is pressurized and sealed under nitrogen and reacted with stirring. After the polymerization reaction is completed, the reaction solution is dripped into a methanol solvent, and the mixture is centrifuged to obtain a solid product, which is then dried in a high-temperature vacuum oven to obtain the dihydroxy-terminated polyisoprene liquid rubber.
[0066] The structure of the dihydroxyl-terminated trithioester chain transfer agent is shown in formula (II):
[0067]
[0068] In formula (II), R is -CH2OH, -CH2CH2OH or -CH(CH3)OH. That is, the dihydroxyl-terminated trisulfide chain transfer agent is
[0069]
[0070] Any one of .
[0071] When the dihydroxyl-terminated trisulfide chain transfer agent is When the prepared double-terminal hydroxyl polyisoprene liquid rubber is
[0072]
[0073] When the dihydroxyl-terminated trisulfide chain transfer agent is When the prepared double-terminal hydroxyl polyisoprene liquid rubber is
[0074]
[0075] When the dihydroxyl-terminated trisulfide chain transfer agent is When the prepared double-terminal hydroxyl polyisoprene liquid rubber is
[0076]
[0077] Technicians can select appropriate dihydroxyl-terminated trithioester chain transfer agents according to actual needs.
[0078] The initiator includes an azo initiator and / or an organic peroxide initiator. Preferably, the azo initiator includes azobisisobutyronitrile and / or azobisisoheptanenitrile; the organic peroxide initiator includes at least one of benzoyl peroxide, acetophenone peroxide, and di-tert-butyl peroxide. A skilled person can select an appropriate initiator based on actual needs. In another preferred embodiment of the present invention, the solvent includes at least one of dioxane, tetrahydrofuran, n-hexane, and cyclohexane. A skilled person can select an appropriate solvent based on actual needs.
[0079] The molar ratio of the isoprene, the chain transfer agent, the initiator, and the solvent is 100-2000:1:0.2-0.5:100-500, preferably 500-1000:1:0.3-0.5:200-400. A technician can select an appropriate molar ratio according to actual needs.
[0080] The reaction time is 2 to 24 hours; the reaction temperature is 65 to 130°C; and the reaction pressure is 0.5 to 1 MPa. Technicians can select appropriate reaction time, reaction temperature, and reaction pressure based on actual needs.
[0081] In the above method for preparing dihydroxy-terminated polyisoprene liquid rubber, dihydroxy-terminated polyisoprene liquid rubbers with different molecular weights can be obtained by changing the reaction time or the feed ratio of isoprene, initiator, and chain transfer agent.
[0082] Compared with the prior art, the present invention has the following beneficial effects:
[0083] The invention uses double-terminal hydroxyl polyisoprene as a soft segment and adopts a two-step method to successfully synthesize polyisoprene-based polyurethane.
[0084] The present invention introduces liquid dihydroxylated isoprene as a soft segment into a polyurethane system. Liquid dihydroxylated isoprene has a high degree of unsaturation. Its use as a soft segment can improve the flexibility and low-temperature performance of polyurethane materials, resulting in a lower glass transition temperature (Tg). This lower Tg leads to a wider range of applications. Furthermore, the unsaturated double bonds in the liquid dihydroxylated isoprene molecular chain can provide chemical modification sites, thereby enabling the regulation of polyurethane material properties.
[0085] The present invention can regulate the micromorphology and macroscopic properties of the double-terminal hydroxyisoprene polyurethane by adjusting the soft segment molecular weight, the hard segment content, and the ratio of the chain extender to the crosslinker, providing important experimental basis and theoretical guidance for the design of high-performance polyisoprene polyurethane elastomers.
[0086] The polyisoprene-based polyurethane provided by the present invention has a low glass transition temperature, excellent low-temperature resistance, and can maintain good stability in low-temperature environments. It also has excellent dynamic mechanical properties, with a low loss factor and energy dissipation, which can effectively reduce wear. BRIEF DESCRIPTION OF THE DRAWINGS
[0087] Figure 1 DSC curves of linear polyisoprene-based polyurethane elastomers with different soft segment molecular weights prepared in Examples 1-3;
[0088] Figure 2 The stress-strain curves of linear polyisoprene-based polyurethane elastomers with different soft segment molecular weights prepared in Examples 1-3;
[0089] Figure 3 DMA curves of linear polyisoprene-based polyurethane elastomers with different soft segment molecular weights prepared in Examples 1-3;
[0090] Figure 4 DSC curves of cross-linked polyisoprene-based polyurethane elastomers with different hard segment contents prepared in Examples 4-6;
[0091] Figure 5These are stress-strain curves of cross-linked polyisoprene-based polyurethane elastomers with different hard segment contents prepared in Examples 4-6;
[0092] Figure 6 DMA curves of linear polyisoprene-based polyurethane elastomers with different soft segment molecular weights prepared in Examples 4-6;
[0093] Figure 7 DSC curves of cross-linked polyisoprene-based polyurethane elastomers prepared in Examples 4, 7, and 8 with different ratios of chain extender to cross-linker;
[0094] Figure 8 The stress-strain curves of the cross-linked polyisoprene-based polyurethane elastomers prepared in Examples 4, 7, and 8 with different ratios of chain extender to cross-linker;
[0095] Figure 9 DMA curves of linear polyisoprene-based polyurethane elastomers with different soft segment molecular weights prepared in Examples 4, 7, and 8;
[0096] Figure 10 The double-terminal hydroxyl polyisoprene (HTPI) prepared in Example 1 1 H NMR spectrum;
[0097] Figure 1 、 4 In Figure 7, the horizontal axis is temperature (°C) and the vertical axis is heat flow rate dH / dt (mW);
[0098] Figure 2 、 5 In Figure 8, the horizontal axis is strain (%) and the vertical axis is stress (MPa);
[0099] Figure 3 、 6 In Figure 9, the horizontal axis is temperature (℃), the vertical axis on the left is the storage modulus E', and the vertical axis on the right is the loss factor tanδ;
[0100] Wherein, HTPI-1800-LPU represents the linear polyisoprene-based polyurethane elastomer with a soft segment molecular weight of 1800 prepared in Example 1; HTPI-3000-LPU represents the linear polyisoprene-based polyurethane elastomer with a soft segment molecular weight of 3000 prepared in Example 2; HTPI-3900-LPU represents the linear polyisoprene-based polyurethane elastomer with a soft segment molecular weight of 3900 prepared in Example 3;
[0101] HS represents hard segment, SS represents soft segment, CPU represents cross-linked polyisoprene-based polyurethane elastomer, B represents chain extender, and T represents cross-linking agent; the subscripts of HS, SS, B, and T represent relative molar numbers. DETAILED DESCRIPTION
[0102] The present invention will be described in detail below with reference to specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art to the present invention based on the contents of the present invention still fall within the scope of protection of the present invention.
[0103] In the following examples, all reagents used are commercially available products.
[0104] Among them, di-tert-butyl peroxide (DTBP) comes from J&K.
[0105] Example 1
[0106] (1) Potassium phosphate trihydrate (0.1 mol), 2-mercaptoethanol (0.1 mol), and acetone were added to a 1000 mL round-bottom flask. After stirring for 10 min, carbon disulfide (0.3 mol) was added. The solution turned bright yellow. 1,4-Bis(bromomethyl)benzene (0.05 mol) dissolved in acetone was then added to the round-bottom flask and allowed to react for 2 h. After the reaction was complete, the mixture was filtered, and the filtrate was concentrated under reduced pressure and recrystallized to obtain 1,4-phenylenebis(methylene)bis(2-hydroxyethyl)bis(trithiocarbamate) (PMHD).
[0107] (2) Take 1,4-phenylenebis(methylene)bis(2-hydroxyethyl)bis(trithiocarbamate) (PMHD) (5mmol), dioxane (50mL), isoprene (125mmol) and initiator di-tert-butyl peroxide (DTBP) (1.5mmol) prepared in step (1) and add them to the polymerization tube. The polymerization tube is degassed by three freeze-vacuum-thaw cycles and sealed and pressurized to 0.5MPa under nitrogen protection. The polymerization tube is stirred (500rpm) and reacted at 125°C for 6 hours. After the reaction is completed, the precipitation-centrifugation-dissolution operation is repeated three times in methanol, and the obtained product is finally vacuum dried to obtain the pure product dihydroxy-terminated polyisoprene (HTPI). By 1 H NMR (such as Figure 10 ) It can be confirmed that the structural formula of the double-terminated hydroxyl polyisoprene liquid rubber is
[0108]
[0109] In the formula, X=18-19, Y=1-2, Z=1-2; X is 88-89% of the sum of X, Y, and Z. After testing, its number average molecular weight is about 1800, and its molecular weight distribution is 1.37.
[0110] (3) 2 mmol of HTPI prepared in step (2) was heated to 110°C and vacuumed for 2 hours to remove water. The temperature was then lowered to 70°C, 30 mL of tetrahydrofuran was added to dissolve HTPI, and 3.82 mmol of 4,4-diphenylmethane diisocyanate (MDI) dissolved in tetrahydrofuran was added to react for 2 hours. The reaction was carried out under a nitrogen atmosphere. After the prepolymer was prepared, 1.64 mmol of chain extender 1,4-butanediol (BDO) and 126 μL of catalyst dibutyltin dilaurate (DY-12) dissolved in tetrahydrofuran were added dropwise to the reaction solution and the reaction was continued for 1 hour. After the reaction was completed, the reaction solution was poured into a tetrafluoroethylene mold, placed at room temperature for 12 hours, and then cured in a vacuum oven at 80°C for 24 hours. A linear polyisoprene-based polyurethane elastomer (HTPI-1800-LPU) with a soft segment molecular weight of 1800 was obtained, and the mass ratio of the hard segment (HS) to the soft segment (SS) was 25:75. The mass ratio of the hard segment (HS) to the soft segment (SS) is calculated as the ratio of the sum of the mass of the isocyanate, the crosslinker and the chain extender to the total mass of the isocyanate, the crosslinker, the chain extender and the polyisoprene.
[0111] Example 2
[0112] (1) Take 1,4-phenylenebis(methylene)bis(2-hydroxyethyl)bis(trithiocarboxate) (PMHD) (5mmol), dioxane (50mL), isoprene (275mmol) and initiator di-tert-butyl peroxide (DTBP) (1.5mmol) prepared in Example 1 and add them into a polymerization tube. Degassing treatment is carried out through three freeze-vacuum-thaw cycles, and the tube is sealed and pressurized to 0.5MPa under nitrogen protection. The polymerization tube is stirred (500rpm) and reacted at 125°C for 6 hours. After the reaction is completed, the precipitation-centrifugation-dissolution operation is repeated three times in methanol, and the obtained product is finally vacuum dried to obtain the pure product dihydroxy-terminated polyisoprene (HTPI). By 1 H NMR can confirm that the structure of the dihydroxy-terminated polyisoprene liquid rubber is:
[0113]
[0114] In the formula, X=33-34, Y=1-2, Z=2-3; X is 89-90% of the sum of X, Y, and Z. After testing, its number average molecular weight is about 3000, and its molecular weight distribution is 1.33.
[0115] (2) 1.5 mmol of HTPI prepared in step (1) was heated to 110°C, vacuumed for 2 hours to remove water, and then the temperature was lowered to 70°C. 30 mL of tetrahydrofuran was added to dissolve the HTPI, and 3.05 mmol of 4,4-diphenylmethane diisocyanate (MDI) dissolved in tetrahydrofuran was added to react for 2 hours. The reaction was carried out under a nitrogen atmosphere. After the prepolymer was prepared, 1.40 mmol of chain extender 1,4-butanediol (BDO) and 149 μL of catalyst dibutyltin dilaurate (DY-12) dissolved in tetrahydrofuran were added dropwise to the reaction solution and the reaction was continued for 1 hour. After the reaction was completed, the reaction solution was poured into a tetrafluoroethylene mold, first placed at room temperature for 12 hours, and then cured in a vacuum oven at 80°C for 24 hours. A linear polyisoprene-based polyurethane elastomer (HTPI-3000-LPU) with a soft segment molecular weight of 1800 was obtained, and the mass ratio of the hard segment (HS) to the soft segment (SS) was 25:75.
[0116] Example 3
[0117] (1) Take 1,4-phenylenebis(methylene)bis(2-hydroxyethyl)bis(trithiocarboxate) (PMHD) (5mmol), dioxane (50mL), isoprene (500mmol) and initiator di-tert-butyl peroxide (DTBP) (1.5mmol) prepared in Example 1 and add them into a polymerization tube. Degassing treatment is carried out through three freeze-vacuum-thaw cycles, and the tube is sealed and pressurized to 0.5MPa under nitrogen protection. The polymerization tube is stirred (500rpm) and reacted at 125°C for 6 hours. After the reaction is completed, the precipitation-centrifugation-dissolution operation is repeated three times in methanol, and the obtained product is finally vacuum dried to obtain the pure product dihydroxy-terminated polyisoprene (HTPI). By 1 H NMR can confirm that the structure of the dihydroxy-terminated polyisoprene liquid rubber is:
[0118]
[0119] In the formula, X=46-47, Y=2-3, Z=3-4; X is 89-90% of the sum of X, Y, and Z. After testing, its number average molecular weight is about 3900, and its molecular weight distribution is 1.36.
[0120] (2) 1 mmol of HTPI prepared in step (1) was heated to 110°C, vacuumed for 2 hours to remove water, and then the temperature was lowered to 70°C. 30 mL of tetrahydrofuran was added to dissolve the HTPI, and 2.55 mmol of 4,4-diphenylmethane diisocyanate (MDI) dissolved in tetrahydrofuran was added to react for 2 hours. The reaction was carried out under a nitrogen atmosphere. After the prepolymer was prepared, 1.43 mmol of chain extender 1,4-butanediol (BDO) and 129 μL of catalyst dibutyltin dilaurate (DY-12) dissolved in tetrahydrofuran were added dropwise to the reaction solution and the reaction was continued for 1 hour. After the reaction was completed, the reaction solution was poured into a tetrafluoroethylene mold, first placed at room temperature for 12 hours, and then cured in a vacuum oven at 80°C for 24 hours. A linear polyisoprene-based polyurethane elastomer (HTPI-3900-LPU) with a soft segment molecular weight of 3900 was obtained, and the mass ratio of the hard segment (HS) to the soft segment (SS) was 25:75.
[0121] Example 4
[0122] (1) Take 1,4-phenylenebis(methylene)bis(2-hydroxyethyl)bis(trithiocarboxate) (PMHD) (5mmol), dioxane (50mL), isoprene (175mmol) and initiator di-tert-butyl peroxide (DTBP) (1.5mmol) prepared in Example 1 and add them into a polymerization tube. Degassing treatment is carried out through three freeze-vacuum-thaw cycles, and the tube is sealed and pressurized to 0.5MPa under nitrogen protection. The polymerization tube is stirred (500rpm) and reacted at 125°C for 6 hours. After the reaction is completed, the precipitation-centrifugation-dissolution operation is repeated three times in methanol, and the obtained product is finally vacuum dried to obtain the pure product dihydroxy-terminated polyisoprene (HTPI). By 1 H NMR can confirm that the structure of the dihydroxy-terminated polyisoprene liquid rubber is:
[0123]
[0124] In the formula, X=21-22, Y=1-2, Z=1-2; X is 88-89% of the sum of X, Y, and Z. After testing, its number average molecular weight is about 2100, and its molecular weight distribution is 1.31.
[0125] (2) 2 mmol of HTPI prepared in step (1) was heated to 110°C, vacuumed for 2 hours to remove water, and then the temperature was lowered to 70°C. 30 mL of tetrahydrofuran was added to dissolve HTPI, and 4.45 mmol of 4,4-diphenylmethane diisocyanate (MDI) dissolved in tetrahydrofuran was added to react for 2 hours. The reaction was carried out under a nitrogen atmosphere. After the prepolymer was prepared, 1.92 mmol of BDO, 150 μL of DY-12, and 0.21 mmol of crosslinking agent trimethylolpropane (TMP) dissolved in tetrahydrofuran were added dropwise to the reaction solution, and the reaction was continued for 1 hour. After the reaction was completed, the reaction solution was poured into a tetrafluoroethylene mold, first placed at room temperature for 12 hours, and then cured in a vacuum oven at 80°C for 24 hours. A cross-linked polyisoprene-based polyurethane elastomer (HS) with a soft segment molecular weight of 2100 was obtained. 25 -SS 75 -CPU); the mass ratio of the hard segment (HS) to the soft segment (SS) is 25:75, and the ratio of the chain extender to the cross-linking agent is 9:1.
[0126] Example 5
[0127] 1.5 mmol of HTPI prepared in step (1) of Example 4 was heated to 110°C, vacuumed for 2 hours to remove water, and then the temperature was lowered to 70°C. 30 mL of tetrahydrofuran was added to dissolve HTPI, and 2.63 mmol of 4,4-diphenylmethane diisocyanate (MDI) dissolved in tetrahydrofuran was added to react for 2 hours. The reaction was carried out under a nitrogen atmosphere. After the prepolymer was prepared, 0.86 mmol of BDO, 107 μL of DY-12, and 0.10 mmol of crosslinking agent trimethylolpropane (TMP) dissolved in tetrahydrofuran were added dropwise to the reaction solution, and the reaction was continued for 1 hour. After the reaction was completed, the reaction solution was poured into a tetrafluoroethylene mold, first placed at room temperature for 12 hours, and then cured in a vacuum oven at 80°C for 24 hours. A cross-linked polyisoprene-based polyurethane elastomer (HS) with a soft segment molecular weight of 2100 was obtained. 20 -SS 80 -CPU); the mass ratio of the hard segment (HS) to the soft segment (SS) is 20:80, and the ratio of the chain extender to the cross-linking agent is 9:1.
[0128] Example 6
[0129] 1.5 mmol of HTPI prepared in step (1) of Example 4 was heated to 110°C, vacuumed for 2 hours to remove water, and then the temperature was lowered to 70°C. 30 mL of tetrahydrofuran was added to dissolve HTPI, and 1.98 mmol of 4,4-diphenylmethane diisocyanate (MDI) dissolved in tetrahydrofuran was added to react for 2 hours. The reaction was carried out under a nitrogen atmosphere. After the prepolymer was prepared, 0.33 mmol of BDO, 101 μL of DY-12, and 0.04 mmol of crosslinking agent trimethylolpropane (TMP) dissolved in tetrahydrofuran were added dropwise to the reaction solution, and the reaction was continued for 1 hour. After the reaction was completed, the reaction solution was poured into a tetrafluoroethylene mold, first placed at room temperature for 12 hours, and then cured in a vacuum oven at 80°C for 24 hours. A cross-linked polyisoprene-based polyurethane elastomer (HS) with a soft segment molecular weight of about 2100 was obtained. 15 -SS 85 -CPU); the mass ratio of the hard segment (HS) to the soft segment (SS) is 15:85, and the ratio of the chain extender to the cross-linking agent is 9:1.
[0130] Example 7
[0131] 1.5 mmol of HTPI prepared in step (1) of Example 4 was heated to 110°C and vacuumed for 2 hours to remove water. The temperature was then lowered to 70°C, and 30 mL of tetrahydrofuran was added to dissolve the HTPI. 3.38 mmol of 4,4-diphenylmethane diisocyanate (MDI) dissolved in tetrahydrofuran was then added and allowed to react for 2 hours. The reaction was carried out under a nitrogen atmosphere. After the prepolymer was prepared, 1.37 mmol of BDO, 114 μL of DY-12, and 0.23 mmol of the crosslinker trimethylolpropane (TMP) dissolved in tetrahydrofuran were added dropwise to the reaction solution. The reaction was continued for 1 hour. After the reaction was completed, the reaction solution was poured into a tetrafluoroethylene mold and allowed to stand at room temperature for 12 hours before being cured in a vacuum oven at 80°C for 24 hours. A cross-linked polyisoprene-based polyurethane elastomer (B6-T1-CPU) with a soft segment molecular weight of 2100 was obtained; the mass ratio of the hard segment (HS) to the soft segment (SS) was 25:75, and the ratio of the chain extender to the cross-linker was 6:1.
[0132] Example 8
[0133] 1.5 mmol of HTPI prepared in step (1) of Example 4 was heated to 110°C and vacuumed for 2 hours to remove water. The temperature was then lowered to 70°C, and 30 mL of tetrahydrofuran was added to dissolve the HTPI. 3.38 mmol of 4,4-diphenylmethane diisocyanate (MDI) dissolved in tetrahydrofuran was then added and allowed to react for 2 hours. The reaction was carried out under a nitrogen atmosphere. After the prepolymer was prepared, 1.15 mmol of BDO, 114 μL of DY-12, and 0.38 mmol of the crosslinker trimethylolpropane (TMP) dissolved in tetrahydrofuran were added dropwise to the reaction solution. The reaction was continued for 1 hour. After the reaction was completed, the reaction solution was poured into a tetrafluoroethylene mold and allowed to stand at room temperature for 12 hours before being cured in a vacuum oven at 80°C for 24 hours. A cross-linked polyisoprene-based polyurethane elastomer (B3-T1-CPU) with a soft segment molecular weight of 2100 was obtained; the mass ratio of the hard segment (HS) to the soft segment (SS) was 25:75, and the ratio of the chain extender to the cross-linker was 3:1.
[0134] Performance Testing
[0135] The thermal and mechanical properties of the polyisoprene-based polyurethane elastomers prepared in Examples 1-8 were tested. Figure 1 、 Figure 4 、 Figure 7 As shown, the DMA test results are as follows Figure 3 、 Figure 6 、 Figure 9 The stress-strain curve is shown in Figure 2 、 Figure 5 、 Figure 8 .
[0136] Depend on Figure 1 、 Figure 4 、 Figure 7 It can be seen that the glass transition temperatures of the polyisoprene-based polyurethanes prepared in Examples 1-8 are all below -50°C. This indicates that the polyisoprene-based polyurethanes synthesized using dihydroxy-terminated polyisoprene as the soft segment of the present invention have a low glass transition temperature, excellent low-temperature resistance, and can maintain good stability in low-temperature environments.
[0137] Depend on Figure 2 、 Figure 5 、 Figure 8 It can be seen that the elongation at break of the polyisoprene-based polyurethanes prepared in Examples 1-8 can reach 450, and the tensile strength can reach 11.63 MPa, indicating that the polyisoprene-based polyurethanes synthesized using dihydroxy-terminated polyisoprene as the soft segment of the present invention have excellent mechanical properties.
[0138] Depend on Figure 3 、 Figure 6 、 Figure 9It can be concluded that the storage modulus of the polyisoprene-based polyurethanes prepared in Examples 1-8 can reach 2911 MPa and the loss factor is close to 1. This indicates that the polyisoprene-based polyurethanes synthesized using dihydroxy-terminated polyisoprene as the soft segment of the present invention have low energy dissipation and can effectively reduce wear.
[0139] Compare Figure 1-Figure 3 It has been found that when the hard segment content of linear polyurethane remains constant, the continuity of the hard segment phase decreases as the soft segment molecular weight increases. This is manifested as a lower glass transition temperature, decreased mechanical properties, lower tensile strength and elongation at break, and a lower storage modulus. However, its loss factor is close to 1, meaning that the storage modulus is close to the loss modulus, indicating that the polyurethane has low energy dissipation and can effectively reduce wear.
[0140] Compare Figure 4-Figure 6 It was found that when the soft segment molecular weight of the cross-linked polyurethane remains unchanged, the chemical structure of the polyurethane is not affected when the hard segment content of the cross-linked polyurethane is changed. Increasing the hard segment content leads to a higher degree of microphase separation, making the polyurethane stronger, with higher tensile strength and elongation at break. The glass transition temperature of the polyurethane slightly increases, and the storage modulus slightly decreases, with no significant change in the thermal properties of the polyurethane.
[0141] Compare Figure 7-Figure 9 It can be found that when a cross-linking agent is added to form a cross-linked (bulk) polyurethane, the change in the ratio of chain extender to cross-linker mainly affects the cross-linking density and toughness of the polyurethane. As the amount of cross-linking agent increases, the number of cross-linking points in the polyurethane network increases, the cross-linking density increases, and the freedom of chain segment movement is restricted. The polyurethane material tends to be rigid, which weakens the toughness of the polyurethane material, manifested as a lower storage modulus and loss factor, a slight increase in the glass transition temperature of the polyurethane material, and a decrease in the elongation at break.
Claims
1. A polyisoprene-based polyurethane, characterized in that: The polyisoprene-based polyurethane comprises repeating structural units represented by formula A, formula B, and formula C; In formula A, R0 is -CH2, -CH2CH2 or -CH(CH3), preferably -CH2; X=15~50, Y=1~3, Z=1~4; Preferably, X=18~19, Y=1~2, Z=1~2, X=21~22, Y=1~2, Z=1~2, X is 88-92% of the sum of X, Y, and Z, preferably 88-90%; Formula B is a structural unit derived from isocyanate, and R1 is preferably selected from Formula C is a structural unit derived from a small molecule diol, and R2 is preferably selected from -CH2CH2CH2CH2-.
2. The polyisoprene-based polyurethane according to claim 1, wherein The molar ratio of the repeating structural units represented by Formula A, Formula B and Formula C is 0.25-0.52:1:0.37-0.6, preferably 0.39-0.45:1:0.43-0.
48.
3. The polyisoprene-based polyurethane according to claim 1, wherein Comprising a repeating structural unit represented by formula D; Formula D is a structural unit derived from a small molecule triol, and R3 is preferably selected from -CH2CR3(CH3)-CH2-.
4. The polyisoprene-based polyurethane according to claim 3, wherein The molar ratio of the repeating structural units represented by formula D to formula B is 0.042-0.068:1, preferably 0.047-0.054:
1.
5. A method for preparing the polyisoprene-based polyurethane according to any one of claims 1 to 4, characterized in that: The preparation method comprises: dissolving the double-terminal hydroxyl polyisoprene after dehydration with solvent A, adding isocyanate dissolved in solvent A, and pre-reacting for 2-5 hours; adding a chain extender-catalyst solution dropwise, and reacting for 1-3 hours; and curing the reaction liquid to obtain the polyisoprene-based polyurethane; The pre-reaction and reaction are carried out under nitrogen atmosphere at 75-85°C; The chain extender-catalyst solution comprises a chain extender, a catalyst and a solvent A; When the polyisoprene-based polyurethane comprises a repeating structural unit represented by Formula D, the chain extender-catalyst solution further comprises a crosslinking agent.
6. The preparation method according to claim 5, characterized in that: The isocyanate is selected from at least one of 4,4-diphenylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, and dicyclohexylmethane diisocyanate; or / and, The chain extender is selected from small molecule diols, preferably 1,4-butanediol; or / and, The cross-linking agent is selected from small molecule triols, preferably trimethylolpropane or glycerol; The solvent A is selected from at least one of tetrahydrofuran, dioxane, dichloromethane and dimethylformamide; The catalyst is selected from organic tin or tertiary amine catalysts; preferably dibutyltin dilaurate.
7. The preparation method according to claim 5, characterized in that: The structural formula of the double-terminal hydroxyl polyisoprene is shown in formula (I); In formula (I), R is -CH2OH, -CH2CH2OH, -CH(CH3)OH, preferably -CH2OH; X=15~50, Y=1~3, Z=1~4; Preferably, X=18~19, Y=1~2, Z=1~2, X=21~22, Y=1~2, Z=1~2, X is 88-92% of the total of X, Y and Z, preferably 88-90%.
8. The preparation method according to claim 7, characterized in that: The number average molecular weight of the dihydroxy-terminated polyisoprene is 1000-50000 g / mol, preferably 1800-3900 g / mol; the molecular weight distribution of the dihydroxy-terminated polyisoprene is less than 1.7, preferably less than 1.
4.
9. The preparation method according to claim 7, characterized in that: The preparation method of the dihydroxy-terminated polyisoprene comprises: Isoprene, chain transfer agent, initiator and solvent B are mixed, heated and pressurized to react, so as to obtain the dihydroxy-terminated polyisoprene liquid rubber; the reaction temperature is 65-130° C.; the reaction pressure is 0.5-1 MPa; and the reaction time is 2-24 hours; The molar ratio of the isoprene, the chain transfer agent, the initiator and the solvent is 100-2000:1:0.2-0.5:100-500; preferably 500-1000:1:0.3-0.5:200-400.
10. The preparation method according to claim 9, characterized in that: The structure of the chain transfer agent is shown in formula (II), In formula (II), R is -CH2OH, -CH2CH2OH, -CH(CH3)OH; or / and, The initiator comprises an azo initiator and / or an organic peroxide initiator, preferably at least one selected from azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, acetophenone peroxide, and di-tert-butyl peroxide; or / and, The solvent B is selected from at least one of dioxane, tetrahydrofuran, n-hexane and cyclohexane.
Citation Information
Patent Citations
Middle-low molecular weight brominated multi-block copolymer flame retardant and solution two-step preparation method thereof
CN108129619A
Mixed soft segment type polyurethane damping material and preparation method thereof
CN112126034A
Wet-skid-resistant low-rolling-resistance thermoplastic polyurethane elastomer and preparation method thereof
CN112574385A
Poly (methyl) acrylate dihydric alcohol and polyurethane type adhesive synthesized by poly (methyl) acrylate dihydric alcohol
CN112940161A
Hydroxyl-terminated polyisoprene polyurethane synthesized by biological method as well as preparation method and application of hydroxyl-terminated polyisoprene polyurethane
CN113667087A