Solid-liquid flow electrochemical reaction device and application thereof in battery field

Phosphate-based cathode materials are synthesized at room temperature through a solid-liquid-liquid flow electrochemical reaction device, which solves the complex and high-cost problems of sodium iron phosphate battery synthesis in the existing technology, and achieves the preparation of high-performance sodium iron phosphate cathode materials. It has excellent rate and cycle performance and is suitable for applications in the new energy field.

CN118773633APending Publication Date: 2024-10-15SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410811433.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The synthesis method of existing sodium iron phosphate batteries is complex and costly, making it difficult to apply on a large scale. Moreover, the electrochemical performance of sodium iron phosphate is insufficient, which limits its development in the field of new energy.

Method used

A solid-liquid-liquid flow electrochemical reaction device is used to realize the simple synthesis of phosphate cathode materials by utilizing the solid-liquid reaction unit and the cyclic connection of the anode and cathode at normal temperature, combined with the ion exchange membrane, including the iron source, phosphorus source and Active metal sources are mixed to form a precursor solution, and sodium iron phosphate or lithium iron phosphate cathode materials are prepared through an electrolysis process.

Benefits of technology

It achieves efficient synthesis of phosphate cathode materials at room temperature, reduces costs, and improves electrochemical performance, especially the rate and cycle performance of sodium iron phosphate cathode materials, which has market application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773633A_ABST
    Figure CN118773633A_ABST
Patent Text Reader

Abstract

The invention discloses a solid-liquid flow electrochemical reaction device and application thereof in the field of batteries. The solid-liquid flow electrochemical reaction device comprises a solid-liquid reaction unit, an anode unit and a cathode unit, the anode unit and the cathode unit are respectively connected with a positive electrode and a negative electrode of a power supply, the cathode unit is used for storing a halogen reduction electron pair solution, the anode unit is used for storing an organic electrolyte, and the anode unit and the cathode unit are communicated through a pipeline; an ion exchange membrane is arranged in the pipeline and is used for enabling active ions generated by anode electrolysis to unidirectionally pass through and enter the cathode unit; the solid-liquid reaction unit is circularly connected with the cathode unit, the solid-liquid reaction unit comprises a feed port and a discharge port, and the feed port is used for adding a precursor solution of a phosphate positive electrode material. The solid-liquid flow electrochemical reaction device provided by the invention can be used for synthesizing a phosphate positive electrode material at normal temperature, and compared with a high-temperature sintering process, the cost is controllable, and the safety is high; compared with an ion exchange method, the electrochemical performance of the sodium iron phosphate positive electrode prepared by the device is better. The solid-liquid flow electrochemical reaction device disclosed by the invention is high in integration degree, and is expected to be applied to the field of preparation of phosphate positive electrode materials on the market.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery material preparation, and relates to a solid-liquid-liquid flow electrochemical reaction device and its application in the battery field. Background Art

[0002] In recent years, with the vigorous development of the new energy industry, especially the lithium-ion secondary battery industry has entered a period of rapid development. At the same time, global lithium resources have been severely consumed, causing lithium prices to continue to rise.

[0003] As a lithium-poor country, my country's development of new energy is severely restricted by the lack of lithium resources. Researchers have begun to pay attention to other alkali metal ion batteries. Among them, sodium ion batteries are expected to enter the secondary battery market first due to their abundant resources, low prices, and excellent low-temperature performance.

[0004] Currently, lithium iron phosphate batteries are widely used in new energy storage and power battery markets. The development of corresponding sodium iron phosphate is particularly important. However, currently most sodium iron phosphates are produced by the replacement method, which is difficult to synthesize and expensive, making it difficult to use on a large scale.

[0005] Therefore, developing a simple synthesis method for phosphate-based positive electrode materials is a technical problem that needs to be solved urgently. Summary of the invention

[0006] In view of the above problems existing in the prior art, the object of the present invention is to provide a solid-liquid-liquid flow electrochemical reaction device and its application in the battery field.

[0007] To achieve the above object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a solid-liquid-liquid flow electrochemical reaction device, characterized in that the solid-liquid-liquid flow electrochemical reaction device comprises a solid-liquid reaction unit, an anode unit and a cathode unit, the anode unit and the cathode unit are respectively connected to the positive electrode and the negative electrode of a power supply, the cathode unit is used to store a halogen reduction electron pair solution, the anode unit is used to store an organic electrolyte, the anode unit and the cathode unit are connected through a pipeline, an ion exchange membrane is provided in the pipeline, and the ion exchange membrane is used to allow active ions generated by anode electrolysis to pass into the cathode unit in a unidirectional manner;

[0009] The solid-liquid reaction unit is cyclically connected to the cathode unit. The solid-liquid reaction unit comprises a feed inlet and a discharge inlet. The feed inlet is used to add a precursor solution of a phosphate-based positive electrode material.

[0010] In the present invention, the phosphate-based positive electrode material may be a sodium iron phosphate positive electrode material or a lithium iron phosphate positive electrode material.

[0011] The solid-liquid-liquid-flow electrochemical reaction device provided by the present invention can synthesize phosphate-based positive electrode materials at room temperature. Compared with the high-temperature sintering process, the cost is controllable and the safety is high. Compared with the ion exchange method, the electrochemical performance of the sodium iron phosphate positive electrode prepared by the device of the present invention is better. The solid-liquid-liquid-flow electrochemical reaction device of the present invention has a high degree of integration and is expected to be the first to be commercialized in the field of phosphate-based positive electrode material preparation.

[0012] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0013] Preferably, a circulation pump is provided on the circulation connection pipeline for allowing the solution in the cathode unit to enter the solid-liquid reaction unit.

[0014] Preferably, the feed inlet is communicated with a grinding device.

[0015] Preferably, the grinding equipment includes any one of a nano grinder and a sand mill.

[0016] Preferably, the discharge port is communicated with a sprayer.

[0017] In a second aspect, the present invention provides a method for preparing a sodium iron phosphate positive electrode material using the solid-liquid-liquid flow electrochemical reaction device as described in the first aspect, the method comprising the following steps:

[0018] (1) mixing an iron source, a phosphorus source, an active metal source and a solvent to obtain a precursor solution of a sodium iron phosphate positive electrode material, wherein the active metal source includes at least one of a lithium source and a sodium source;

[0019] (2) Adding the precursor solution of the sodium iron phosphate positive electrode material to the solid-liquid reaction unit through the feed port, adding the halogen reduction electron pair solution and the organic electrolyte to the cathode unit and the anode unit respectively, starting the circulation pump and the electrolysis device, and after circulating for a period of time at a certain current density and liquid circulation flow rate, discharging the feed liquid through the discharge port, and obtaining the phosphate-based positive electrode material after drying.

[0020] In the method of the present invention, when the prepared phosphate-based positive electrode material is sodium iron phosphate, the active metal source in step (1) is a sodium source; when the prepared phosphate-based positive electrode material is lithium iron phosphate, the active metal source in step (1) is a lithium source.

[0021] The method of the present invention utilizes solid-liquid-liquid flow electrochemical reaction to prepare phosphate-based positive electrode materials. The mechanism is described by taking sodium iron phosphate as an example of the phosphate-based positive electrode material, as follows:

[0022] 3X - +2FePO4+2Na+ →2NaFePO4+X3 - (X is a halogen atom)

[0023] Liquid flow reaction mechanism:

[0024] Cathode: X3 - +e - →3X -

[0025] Anode: Na-e - →Na +

[0026] The method of the present invention is simple and does not require high-temperature treatment. High-performance phosphate-based positive electrode materials can be prepared at room temperature, thereby reducing preparation costs. Moreover, the primary particles prepared by the present invention have a small particle size and high compaction, and the sodium ion battery prepared using the primary particles has excellent rate performance and cycle performance.

[0027] Preferably, the iron source and phosphorus source in step (1) are derived from iron phosphate.

[0028] Preferably, the A value of the iron phosphate is 3 to 4, and the B value is 1.5 to 1.8, wherein the A value is the ratio of the 101 peak intensity to the 210 peak intensity in the XRD of the iron phosphate, and the B value is the ratio of the 101 peak intensity to the 200 peak intensity. Exemplarily, the A value may be, for example, 3, 3.2, 3.3, 3.4, 3.6, 3.8 or 4, etc.; the B value may be, for example, 1.5, 1.6, 1.7 or 1.8, etc.

[0029] Preferably, the iron phosphate is iron phosphate prepared by recycling retired lithium iron phosphate batteries, so as to realize the recycling of circulating resources. The recycling method is not limited, for example, it can be an extraction method.

[0030] Preferably, the sodium source in step (1) comprises at least one of trisodium phosphate, sodium carbonate and sodium sulfate;

[0031] Preferably, in the precursor solution of the phosphate-based cathode material in step (1), the phosphate-based cathode material includes sodium iron phosphate and / or lithium iron phosphate, and the molar ratio of sodium and / or lithium to Fe is 1.02 to 1.05, for example, it can be 1.02, 1.03, 1.04 or 1.05.

[0032] Preferably, the solid content of the precursor solution of the phosphate-based cathode material in step (1) is 30% to 40%, for example, it may be 30%, 32%, 33%, 35%, 36%, 38% or 40%.

[0033] Preferably, the solute in the halogen-reduced electron pair solution in step (2) is a sodium-based solute and / or a lithium-based solute.

[0034] Preferably, the sodium-based solute includes at least one of sodium iodide, sodium bromide and sodium fluoride.

[0035] Preferably, the solvent in the halogen-reduced electron pair solution in step (2) is water.

[0036] Preferably, the concentration of the halogen-reduced electron pair solution in step (2) is 2 mol / L to 3 mol / L, for example, 2 mol / L, 2.2 mol / L, 2.3 mol / L, 2.4 mol / L, 2.6 mol / L, 2.8 mol / L or 3 mol / L.

[0037] Preferably, the organic electrolyte in step (2) comprises a solute and an organic solvent.

[0038] Preferably, the solute in the organic electrolyte is a sodium salt and / or a lithium salt.

[0039] Preferably, the sodium salt comprises at least one of NaPF6 and sodium bisfluorosulfonamide (NaFSI).

[0040] Preferably, the organic solvent includes at least one of ethylene carbonate (EC) and dimethyl carbonate (DMC).

[0041] Preferably, the concentration of the organic electrolyte is 1 mol / L to 2 mol / L, for example, it may be 1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L or 2 mol / L.

[0042] Preferably, the cathode in the cathode unit includes one of Ti, Ta, Pt, Au and alloys thereof, but is not limited to the above-listed types. Other inert electrode metals commonly used in the art are also applicable to the present invention.

[0043] Preferably, the anode in the anode unit is metallic sodium and / or metallic lithium.

[0044] Preferably, the certain current density is 500 mA / cm 2 ~800mA / cm 2 , for example, it can be 500mA / cm 2 , 525mA / cm 2 , 550mA / cm 2 、580mA / cm 2 、600mA / cm 2 、630mA / cm 2 、660mA / cm 2 、680mA / cm 2 , 700mA / cm2 , 730mA / cm 2 , 750mA / cm 2 、770mA / cm 2 or 800mA / cm 2 wait.

[0045] Preferably, the liquid circulation flow rate is 100 μL / s to 200 μL / s, for example, it can be 100 μL / s, 110 μL / s, 120 μL / s, 140 μL / s, 160 μL / s, 180 μL / s or 200 μL / s.

[0046] Preferably, the cycle time is 10 h to 15 h, for example, 10 h, 11 h, 12 h, 13 h, 14 h or 15 h.

[0047] Preferably, the voltage used by the electrolysis device is 3.6V to 4.5V, for example, it can be 3.6V, 3.7V, 3.8V, 3.9V, 4.0V, 4.2V, 4.3V or 4.5V.

[0048] As a preferred technical solution of the method of the present invention, the method further comprises grinding the precursor solution of the sodium iron phosphate positive electrode material obtained in step (1), and then adding the solid-liquid reaction unit after grinding to a certain particle size.

[0049] Preferably, the certain particle size is: D50 is 0.5μm to 0.7μm, for example, it can be 0.5μm, 0.6μm or 0.7μm, etc.; the particle size concentration C is 2 to 4, for example, it can be 2, 2.2, 2.5, 2.8, 3, 3.2, 3.4, 3.6, 3.8 or 4, etc., wherein the particle size concentration C = (D90-D10) / D50.

[0050] Preferably, the method of the present invention comprises the steps of filtering and washing the feed liquid before drying.

[0051] In some embodiments, the drying method may be oven drying.

[0052] As a preferred technical solution of the method of the present invention, the method also includes preparing a coating liquid with the powder obtained after drying and a carbon source, and spray drying with the coating liquid to obtain a sodium iron phosphate positive electrode material coated with a carbon material.

[0053] Preferably, the carbon source is an inorganic carbon source.

[0054] Preferably, the inorganic carbon source includes at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes, carbon black, graphene and C60.

[0055] Preferably, the added amount of the inorganic carbon source accounts for 2% to 3% of the mass of the powder, for example, it can be 2%, 2.2%, 2.5%, 2.7%, 2.8% or 3%.

[0056] Preferably, the inlet air temperature of the spray drying is 170°C to 200°C, for example, 170°C, 180°C, 190°C, 195°C or 200°C.

[0057] Preferably, the coating liquid is ground before the spray drying.

[0058] In a third aspect, the present invention provides a sodium iron phosphate positive electrode material, which is prepared by the method described in the second aspect.

[0059] Preferably, the surface of the sodium iron phosphate positive electrode material is coated with a carbon material.

[0060] In a fourth aspect, the present invention provides a positive electrode, wherein the positive electrode comprises the sodium iron phosphate positive electrode material described in the third aspect.

[0061] In a fifth aspect, the present invention provides a sodium ion battery, comprising the positive electrode described in the fourth aspect.

[0062] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0063] Compared with the prior art, the present invention has the following beneficial effects:

[0064] (1) The solid-liquid-liquid flow electrochemical reaction device provided by the present invention can synthesize phosphate-based cathode materials at room temperature. Compared with the high-temperature sintering process, the cost is controllable and the safety is high. The solid-liquid-liquid flow electrochemical reaction device of the present invention has a high degree of integration and is expected to be the first to be commercialized in the field of phosphate-based cathode material preparation.

[0065] (2) The method of the present invention is simple and does not require high-temperature treatment. High-performance phosphate-based positive electrode materials can be prepared at room temperature, thereby reducing the preparation cost. Moreover, the primary particles prepared by the present invention have a small particle size and high compaction. The sodium ion battery prepared using the primary particles has excellent rate performance and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] Figure 1 It is a schematic structural diagram of a solid-liquid-liquid flow electrochemical reaction device provided in one embodiment of the present invention.

[0067] Figure 2 It is a comparison chart of the XRD spectrum of the sodium iron phosphate synthesized in Example 1 and the standard card. DETAILED DESCRIPTION

[0068] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0069] The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0070] One embodiment of the present invention provides a solid-liquid-liquid flow electrochemical reaction device, the structural schematic diagram of which is shown in FIG. Figure 1 The solid-liquid-liquid flow electrochemical reaction device comprises a solid-liquid reaction unit 1, an anode unit 2 and a cathode unit 3, wherein the anode unit 2 and the cathode unit 3 are respectively connected to the positive electrode and the negative electrode of the power supply, the cathode unit 3 is used to store a halogen reduction electron pair solution, the anode unit 2 is used to store an organic electrolyte, the anode unit 2 and the cathode unit 3 are connected through a pipeline, an ion exchange membrane 4 is provided in the pipeline, and the ion exchange membrane 4 is used to allow active ions generated by anode electrolysis to pass into the cathode unit 3 in a unidirectional manner;

[0071] The solid-liquid reaction unit 1 is cyclically connected to the cathode unit 3 . The solid-liquid reaction unit 1 comprises a feed port 11 and a discharge port 12 . The feed port 11 is used to add a precursor solution of a phosphate-based positive electrode material.

[0072] The circulating connection pipeline is provided with a circulating pump 5 for allowing the solution in the cathode unit 3 to enter the solid-liquid reaction unit 1 .

[0073] The feed port 11 is communicated with the grinding device 6 .

[0074] The grinding device 6 includes any one of a nano grinder and a sand grinder.

[0075] The discharge port 12 is communicated with the sprayer 7 .

[0076] In another embodiment, the present invention provides a method for preparing a sodium iron phosphate positive electrode material using the above-mentioned solid-liquid-liquid flow electrochemical reaction device, the method comprising the following steps:

[0077] (1) mixing an iron source, a phosphorus source, an active metal source and a solvent to obtain a precursor solution of a sodium iron phosphate positive electrode material, wherein the active metal source includes at least one of a lithium source and a sodium source;

[0078] (2) Adding the precursor solution of the sodium iron phosphate positive electrode material to the solid-liquid reaction unit through the feed port, adding the halogen reduction electron pair solution and the organic electrolyte to the cathode unit and the anode unit respectively, starting the circulation pump and the electrolysis device, and discharging the feed liquid through the discharge port after the circulating liquid circulates for a period of time at a certain current density, and obtaining the phosphate-based positive electrode material after drying.

[0079] The following are typical but non-limiting examples:

[0080] Example 1

[0081] This embodiment provides a method for preparing sodium iron phosphate, comprising the following steps:

[0082] Step 1: Take 100g of iron phosphate with an A value of 3.21 and a B value of 1.68 and 40g of sodium carbonate, add water and stir to prepare a solution A with a solid content of 30%;

[0083] The second step is to put solution A into a nano-grinder for grinding. The particle size of the material obtained by grinding satisfies: D50 is 0.5 μm, particle size concentration C = (D90-D10) / D50 = 2.3, and the solution is discharged to obtain solution B.

[0084] Step 3: Add solution B into the solid-liquid reactor, start the circulation pump, control the liquid circulation flow rate to 150 μL / s, start the power supply, and control the current density to 600 mA / cm 2 , cycle 12h.

[0085] The fourth step is to discharge the solid after the completion of the third step reaction, wash it with clean water three times and then dry it, take 100g of the material, add it into an aqueous solution with a solid content of 30% prepared by 2g of carbon nanotubes, and spray dry it in a spray dryer (wherein the inlet air temperature is 170°C) to obtain a sodium iron phosphate positive electrode material coated with a carbon material.

[0086] Figure 2 1 is a comparison chart of the XRD spectrum of the sodium iron phosphate synthesized in this embodiment and the standard card. It can be seen from the figure that the sodium iron phosphate is successfully synthesized in the present invention.

[0087] Example 2

[0088] The difference between Example 2 and Example 1 is that the A value of the iron phosphate precursor in the first step is 1.68 and the B value is 3.

[0089] Example 3

[0090] The difference between Example 3 and Example 1 is that in the second step, the concentrated particle size C is 10.

[0091] Example 4

[0092] The difference between Example 4 and Example 1 is that in the third step, the liquid circulation flow rate is 300 μL / s.

[0093] Example 5

[0094] The difference between Example 5 and Example 1 is that in the third step, the cycle time is 5 hours.

[0095] Example 6

[0096] The difference between Example 6 and Example 1 is that in the third step, the cycle time is 20 hours.

[0097] Example 7

[0098] The difference between Example 7 and Example 1 is that in the fourth step, the amount of carbon nanotubes used is 0.5 g.

[0099] Example 8

[0100] The difference between Example 8 and Example 1 is that in the fourth step, the amount of carbon nanotubes used is 5 g.

[0101] Example 9

[0102] Step 1: Take 100g of iron phosphate with an A value of 3.14 and a B value of 1.73 and 36g of sodium carbonate, add water and stir to prepare a solution A with a solid content of 35%;

[0103] The second step is to put solution A into a nano-grinder for grinding. The particle size of the material obtained by grinding satisfies: D50 is 0.6 μm, particle size concentration C = (D90-D10) / D50 = 3.2, and the solution is discharged to obtain solution B.

[0104] Step 3: Add solution B into the solid-liquid reactor, start the circulation pump, control the liquid circulation flow rate to 180 μL / s, start the power supply, and control the current density to 800 mA / cm 2 , cycle 12h.

[0105] Step 4: Discharge the solid after the reaction in step 3, wash it with clean water three times and then dry it. Take 100g of the material and add it to an aqueous solution with a solid content of 30% prepared by 3g of carbon nanotubes. Spray dry it in a spray dryer (wherein the air inlet temperature is 170°C) to obtain a sodium iron phosphate positive electrode material coated with a carbon material.

[0106] Comparative Example 1

[0107] Comparative Example 1: Sodium iron phosphate was prepared by ion exchange method, comprising the following steps:

[0108] First, lithium iron phosphate is deeply electrolyzed at 4.5V to prepare ferric phosphate, and then the ferric phosphate is used as the cathode and the sodium sheet as the anode, and placed in a 1M NaPF6 organic solution and electrolyzed at 3.6V for 10h to obtain sodium iron phosphate by ion exchange method.

[0109] Button assembly: Using a metal sodium sheet as the negative electrode, the positive electrode sheet is prepared using the sodium iron phosphate positive electrode material prepared in Examples 1 to 9 and Comparative Example 1. The method for preparing the positive electrode sheet is as follows: using NMP as a solvent, according to the positive electrode material, binder (PVDF), conductive agent (SP) weight ratio of 90:5:5, the positive electrode material, PVDF glue (solid content of 6.05%) and SP are mixed in the solvent, and after mixing evenly, the mixture is coated on both sides of the aluminum foil. The thickness of the aluminum foil is 12 μm, the purity of the aluminum foil is more than 99%, and the pole piece is compacted to 2.5 g / cm 3 , using Celgand2325 as the separator, assembled into a button-type half-cell in a vacuum glove box.

[0110] Performance Test:

[0111] (1) Battery performance test: The assembled button cell was subjected to a performance test using the following test methods: 0.1C charging to 3.65V, 0.1C discharging to 2.0V, nominal capacity 150mAh / g, 1C cycle for 50 cycles.

[0112] (2) Powder compaction density test: Take 1g of positive electrode material powder and put it into the mold for testing compaction density. Record the initial height h0, then put it into the press, apply a pressure of 2T, maintain the pressure for 1min, and test the height h1 after pressing. The calculation formula of compaction density is:

[0113] ρ=m1 / ((h0-h1)*Π / 4*D 2 )

[0114] Among them, ρ is the compaction density, m1 is the mass of the positive electrode material powder, and D is the diameter of the mold.

[0115] The test results are shown in Table 1.

[0116] Table 1

[0117] Implementation / Comparative Example 1C / 0.1C 1C cycle 50 weeks capacity retention rate (%) <![CDATA[Composite powder compaction 2T (g / cm 3 )]]> Example 1 0.88 94.6 2.38 Example 2 0.82 93.1 2.24 Example 3 0.83 92.4 2.31 Example 4 0.84 91.8 2.28 Example 5 0.86 92.5 2.33 Example 6 0.81 93.1 2.27 Example 7 0.80 92.1 2.39 Example 8 0.89 93.3 2.03 Example 9 0.88 94.5 2.37 Comparative Example 1 0.76 87.3 2.13

[0118] It can be seen from Table 1 that the present invention successfully synthesized a high-performance sodium iron phosphate positive electrode material. Compared with the sodium iron phosphate positive electrode prepared by the ion exchange method (Comparative Example 1), the rate cycle performance and the powder compaction density are improved.

[0119] Comparing Example 2 with Example 1, it can be seen that the A value of the iron phosphate precursor is low and the B value is large. The precursor is iron-rich iron phosphate. The use of iron-rich iron phosphate positive electrode material to synthesize the positive electrode sodium ion migration channel leads to a decrease in the battery rate performance.

[0120] Comparing Example 3 with Example 1, it can be seen that the concentrated particle size of Solution B is too large and there are large particles with larger particle size. On the one hand, the reaction is incomplete in the solid-liquid reaction. On the other hand, the particle size of the primary particles of the synthesized positive electrode material becomes larger and the rate performance becomes worse.

[0121] By comparing Example 4 and Example 5 with Example 1, it can be seen that due to the excessive reaction flow rate or the short reaction time, the phase purity of the synthesized sodium iron phosphate positive electrode material is low, resulting in excessive impurity phases and poor cycle performance.

[0122] By comparing Example 6 with Example 1, it can be seen that the reaction time is too long, and the sodium ions are not completely embedded in the iron phosphate in the later stage, but are adsorbed on the surface of the positive electrode material, resulting in an increase in the residual alkali content of the material and a deterioration in the cycle performance.

[0123] By comparing Example 7 with Example 1, it can be seen that when the carbon content used is too low, the conductivity of the synthesized positive electrode material deteriorates, thereby reducing the battery rate and cycle performance.

[0124] It can be seen from the comparison between Example 8 and Example 1 that when the carbon content used is too high, the compaction density of the positive electrode material will be greatly reduced.

[0125] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A solid-liquid-liquid flow electrochemical reaction device, It is characterized in that The solid-liquid-liquid flow electrochemical reaction device comprises a solid-liquid reaction unit, an anode unit and a cathode unit, wherein the anode unit and the cathode unit are respectively connected to the positive electrode and the negative electrode of the power supply, the cathode unit is used to store a halogen reduction electron pair solution, and the anode unit is used to store an organic electrolyte. The anode unit and the cathode unit are connected through a pipeline, and an ion exchange membrane is provided in the pipeline, and the ion exchange membrane is used to allow active ions generated by anode electrolysis to pass into the cathode unit in a unidirectional manner; The solid-liquid reaction unit is cyclically connected to the cathode unit. The solid-liquid reaction unit comprises a feed inlet and a discharge inlet. The feed inlet is used to add a precursor solution of a phosphate-based positive electrode material.

2. The solid-liquid-liquid flow electrochemical reaction device according to claim 1, It is characterized in that The circulating connection pipeline is provided with a circulating pump for allowing the solution in the cathode unit to enter the solid-liquid reaction unit; Preferably, the feed port is connected to the grinding equipment; Preferably, the grinding equipment includes any one of a nano grinder and a sand mill; Preferably, the discharge port is communicated with a sprayer.

3. A method for preparing sodium iron phosphate positive electrode material using the solid-liquid-liquid flow electrochemical reaction device as claimed in claim 1 or 2, It is characterized in that The method comprises the following steps: (1) mixing an iron source, a phosphorus source, an active metal source and a solvent to obtain a precursor solution of a sodium iron phosphate positive electrode material, wherein the active metal source includes at least one of a lithium source and a sodium source; (2) Adding the precursor solution of the sodium iron phosphate positive electrode material to the solid-liquid reaction unit through the feed port, adding the halogen reduction electron pair solution and the organic electrolyte to the cathode unit and the anode unit respectively, starting the circulation pump and the electrolysis device, and after circulating for a period of time at a certain current density and liquid circulation flow rate, discharging the feed liquid through the discharge port, and obtaining the phosphate-based positive electrode material after drying.

4. The method according to claim 3, It is characterized in that The iron source and phosphorus source in step (1) are derived from iron phosphate; Preferably, the A value of the iron phosphate is 3 to 4, and the B value is 1.5 to 1.8, wherein the A value is the ratio of the 101 peak intensity to the 210 peak intensity in the XRD of the iron phosphate, and the B value is the ratio of the 101 peak intensity to the 200 peak intensity; Preferably, the iron phosphate is iron phosphate prepared by recycling retired lithium iron phosphate batteries; Preferably, the sodium source in step (1) comprises at least one of trisodium phosphate, sodium carbonate and sodium sulfate; Preferably, in the precursor solution of the phosphate-based cathode material in step (1), the phosphate-based cathode material comprises sodium iron phosphate and / or lithium iron phosphate, and the molar ratio of sodium and / or lithium to Fe is 1.02 to 1.05; Preferably, the solid content of the precursor solution of the phosphate-based cathode material in step (1) is 30% to 40%; Preferably, the solute in the halogen-reduced electron pair solution in step (2) is a sodium-based solute and / or a lithium-based solute; Preferably, the sodium-based solute includes at least one of sodium iodide, sodium bromide and sodium fluoride; Preferably, the solvent in the halogen-reduced electron pair solution in step (2) is water; Preferably, the concentration of the halogen-reduced electron pair solution in step (2) is 2 mol / L to 3 mol / L; Preferably, the organic electrolyte in step (2) comprises a solute and an organic solvent; Preferably, the solute in the organic electrolyte is a sodium salt and / or a lithium salt; Preferably, the sodium salt comprises NaPF 6 and at least one of sodium bisfluorosulfonamide; Preferably, the organic solvent comprises at least one of ethylene carbonate and dimethyl carbonate; Preferably, the concentration of the organic electrolyte is 1 mol / L to 2 mol / L.

5. The method according to claim 3 or 4, It is characterized in that The cathode in the cathode unit includes one of Ti, Ta, Pt, Au and alloys thereof; Preferably, the anode in the anode unit is metallic sodium and / or metallic lithium; Preferably, the certain current density is 500 mA / cm 2 ~800mA / cm 2 ; Preferably, the liquid circulation flow rate is 100 μL / s to 200 μL / s; Preferably, the cycle time is 10h to 15h; Preferably, the voltage used by the electrolysis device is 3.6V to 4.5V.

6. The method according to any one of claims 3 to 5, It is characterized in that The method further comprises grinding the precursor solution of the sodium iron phosphate positive electrode material obtained in step (1), and adding the solid-liquid reaction unit after grinding to a certain particle size; Preferably, the certain particle size is: D50 is 0.5 μm to 0.7 μm, and the particle size concentration C is 2 to 4, wherein the particle size concentration C = (D90-D10) / D50.

7. The method according to any one of claims 3 to 6, It is characterized in that The method further comprises preparing a coating liquid by mixing the powder obtained after drying with a carbon source, and spray drying the coating liquid to obtain a sodium iron phosphate positive electrode material coated with a carbon material; Preferably, the carbon source is an inorganic carbon source; Preferably, the inorganic carbon source comprises at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes, carbon black, graphene and C60; Preferably, the amount of the inorganic carbon source added accounts for 2% to 3% of the mass of the powder; Preferably, the inlet air temperature of the spray drying is 170°C to 200°C; Preferably, the coating liquid is ground before the spray drying.

8. A sodium iron phosphate positive electrode material, It is characterized in that The sodium iron phosphate positive electrode material is prepared by the method described in any one of claims 3 to 7; Preferably, the surface of the sodium iron phosphate positive electrode material is coated with a carbon material.

9. A positive electrode, It is characterized in that The positive electrode includes the sodium iron phosphate positive electrode material according to claim 8.

10. A sodium ion battery, It is characterized in that The sodium ion battery comprises the positive electrode according to claim 9.