Lithium ion battery
By controlling the ID/IG of the negative active material and adding fluoronitrile compounds to the electrolyte, the problem of the negative electrode sheet detaching from the separator due to volume expansion in lithium-ion batteries is solved, the cycle life and mechanical stability of the battery are improved, and a better High puncture resistance and safety performance.
Patent Information
- Application Number
- CN202410779914.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-15
AI Technical Summary
During the charging and discharging process of lithium-ion batteries, the volume expansion of the negative electrode material causes the negative electrode sheet to separate from the separator, shortening the battery cycle life and reducing safety performance.
By controlling the ID/IG of the negative electrode active material in the range of 0.1 to 1.2, and adding fluorinated nitrile compounds to the electrolyte to enhance its adsorption force, the fluorinated nitrile compounds can participate in the formation of the SEI film, repair defects on the surface of the negative electrode material, and improve The interface between the negative electrode and the SEI film is stable and inhibits volume expansion.
Significantly improve the cycle life, mechanical stability and puncture resistance of lithium-ion batteries, extend the service life of the battery and improve safety performance.
Smart Images

Figure BDA0004896786650000021 
Figure BDA0004896786650000071 
Figure BDA0004896786650000231
Abstract
Description
Technical Field
[0001] The invention belongs to the field of lithium ion batteries and relates to a lithium ion battery. Background Art
[0002] Lithium-ion batteries have been widely used in the fields of electric vehicles, aerospace, energy storage power stations, consumer electronics, etc. due to their many advantages such as high energy density, fast charging capability, long life, low self-discharge, and no memory effect.
[0003] Lithium-ion batteries are mainly composed of negative electrode sheets, positive electrode sheets, separators and electrolytes. When charging lithium-ion batteries, lithium ions move from the positive electrode through the electrolyte to the negative electrode, and intercalation occurs. Therefore, the negative electrode active material generally undergoes significant volume expansion as the depth of lithium insertion increases. For example, graphite negative electrode materials generally produce a volume expansion of 10-15%, and silicon-based negative electrode materials can produce a maximum volume expansion of 300%. The volume expansion will cause the negative electrode sheet to separate from the separator, which will in turn shorten the cycle life of the lithium-ion battery and reduce safety performance.
[0004] Therefore, in view of the above defects, it is urgent to develop a new lithium-ion battery to improve the problem of the negative electrode sheet detaching from the diaphragm due to volume expansion, thereby improving the cycle life and safety performance of the battery. Summary of the invention
[0005] In view of the defect that the negative electrode sheet is easily separated from the diaphragm, the present invention provides a lithium ion battery with a long cycle life and high mechanical stability and puncture resistance.
[0006] The present invention provides a lithium ion battery, comprising a negative electrode sheet and an electrolyte, wherein the negative electrode sheet comprises a negative electrode active material, and the electrolyte comprises an additive;
[0007] The ID / IG of the negative electrode active material is 0.1 to 1.2, and the additive includes a fluorinated nitrile compound.
[0008] Furthermore, the lithium-ion battery further comprises a diaphragm; the diaphragm comprises a substrate and a polymer layer disposed on at least one side of the substrate;
[0009] The lithium-ion battery satisfies the following relationship:
[0010] 2.5≤A / (B+H)≤8.5,
[0011] Wherein, A is the mass percentage of the fluorinated nitrile compound in the electrolyte, in %; B is the ID / IG of the negative electrode active material; and H is the thickness of the polymer layer, in μm.
[0012] Furthermore, the mass percentage A of the fluoronitrile compound in the electrolyte is 5-20 wt %, and / or the thickness H of the polymer layer is 0.5-3 μm.
[0013] Furthermore, the polymer layer includes fluorine element; the mass percentage of the fluorine element in the polymer layer is 10-75wt%.
[0014] Furthermore, the ratio of the mass percentage of the fluorine element in the polymer layer to the mass percentage of the fluorinated nitrile compound in the electrolyte is (2-12):1.
[0015] Further, the fluoronitrile compound includes at least one of the compounds represented by Formula 1, Formula 2, Formula 3, Formula 4, Formula 5, Formula 6, Formula 7, Formula 8, and Formula 9,
[0016]
[0017] Further, the fluoronitrile compound includes the compound shown in Formula 2 and the compound shown in Formula 4;
[0018] The mass ratio of the compound represented by Formula 2 to the compound represented by Formula 4 is 1:(1-2).
[0019] Further, the negative electrode active material includes a silicon-carbon composite material and graphite;
[0020] The mass ratio of the silicon-carbon composite material to the graphite is (5-20):100.
[0021] Furthermore, the median particle size Dv50 of the silicon-carbon composite material is 7 to 35 μm, and / or the median particle size Dv50 of the graphite is 5 to 20 μm.
[0022] Furthermore, the electrolyte also includes an organic solvent, an electrolyte salt and a functional additive;
[0023] The mass percentage of the organic solvent in the electrolyte is not higher than 80wt%; and / or the mass percentage of the electrolyte salt in the electrolyte is 12-18wt%; and / or the mass percentage of the functional additive in the electrolyte is 8-20wt%.
[0024] The lithium ion battery of the present invention controls the ID / IG of the negative electrode active material to be 0.1-1.2, and adds a fluoronitrile compound to the electrolyte, thereby enhancing the adsorption of the fluoronitrile compound to hydrogen-containing functional groups (-COOH, -OH, etc.) and doped metal ions (iron, magnesium, etc.) on the surface of the negative electrode, promoting the adsorption of the fluoronitrile compound on the surface of the negative electrode active material, participating in the formation of the SEI film during the first charge and discharge process of the lithium ion battery, and interacting with the defects on the surface of the negative electrode material to repair the defects, thereby improving the interface stability between the negative electrode active material and the SEI film, thereby inhibiting the volume expansion of the negative electrode, improving the problem of the negative electrode sheet detaching from the diaphragm, and further improving the cycle life, mechanical stability and puncture resistance of the battery. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The present invention provides a lithium ion battery, comprising a negative electrode sheet and an electrolyte, wherein the negative electrode sheet comprises a negative electrode active material, and the electrolyte comprises an additive;
[0027] The ID / IG of the negative electrode active material is 0.1-1.2, and the additive comprises a fluorinated nitrile compound.
[0028] The fluorinated nitrile compound in the present invention refers to a nitrile compound in which a hydrogen atom on carbon is replaced by a fluorine atom.
[0029] ID / IG in the present invention refers to the peak intensity ratio of the D peak and the G peak in the Raman spectrum of the negative electrode active material, and the position of the D peak is 1350±10cm -1 , the position of G peak is 1580±10cm -1 Specifically, the ID / IG of the negative electrode active material can be made to be 0.1 to 1.2 by controlling the reaction temperature, holding time, cooling time and other parameters in the preparation process of the negative electrode active material, or by doping the precursor. For example, ID / IG is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2.
[0030] The present invention does not specifically limit the sources of the negative electrode active material and the fluoronitrile compound, and any commercially available product or a product prepared by a conventional preparation method well known to those skilled in the art may be used.
[0031] The lithium-ion battery in the present invention includes a negative electrode sheet and an electrolyte. By making the ID / IG of the negative electrode active material included in the negative electrode sheet between 0.1 and 1.2, and making the electrolyte include a fluoronitrile compound, the problem of the negative electrode sheet detaching from the diaphragm due to the expansion of the negative electrode can be effectively alleviated, thereby significantly improving the cycle performance, mechanical stability and puncture resistance of the lithium-ion battery. Based on this phenomenon, the inventors analyzed lithium-ion batteries and believed that the reason may be: when the ID / IG of the negative electrode active material is in a specific range and the electrolyte includes a fluoronitrile compound, the defects and hydrogen-containing functional groups (-COOH, -OH, etc.) on the surface of the negative electrode active material can interact with the fluoronitrile compound, so that the fluoronitrile compound can be adsorbed on the surface of the negative electrode active material. During the first charge and discharge, the electrolyte undergoes a reduction reaction on the surface of the negative electrode. At this time, the fluoronitrile compound adsorbed on the surface of the negative electrode active material participates in the formation of the SEI film and is embedded in the SEI film structure, wherein the F and -CN groups can form hydrogen bonds with the hydrogen of the organic components in the SEI film, thereby improving the molecular structure stability and interaction force of the SEI components, thereby improving the interface stability between the negative electrode active material and the SEI film, thereby inhibiting the volume expansion of the negative electrode, improving the problem of the negative electrode sheet detaching from the separator due to volume expansion, thereby extending the cycle life of the battery and improving its mechanical stability and puncture resistance.
[0032] Furthermore, the negative electrode active material is doped with metal ions, including Fe 2+ Mg 2+ 、Al 3+ , Ca 2+ 、Zn 2+ At this time, the fluoronitrile compound can also interact with the metal ions doped in the negative electrode active material, so that the fluoronitrile compound can be better adsorbed on the surface of the negative electrode active material and participate in the formation reaction of the SEI interface film.
[0033] In a specific embodiment, the lithium ion battery further comprises a separator; the separator comprises a substrate and a polymer layer disposed on at least one side of the substrate;
[0034] Lithium-ion batteries satisfy the following relationship:
[0035] 2.5≤A / (B+H)≤8.5,
[0036] Wherein, A is the mass percentage of the fluorinated nitrile compound in the electrolyte, in %; B is the ID / IG of the negative electrode active material; and H is the thickness of the polymer layer, in μm.
[0037] The polymer in the polymer layer of the present invention is preferably a fluorine-containing polymer, and the fluorine-containing polymer is preferably at least one of polyvinylidene fluoride, polychlorotrifluoroethylene, polyperfluoroethylene propylene and polytetrafluoroethylene.
[0038] The substrate in the present invention is preferably any one of a polyethylene substrate, a polypropylene substrate, and a polyethylene-polypropylene composite substrate.
[0039] The present invention does not specifically limit the molecular weight of the polymer. For example, the molecular weight is 10,000 to 1,000,000.
[0040] The present invention does not specifically limit the source of the polymer, and any commercially available product or a product prepared by a conventional preparation method well known to those skilled in the art may be used.
[0041] When the mass percentage of the fluoronitrile compound in the electrolyte, the ID / IG of the negative electrode active material and the thickness of the polymer layer satisfy the above relationship, the fluoronitrile compound can better interact with the surface of the negative electrode active material, further improve the interface stability between the negative electrode active material and the SEI film, and inhibit the volume expansion of the negative electrode, thereby being able to comprehensively improve the cycle performance, mechanical stability and puncture resistance of the battery.
[0042] Furthermore, the separator also includes an inorganic material layer; the inorganic material layer is disposed on at least one side of the substrate, and the polymer layer is disposed on the substrate and / or the surface of the inorganic material layer. By disposing the inorganic material layer on the surface of the substrate, the strength and thermal stability of the separator can be further improved, thereby further improving the mechanical stability and puncture resistance of the battery.
[0043] Preferably, the thickness of the separator is 6 to 18 μm. For example, the thickness of the separator is 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm or 18 μm. When the thickness of the separator is within the aforementioned range, it not only helps to improve the mechanical stability and puncture resistance of the battery, but also reduces the loss of energy density; at the same time, it can also ensure high mechanical strength and thermal stability, reduce the internal resistance of the battery, and the stability of the electrochemical performance.
[0044] Preferably, the thickness of the substrate is 5 to 10 μm. For example, the thickness of the substrate is 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm or 10 μm. Within this range, not only the mechanical strength of the separator can be ensured, but also the loss of energy density can be reduced.
[0045] Preferably, the thickness of the inorganic material layer is 0.5 to 2 μm. For example, the thickness of the inorganic material layer is 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm or 2.0 μm. The thickness of the inorganic material layer in the present invention refers to the thickness on one side. Within this range, the diaphragm has higher stability and better electrolyte wettability, which not only helps to form a stable SEI film, but also facilitates the migration of lithium ions.
[0046] The inorganic material in the present invention may include at least one of aluminum hydroxide, aluminum oxide, magnesium hydroxide, silicon oxide, and boehmite.
[0047] In a specific embodiment, the mass percentage A of the fluoronitrile compound in the electrolyte is 5 to 20wt%. For example, A is 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt% or 20wt%. Within this range, the interaction force between the fluoronitrile compound and the surface defects of the negative electrode active material can be further improved, so that the fluoronitrile compound can be better adsorbed on the surface of the negative electrode active material and participate in the formation of the SEI film to a greater extent, further improving the interface stability between the negative electrode and the SEI film, thereby further alleviating the problem of the negative electrode detaching from the separator caused by the expansion of the negative electrode; at the same time, when the content of the fluoronitrile compound in the electrolyte is within the above range, it can better penetrate into the polymer layer, further improve the chemical stability of the separator, thereby further improving the cycle performance, mechanical stability and puncture resistance of the battery.
[0048] In a specific embodiment, the thickness H of the polymer layer is 0.5 to 3 μm. For example, H is 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2.0 μm, 2.1 μm, 2.2 μm, 2.3 μm, 2.4 μm, 2.5 μm, 2.6 μm, 2.7 μm, 2.8 μm, 2.9 μm or 3.0 μm. The thickness of the polymer layer in the present invention refers to the thickness on one side. Within this range, not only can the penetration effect of the fluoronitrile compound in the polymer layer be improved, but also the loss of energy density can be reduced, and the internal resistance can be reduced, so that the battery has higher cycle performance.
[0049] In a specific embodiment, the polymer layer includes fluorine element; the mass percentage of fluorine element in the polymer layer is 10-75wt%. For example, the mass percentage of fluorine element in the polymer layer is 10%wt, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt% or 75wt%, preferably 40-70wt%. When the polymer layer includes fluorine element and the content is in the above range, firstly, it can not only improve the affinity of the electrolyte to the diaphragm, but also avoid the dissolution and deformation of the diaphragm; secondly, it helps the fluorinated nitrile compound to enrich on the surface of the diaphragm to form a protective film, improve the thermal stability of the diaphragm, thereby improving the mechanical stability and puncture resistance of the battery; finally, the diaphragm has good adhesion to the pole piece, and is conducive to the transmission of lithium ions. Therefore, when the mass percentage of fluorine element in the polymer layer is in the above range, the thermal stability of the battery can be further improved.
[0050] The mass percentage of fluorine element in the polymer layer of the present invention can be obtained by subjecting the polymer layer to oxygen (bottle) bomb combustion treatment and then analyzing it by ion chromatography; it can also be obtained by dissolving the polymer layer in a tritiated reagent and performing nuclear magnetic resonance analysis.
[0051] In a specific embodiment, the ratio of the mass percentage of fluorine in the polymer layer to the mass percentage of the fluoronitrile compound in the electrolyte is (2 to 12): 1. For example, the ratio of the mass percentage of fluorine in the polymer layer to the mass percentage of the fluoronitrile compound in the electrolyte is 2: 1, 3: 1, 4: 1, 5: 1:, 6: 1, 7: 1, 8: 1, 9: 1, 10: 1, 11: 1 or 12: 1. Within this range, the fluoronitrile compound has better compatibility with the fluorine-containing membrane, which promotes the enrichment of the fluoronitrile compound in the polymer layer, thereby further improving the penetration effect of the fluoronitrile compound in the polymer layer, further improving the thermal stability and mechanical stability of the membrane, and at the same time, the protective film on the surface of the membrane can maintain a stable shape at high temperature, reduce the thermal shrinkage of the membrane, thereby improving the thermal stability of the entire membrane, and can also enhance the mechanical strength of the membrane, making it more resistant to external physical impact and reducing the risk of damage, so that the battery can have higher mechanical stability and puncture resistance.
[0052] In a specific embodiment, the fluoronitrile compound includes at least one of the compounds shown in Formula 1, Formula 2, Formula 3, Formula 4, Formula 5, Formula 6, Formula 7, Formula 8, and Formula 9,
[0053]
[0054] In a specific embodiment, the fluoronitrile compound includes a compound shown in Formula 2 and a compound shown in Formula 4;
[0055] The mass ratio of the compound represented by Formula 2 to the compound represented by Formula 4 is 1:(1-2). When the fluoronitrile compound is the aforementioned combination and the content is within the aforementioned range, the adsorption of the fluoronitrile compound on the negative electrode active material can be further enhanced, so that the fluoronitrile compound can participate in the formation reaction of the SEI film to a greater extent, thereby further improving the interface stability between the negative electrode active material and the SEI film, so that the battery has a longer cycle life and higher mechanical stability and puncture resistance; at the same time, the fluoronitrile compound can complex the metal ions in the positive electrode active material, thereby helping to improve the positive electrode stability.
[0056] In a specific embodiment, the negative electrode active material includes a silicon-carbon composite material and graphite; the mass ratio of the silicon-carbon composite material to the graphite is (5-20):100. For example, the mass ratio of the silicon-carbon composite material to the graphite is 5:100, 8:100, 11:100, 14:100, 17:100 or 20:100. At this time, not only a higher energy density can be achieved, but also it helps to make the graphite particles and the silicon-carbon composite material particles better contact during the preparation and coating of the negative electrode active slurry, alleviate the volume expansion problem of the silicon-carbon composite material during the charge and discharge process, and further improve the separation of the negative electrode sheet from the separator due to the volume change of the negative electrode active material.
[0057] In a specific embodiment, the median particle size Dv50 of the silicon-carbon composite material is 7 to 35 μm, and / or the median particle size Dv50 of graphite is 5 to 20 μm. For example, the median particle size Dv50 of the silicon-carbon composite material is 7 μm, 12 μm, 15 μm, 18 μm, 21 μm, 24 μm, 27 μm, 30 μm or 35 μm; the median particle size Dv50 of graphite is 5 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm or 20 μm. Preferably, the median particle size Dv50 of the silicon-carbon composite material is 12 to 30 μm, and / or the median particle size Dv50 of graphite is 10 to 15 μm. Wherein, Dv50 represents the particle size of 50% volume accumulation. When the Dv50 of the silicon-carbon composite material and graphite is within the aforementioned range, it is beneficial to the accumulation of negative electrode active materials, reducing the gaps formed between the negative electrode active material particles, and reducing the occurrence of side reactions between the electrolyte and the negative electrode material during the charge and discharge process, preventing excessive formation of SEI, thereby reducing the irreversible lithium loss of the battery; at the same time, it can also reduce the breakage of the electrode material and improve the stability of the electrode structure, so that the battery has better cycle performance.
[0058] In a specific embodiment, the electrolyte further includes an organic solvent; the mass percentage of the organic solvent in the electrolyte is not higher than 80wt%. When the proportion of the organic solvent in the electrolyte is within the above range, the kinetic performance of the electrolyte is good, and the cycle stability and rate performance of the battery can be further improved.
[0059] The organic solvent in the present invention includes carbonate and / or carboxylate; wherein the carboxylate includes at least one of substituted or unsubstituted propyl acetate, substituted or unsubstituted n-butyl acetate, substituted or unsubstituted isobutyl acetate, substituted or unsubstituted n-pentyl acetate, substituted or unsubstituted isopentyl acetate, substituted or unsubstituted methyl propionate, substituted or unsubstituted propyl propionate, substituted or unsubstituted ethyl propionate, and substituted or unsubstituted methyl butyrate; the carbonate includes substituted or unsubstituted ethylene carbonate, substituted or unsubstituted propylene carbonate, substituted or unsubstituted dimethyl carbonate, substituted or unsubstituted diethyl carbonate, and substituted or unsubstituted ethyl methyl carbonate. When the organic solvent is a mixture of the aforementioned multiple specific compounds, the present invention does not place too many restrictions on the ratio between the specific compounds.
[0060] In a specific embodiment, the electrolyte further includes electrolyte salt; the mass percentage of the electrolyte salt in the electrolyte is 12-18wt%. For example, the mass percentage of the electrolyte salt in the electrolyte is 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt% or 18wt%. When the content of the electrolyte salt in the electrolyte is within the above range, sufficient lithium ions can be provided for the battery to work, avoiding the problem that the lithium ions cannot be replenished in time due to the consumption of lithium ions during the cycle due to too little lithium ion content, and the problem that the electrolyte viscosity is too high due to too much lithium ion content, and the rate performance is reduced, thereby further improving the battery performance.
[0061] The electrolyte salt in the present invention includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, and lithium tetrafluoroborate.
[0062] In a specific embodiment, the electrolyte further includes a functional additive; the mass percentage of the functional additive in the electrolyte is 8 to 20 wt%;
[0063] The functional additives include at least one of nitrile additives, cyclic carbonate additives, and cyclic sultone additives;
[0064] The nitrile additive includes at least one of ethylene glycol bis(propionitrile) ether, adiponitrile, succinonitrile, 1,3,6-hexanetrinitrile, glutaronitrile, trans-butenedinitrile, and trans-hexenedinitrile;
[0065] The cyclic carbonate additive includes at least one of fluoroethylene carbonate, difluoroethylene carbonate, vinylene carbonate, and vinylethylene carbonate;
[0066] The cyclic sultone additive includes at least one of 1,3-propane sultone, 1,3-propylene sultone, 2,4-butane sultone, 1,4-butane sultone and methylene methane disulfonate.
[0067] For example, the mass percentage of the functional additive in the electrolyte is 8wt%, 10wt%, 12wt%, 14wt%, 16wt%, 18wt% or 20wt%. When the content of the functional additive is within the above range, a good interface film can be formed on the electrode surface to improve battery stability and rate performance.
[0068] In a specific embodiment, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer arranged on at least one side of the negative electrode current collector; the negative electrode active material layer includes, by mass percentage: 80-99.5wt% of negative electrode active material, 0.25-10wt% of conductive agent, and 0.25-10wt% of binder.
[0069] The conductive agent in the present invention is preferably at least one of conductive carbon black, acetylene black, Ketjen black, graphene, conductive carbon fiber, carbon nanotubes, and mesophase carbon microspheres.
[0070] The binder in the present invention is preferably at least one of polyacrylic acid, sodium polyacrylate, polyacrylamide, sodium alginate, polyvinyl alcohol, sodium carboxymethyl cellulose, styrene-butadiene latex, polytetrafluoroethylene, polyethylene oxide, and polyvinylidene fluoride.
[0071] In the present invention, the negative electrode current collector is preferably any one of copper foil, carbon-coated copper foil, nickel current collector, stainless steel current collector and carbon current collector.
[0072] In a specific embodiment, the lithium-ion battery further comprises a positive electrode sheet; the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one side surface of the positive electrode current collector; the positive electrode active material layer comprises a positive electrode active material.
[0073] The positive electrode active material in the present invention is preferably a doped and / or coated modified lithium cobalt oxide material, that is, the lithium cobalt oxide material is modified by element doping and / or coating to improve the structural stability of the positive electrode material. Preferably, the chemical formula of the positive electrode active material of the present invention is LiCo 1-d-e M d N eO2, wherein 0.01≤d≤0.1, 0≤e≤0.05, M includes at least one of Mn and Al, and N includes at least one of Mg, Zr, Ni, Y, LD, Sr, W, Sc, B, W, Si, Ti, Zr, Sr, Sn, Tb, Nb, Sb, Se, Ce, and Te.
[0074] The positive electrode current collector of the present invention can be selected from any one of an aluminum current collector, a nickel current collector, a stainless steel current collector, and a carbon current collector.
[0075] The lithium-ion battery of the present invention is described in detail below through specific embodiments.
[0076] Example 1
[0077] (1) Preparation of positive electrode sheet: Lithium cobalt oxide, binder polyvinylidene fluoride (PVDF 500), and conductive carbon material (Super P) were mixed with N-methylpyrrolidone (NMP) in a mass ratio of 97:2:3, and continuously stirred in a stirrer to form a uniform positive electrode active slurry; then, the positive electrode active slurry was coated on an aluminum foil with a thickness of 10 μm, placed in a vacuum oven at 120°C and dried for 6 h, and then rolled and cut to obtain the required compaction density of 4.2 g / cm 3 The positive electrode;
[0078] (2) Preparation of negative electrode sheet: 97.5wt% of negative electrode active material (including 87.5wt% of graphite and 10wt% of silicon-carbon composite material), 1wt% of conductive carbon black (Super P), 0.3wt% of sodium carboxymethyl cellulose (CMC) and 1.2wt% of styrene-butadiene rubber (SBR) were mixed with water and continuously stirred in a stirrer to form a uniform and flowing negative electrode active slurry, wherein the Dv50 of graphite was 12.4μm, the Dv50 of silicon-carbon composite material was 22.5μm, and the ID / IG of negative electrode active material was 0.8; then, the negative electrode active slurry was coated on the surface of copper foil with a thickness of 10μm, sent to a vacuum oven at 120℃ for drying for 6h, and then rolled and cut to obtain a compacted density of 0.95g / cm 3 The negative electrode;
[0079] (3) Preparation of electrolyte: In a glove box filled with argon (water <1 ppm, oxygen <1 ppm), ethylene carbonate, propylene carbonate, ethyl propionate and propyl propionate were mixed in a mass ratio of 20:10:50:20 to form a uniform organic solvent, 14.3 wt % of LiPF6 was slowly added to the organic solvent, and then 6.0 wt % of the compound represented by formula 1, 7 wt % of fluoroethylene carbonate, 3 wt % of 1,3-propane sultone, and 3.5 wt % of 1,3,6-hexanetrinitrile were added, and the mixture was stirred evenly to obtain the electrolyte of this embodiment;
[0080] (4) Preparation of diaphragm: After coating a 1 μm thick aluminum hydroxide ceramic layer on one side of an 8 μm polyethylene substrate, a 1.2 μm thick polyvinylidene fluoride polymer layer is coated on the substrate surface and the aluminum hydroxide ceramic layer surface respectively. Ion chromatography analysis shows that the fluorine content in the polymer layer is 56 wt %, thereby obtaining the diaphragm of this embodiment;
[0081] (5) Preparation of lithium-ion battery: The positive electrode sheet, separator and negative electrode sheet prepared above are wound to prepare a bare battery cell; the bare battery cell is then placed in an aluminum-plastic film package, and the prepared electrolyte is injected into the dried bare battery cell. After vacuum packaging, room temperature standing, high-temperature formation and other processes, the lithium-ion battery of this embodiment is obtained.
[0082] Example 2
[0083] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the compound represented by Formula 2 is used instead of the compound represented by Formula 1.
[0084] Example 3
[0085] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the compound shown in Formula 3 is used instead of the compound shown in Formula 1.
[0086] Example 4
[0087] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the compound represented by Formula 4 is used instead of the compound represented by Formula 1.
[0088] Example 5
[0089] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the compound represented by Formula 5 is used instead of the compound represented by Formula 1.
[0090] Example 6
[0091] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (6), the compound shown in Formula 6 is used instead of the compound shown in Formula 1.
[0092] Example 7
[0093] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the compound represented by Formula 7 is used instead of the compound represented by Formula 1.
[0094] Example 8
[0095] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the compound shown in Formula 8 is used instead of the compound shown in Formula 1.
[0096] Example 9
[0097] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the compound represented by Formula 9 is used instead of the compound represented by Formula 1.
[0098] Example 10
[0099] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the compound represented by Formula 2 and the compound represented by Formula 4 are used to replace the compound represented by Formula 1, and the mass ratio of the compound represented by Formula 2 to the compound represented by Formula 4 is 1:1.
[0100] Embodiment 11
[0101] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the mass percentage of the compound represented by Formula 1 in the electrolyte is adjusted to 10 wt %, and the mass percentage of the organic solvent becomes 62.2 wt %.
[0102] Example 12
[0103] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the mass percentage of the compound represented by Formula 1 in the electrolyte is adjusted to 15 wt %, and the mass percentage of the organic solvent becomes 57.2 wt %.
[0104] Example 13
[0105] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the mass percentage of the compound represented by Formula 1 in the electrolyte is adjusted to 17 wt %, and the mass percentage of the organic solvent becomes 55.2 wt %.
[0106] Embodiment 14
[0107] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (2), the ID / IG of the negative electrode active material is adjusted to 0.1. Specifically, the graphite raw material is sent into an inert gas atmosphere and sintered at 2000° C. for 6 hours to obtain the result.
[0108] Embodiment 15
[0109] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (2), the ID / IG of the negative electrode active material is adjusted to 0.5. Specifically, the graphite raw material is sent into an inert gas atmosphere and sintered at 1600° C. for 6 hours.
[0110] Example 16
[0111] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 1, except that in step (2), the ID / IG of the negative electrode active material is adjusted to 1.2. Specifically, the graphite raw material is introduced into an ammonia gas atmosphere and sintered at 300° C. for 6 hours.
[0112] Embodiment 17
[0113] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 11, except that in step (4), the thickness of the polymer layer is adjusted to 0.5 μm.
[0114] Embodiment 18
[0115] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 11, except that in step (4), the thickness of the polymer layer is adjusted to 2.0 μm.
[0116] Embodiment 19
[0117] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 11, except that in step (4), the thickness of the polymer layer is adjusted to 3.0 μm.
[0118] Embodiment 20
[0119] The preparation method of the lithium ion battery in this embodiment is basically the same as that in embodiment 11, except that in step (2), the ID / IG of the negative electrode active material is adjusted to 0.1. Specifically, the graphite raw material is introduced into an inert gas atmosphere and sintered at 2000° C. for 6 h to obtain the graphite raw material;
[0120] In step (3), the mass percentage of the compound represented by formula 1 in the electrolyte is adjusted to 5 wt %, and the mass percentage of the organic solvent becomes 67.2 wt %;
[0121] In step (4), the thickness of the polymer layer was adjusted to 0.5 μm.
[0122] Embodiment 21
[0123] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 13, except that in step (3), the mass percentage of the compound represented by Formula 1 in the electrolyte is adjusted to 20 wt %, and the mass percentage of the organic solvent becomes 52.2 wt %.
[0124] Embodiment 22
[0125] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 18, except that in step (3), the mass percentage of the compound represented by Formula 1 in the electrolyte is adjusted to 22 wt %, and the mass percentage of the organic solvent becomes 50.2 wt %.
[0126] Embodiment 23
[0127] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 18, except that, in (2), the ID / IG of the negative electrode active material is adjusted to 1.3. Specifically, the graphite raw material is sent into an ammonia gas atmosphere and sintered at 300°C for 12 hours.
[0128] Embodiment 24
[0129] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 18, except that in step (4), the thickness of the polymer layer is adjusted to 3.2 μm.
[0130] Embodiment 25
[0131] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 18, except that, in step (2), the ID / IG of the negative electrode active material is adjusted to 1.4. Specifically, the graphite raw material is introduced into an ammonia gas atmosphere and sintered at 500° C. for 12 h to obtain the result;
[0132] In step (3), the mass percentage of the compound represented by formula 1 in the electrolyte is adjusted to 22 wt %, and the mass percentage of the organic solvent becomes 50.2 wt %.
[0133] Embodiment 26
[0134] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 18, except that, in step (2), the ID / IG of the negative electrode active material is adjusted to 1.4. Specifically, the graphite raw material is introduced into an ammonia gas atmosphere and sintered at 500° C. for 12 h to obtain the result;
[0135] In step (4), the thickness of the polymer layer was adjusted to 3.5 μm.
[0136] Embodiment 27
[0137] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 18, except that in step (3), the mass percentage of the compound represented by Formula 1 in the electrolyte is adjusted to 22wt%, and the mass percentage of the organic solvent becomes 50.2wt%;
[0138] In step (4), the thickness of the polymer layer was adjusted to 3.5 μm.
[0139] Embodiment 28
[0140] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 18, except that, in step (2), the ID / IG of the negative electrode active material is adjusted to 1.4. Specifically, the graphite raw material is introduced into an ammonia gas atmosphere and sintered at 500° C. for 12 h to obtain the result;
[0141] In step (3), the mass percentage of the compound represented by formula 1 in the electrolyte is adjusted to 22 wt %, and the mass percentage of the organic solvent becomes 50.2 wt %;
[0142] In step (4), the thickness of the polymer layer was adjusted to 3.5 μm.
[0143] Embodiment 29
[0144] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 18, except that, in step (2), the ID / IG of the negative electrode active material is adjusted to 1.4. Specifically, the graphite raw material is introduced into an ammonia gas atmosphere and sintered at 500° C. for 12 h to obtain the result;
[0145] In step (3), the mass percentage of the compound represented by formula 1 in the electrolyte is adjusted to 4 wt %, and the mass percentage of the organic solvent becomes 68.2 wt %;
[0146] In step (4), the thickness of the polymer layer was adjusted to 3.5 μm.
[0147] Embodiment 30
[0148] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 20, except that, in step (4), the content of fluorine element in the polymer layer is adjusted to 10wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polymethyl methacrylate (PMMA) are mixed to obtain a mixed material, the mass percentage of PMMA in the mixed material is 90wt%, and the mixed material is used as the polymer layer.
[0149] Embodiment 31
[0150] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 20, except that, in step (4), the content of fluorine element in the polymer layer is adjusted to 20wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polymethyl methacrylate (PMMA) are mixed to obtain a mixed material, the mass percentage of PMMA in the mixed material is 85wt%, and the mixed material is used as the polymer layer.
[0151] Embodiment 32
[0152] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 20, except that, in step (4), the content of fluorine element in the polymer layer is adjusted to 30wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polymethyl methacrylate (PMMA) are mixed to obtain a mixed material, the mass percentage of PMMA in the mixed material is 80wt%, and the mixed material is used as the polymer layer.
[0153] Embodiment 33
[0154] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that, in step (4), the content of fluorine element in the polymer layer is adjusted to 40wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polymethyl methacrylate (PMMA) are mixed to obtain a mixed material, the mass percentage of PMMA in the mixed material is 20wt%, and the mixed material is used as the polymer layer.
[0155] Embodiment 34
[0156] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that, in step (4), the content of fluorine element in the polymer layer is adjusted to 50wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polymethyl methacrylate (PMMA) are mixed to obtain a mixed material, in which the mass percentage of PMMA to PVDF is 10wt%, and the mixed material is used as the polymer layer.
[0157] Embodiment 35
[0158] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that, in step (4), the content of fluorine element in the polymer layer is adjusted to 60wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polytetrafluoroethylene (PTFE) are mixed to obtain a mixed material, the mass percentage of PTFE in the mixed material is 10wt%, and the mixed material is used as the polymer layer.
[0159] Embodiment 36
[0160] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that, in step (4), the content of fluorine element in the polymer layer is adjusted to 70wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polytetrafluoroethylene (PTFE) are mixed to obtain a mixed material, the mass percentage of PTFE in the mixed material is 30wt%, and the mixed material is used as the polymer layer.
[0161] Embodiment 37
[0162] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 13, except that, in step (4), the content of fluorine element in the polymer layer is adjusted to 75wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polytetrafluoroethylene (PTFE) are mixed to obtain a mixed material, the mass percentage of PTFE in the mixed material is 95wt%, and the mixed material is used as the polymer layer.
[0163] Embodiment 38
[0164] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 13, except that, in step (4), the content of fluorine element in the polymer layer is adjusted to 40wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polymethyl methacrylate (PMMA) are mixed to obtain a mixed material, the mass percentage of PMMA in the mixed material is 20wt%, and the mixed material is used as the polymer layer.
[0165] Embodiment 39
[0166] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Example 33, except that in step (3), the mass percentage of the compound represented by Formula 1 in the electrolyte is adjusted to 9.5wt%, and the mass percentage of the organic solvent in the electrolyte is changed to 62.7wt%.
[0167] Embodiment 40
[0168] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Example 33, except that in step (4), the content of fluorine element in the polymer layer is adjusted to 37wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polymethyl methacrylate (PMMA) are mixed to obtain a mixed material, the mass percentage of PMMA in the mixed material is 50wt%, and the mixed material is used as the polymer layer.
[0169] Embodiment 41
[0170] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 20, except that, in step (3), the mass percentage of the compound represented by Formula 1 in the electrolyte is adjusted to 4wt%, and the mass percentage of the organic solvent in the electrolyte is changed to 68.2wt%;
[0171] In step (4), the content of fluorine element in the polymer layer is adjusted to 40wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polymethyl methacrylate (PMMA) are mixed to obtain a mixture, in which the mass percentage of PMMA in the mixture is 20wt%, and the mixture is used as the polymer layer.
[0172] Embodiment 42
[0173] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Example 36, except that in step (3), the mass percentage of the compound represented by Formula 1 in the electrolyte is adjusted to 5wt%, and the mass percentage of the organic solvent in the electrolyte is changed to 67.2wt%.
[0174] Embodiment 43
[0175] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 20, except that, in step (3), the mass percentage of the compound represented by Formula 1 in the electrolyte is adjusted to 4wt%, and the mass percentage of the organic solvent in the electrolyte is changed to 68.2wt%;
[0176] In step (4), the content of fluorine element in the polymer layer is adjusted to 37wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polymethyl methacrylate (PMMA) are mixed to obtain a mixture, in which the mass percentage of PMMA in the mixture is 50wt%, and the mixture is used as the polymer layer.
[0177] Embodiment 44
[0178] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Example 22, except that in step (4), the content of fluorine element in the polymer layer is adjusted to 37wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polymethyl methacrylate (PMMA) are mixed to obtain a mixed material, the mass percentage of PMMA in the mixed material is 50wt%, and the mixed material is used as the polymer layer.
[0179] Embodiment 45
[0180] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 20, except that, in step (4), the content of fluorine element in the polymer layer is adjusted to 7wt%. Specifically, polyvinylidene fluoride (PVDF 500) and polymethyl methacrylate (PMMA) are mixed to obtain a mixed material, the percentage of PMMA in the mixed material is 90wt%, and the mixed material is used as the polymer layer.
[0181] Embodiment 46
[0182] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 13, except that in step (4), the content of fluorine in the polymer layer is adjusted to 78 wt %. Specifically, polytetrafluoroethylene (PTFE) is used as the polymer layer.
[0183] Embodiment 47
[0184] The preparation method of the lithium-ion battery in the embodiment is basically the same as that in embodiment 1, except that the Dv50 of the silicon-carbon composite material is adjusted to 7.4 μm.
[0185] Embodiment 48
[0186] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 1, except that the Dv50 of the silicon-carbon composite material is adjusted to 12.2 μm.
[0187] Embodiment 49
[0188] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 1, except that the Dv50 of the silicon-carbon composite material is adjusted to 17.1 μm.
[0189] Embodiment 50
[0190] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 1, except that the Dv50 of the silicon-carbon composite material is adjusted to 26.4 μm.
[0191] Embodiment 51
[0192] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 1, except that the Dv50 of the silicon-carbon composite material is adjusted to 29.8 μm.
[0193] Embodiment 52
[0194] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 1, except that the Dv50 of the silicon-carbon composite material is adjusted to 34.5 μm.
[0195] Embodiment 53
[0196] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that the graphite Dv50 is adjusted to 5.6 μm.
[0197] Embodiment 54
[0198] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that the graphite Dv50 is adjusted to 10.4 μm.
[0199] Embodiment 55
[0200] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that the graphite Dv50 is adjusted to 14.6 μm.
[0201] Embodiment 56
[0202] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that the graphite Dv50 is adjusted to 19.8 μm.
[0203] Embodiment 57
[0204] The preparation method of the lithium ion battery in this embodiment is basically the same as that in Embodiment 1, except that the graphite Dv50 is adjusted to 9.1 μm.
[0205] Embodiment 58
[0206] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 1, except that the Dv50 of the silicon-carbon composite material is adjusted to 32.2 μm.
[0207] Embodiment 59
[0208] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 1, except that the Dv50 of graphite is adjusted to 17.2 μm and the Dv50 of the silicon-carbon composite material is adjusted to 10.6 μm.
[0209] Embodiment 60
[0210] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 1, except that the Dv50 of the silicon-carbon composite material is adjusted to 37.8 μm.
[0211] Embodiment 61
[0212] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 1, except that the graphite Dv50 is adjusted to 3.8 μm.
[0213] Embodiment 62
[0214] The preparation method of the lithium-ion battery in this embodiment is basically the same as that in Embodiment 1, except that the Dv50 of graphite is adjusted to 22.4 μm and the Dv50 of the silicon-carbon composite material is adjusted to 5.4 μm.
[0215] Comparative Example 1
[0216] The preparation method of the lithium ion battery in this comparative example is basically the same as that in Example 1, except that in step (2), the ID / IG of the negative electrode active material is adjusted to 0.08.
[0217] Comparative Example 2
[0218] The preparation method of the lithium ion battery in this comparative example is basically the same as that in Example 1, except that in step (2), the ID / IG of the negative electrode active material is adjusted to 1.24.
[0219] Comparative Example 3
[0220] The preparation method of the lithium ion battery in this comparative example is basically the same as that in Example 1, except that in step (3), no fluorinated nitrile compound is added to the electrolyte, and the mass percentage of the organic solvent becomes 72.2 wt %.
[0221] Comparative Example 4
[0222] The preparation method of the lithium ion battery in this comparative example is basically the same as that in Example 1, except that in step (3), the fluoronitrile compound is replaced by succinonitrile.
[0223] Comparative Example 5
[0224] The preparation method of the lithium ion battery in this comparative example is basically the same as that in Example 1, except that in step (3), the fluorinated nitrile compound is replaced by 1,3,6-hexanetrinitrile.
[0225] Test example
[0226] 1. The peeling force between the negative electrode sheet and the separator, the cycle performance, the mechanical stability and the puncture resistance of the lithium-ion batteries in the above-mentioned Examples 1 to 29 and Comparative Examples 1 to 5 were tested.
[0227] (1) Peeling force test between negative electrode sheet and separator
[0228] The lithium-ion battery prepared in the above examples and comparative examples was placed in an ambient temperature of (25±2)℃, and charged to 4.48V at a constant current density of 1C, and discharged to 3.0V at a constant current density of 0.5C; after 20 cycles of charge and discharge, the separator and negative electrode sheet in the battery were disassembled and cut into samples of a specified size of 2 (length) × 2 (width) mm. The negative electrode sheet bonded with the adhesive layer was installed on the peeling force tester, the free end of the sample was folded at a certain angle (usually 180°), and the adhesive surface was peeled off by about 50mm for testing, and the peeling force N was obtained.
[0229] (2) Cyclic performance test
[0230] The lithium ion batteries prepared in the above embodiments and comparative examples are placed in an ambient temperature of (25±2)°C, charged to 4.48V at a constant current density of 1C, discharged to 3.0V at a constant current density of 0.5C, and the discharge capacity is recorded as the initial capacity Q0; the charge and discharge cycle is repeated for 500 cycles, and the discharge capacity after the cycle is recorded as Q1. The cycle capacity retention rate is the ratio of Q1 to Q0.
[0231] (3) Drop test
[0232] The lithium-ion batteries prepared in the above embodiments and comparative examples were dropped from a height of 1 m onto a concrete floor, with 6 faces and 4 corners dropped once each. During the test, the battery was dropped in a directional manner with a clamping arm. When the battery did not catch fire, explode, or emit smoke, and the voltage was not less than 90% of that before the test, it passed 1.
[0233] (4) Acupuncture test
[0234] The lithium-ion batteries prepared in the above embodiments and comparative examples are pierced with a high-temperature resistant steel needle with a diameter of ф8 mm at a speed of (25±5) mm / s from a direction perpendicular to the battery plate. The puncture position is preferably close to the geometric center of the punctured surface (the steel needle stays in the battery), and the battery status is recorded. If the battery does not catch fire or explode, it means it has passed.
[0235] The test results are shown in Table 1.
[0236] Table 1
[0237]
[0238]
[0239]
[0240] From Table 1, we can see that:
[0241] The lithium ion batteries of Examples 1 to 29 have higher mechanical stability, puncture resistance and cycle performance than those of Comparative Examples 1 to 5. Specifically, the maximum peeling force of the diaphragm in the examples is 13.97 mN / cm, the cycle capacity retention rate is up to 86.75%, and the pass rates of the drop test and the puncture test are high; while the maximum peeling force of the diaphragm in the comparative example is only 4.52 mN / cm, the cycle capacity retention rate is only 65.86%, and the pass rates of the drop test and the puncture test are low. Therefore, the lithium ion battery of the present invention has a longer cycle life and higher mechanical stability and puncture resistance.
[0242] At the same time, it can be seen from Examples 21 to 29 that the mass content of the fluoronitrile compound, the negative electrode active material ID / IG and the thickness of the polymer layer in the lithium-ion battery have a great influence on the mechanical stability, puncture resistance and cycle life of the lithium-ion battery, and the relationship between the mass content of the fluoronitrile compound, the negative electrode active material ID / IG and the thickness of the polymer layer also has a certain influence on the lithium-ion battery. When the above-mentioned set range is not met, the mechanical stability, puncture resistance and cycle performance of the lithium-ion battery will be reduced to a certain extent.
[0243] 2. Testing the tensile force of the diaphragms in the above-mentioned Examples 1, 13, 20, 22, 30 to 46 comprises the following steps:
[0244] The lithium-ion batteries prepared in the above examples and comparative examples were charged at 1.2 MPa and 0.2C to a cut-off voltage of 4.48 V at 25°C, 60°C, and 80°C, respectively. The formed lithium-ion batteries were disassembled to obtain the diaphragms, which were cut into samples of a specified size of 5 (length) cm×15 (width) mm. The diaphragms were fixedly mounted on the diaphragm tensile test device, and the test speed was set to 100 mm / min until the diaphragm broke and the tensile force N was obtained. The results are shown in Table 2.
[0245] Table 2
[0246]
[0247]
[0248] From Table 2, we can see that:
[0249] The mass content of fluorine in the polymer layer, the mass content of fluorinated nitrile compounds, and the mass content of fluorine in the polymer layer / mass content of fluorinated nitrile compounds in Examples 1, 13, 20, 22, 30-39 all meet the aforementioned settings, and therefore have a higher tensile force for the diaphragm; while Examples 40-46 do not meet the aforementioned settings, and have a lower tensile force for the diaphragm than the aforementioned examples. It can be seen that when the mass content of fluorine in the polymer layer, the mass content of fluorinated nitrile compounds, and the mass content of fluorine in the polymer layer / mass content of fluorinated nitrile compounds meet the aforementioned settings, the stability and high temperature performance of the diaphragm can be effectively improved, so that the battery has higher mechanical stability and puncture resistance.
[0250] 3. The capacity retention rate of the lithium-ion batteries in the above-mentioned Examples 1 and 47 to 62 was tested using the same test method as described above. The test results are shown in Table 3.
[0251] Table 3
[0252]
[0253]
[0254] From Table 3, we can see that:
[0255] The median particle size Dv50 of the graphite in Example 1, Example 47-Example 59 is between 5 and 20 μm, and the median particle size Dv50 of the silicon-carbon composite material is between 7 and 35 μm, and the corresponding cycle capacity retention rate of the lithium-ion battery is relatively high, up to 86.75%; while the median particle size of the graphite and silicon-carbon composite material in Example 60-Example 62 is not within the specified range, and accordingly, the cycle capacity retention rate of the battery decreases. It can be seen that when the median particle size of the graphite and silicon-carbon composite material is within the aforementioned specified range, the cycle capacity retention rate of the battery can be effectively improved.
[0256] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A lithium-ion battery, It is characterized in that The invention comprises a negative electrode sheet and an electrolyte, wherein the negative electrode sheet comprises a negative electrode active material, and the electrolyte comprises an additive; The ID / IG of the negative electrode active material is 0.1 to 1.2, and the additive includes a fluorinated nitrile compound.
2. The lithium ion battery according to claim 1, It is characterized in that The lithium-ion battery further comprises a diaphragm; the diaphragm comprises a substrate and a polymer layer disposed on at least one side of the substrate; The lithium-ion battery satisfies the following relationship: 2.5≤A / (B+H)≤8.5, Wherein, A is the mass percentage of the fluorinated nitrile compound in the electrolyte, in %; B is the ID / IG of the negative electrode active material; and H is the thickness of the polymer layer, in μm.
3. The lithium ion battery according to claim 2, It is characterized in that The mass percentage A of the fluoronitrile compound in the electrolyte is 5-20wt%, and / or the thickness H of the polymer layer is 0.5-3μm.
4. The lithium ion battery according to claim 2 or 3, It is characterized in that The polymer layer includes fluorine element; the mass percentage of the fluorine element in the polymer layer is 10-75wt%.
5. The lithium ion battery according to any one of claims 2 to 4, It is characterized in that The ratio of the mass percentage of the fluorine element in the polymer layer to the mass percentage of the fluorinated nitrile compound in the electrolyte is (2-12):
1.
6. The lithium ion battery according to any one of claims 1 to 5, It is characterized in that The fluoronitrile compound includes at least one of the compounds shown in Formula 1, Formula 2, Formula 3, Formula 4, Formula 5, Formula 6, Formula 7, Formula 8, and Formula 9, 7. The lithium ion battery according to claim 6, It is characterized in that The fluoronitrile compound includes a compound represented by Formula 2 and a compound represented by Formula 4; The mass ratio of the compound represented by Formula 2 to the compound represented by Formula 4 is 1:(1-2).
8. The lithium ion battery according to any one of claims 1 to 7, It is characterized in that The negative electrode active material includes a silicon-carbon composite material and graphite; The mass ratio of the silicon-carbon composite material to the graphite is (5-20):
100.
9. The lithium ion battery according to claim 8, It is characterized in that The median particle size Dv50 of the silicon-carbon composite material is 7 to 35 μm, and / or the median particle size Dv50 of the graphite is 5 to 20 μm.
10. The lithium ion battery according to any one of claims 1 to 9, It is characterized in that The electrolyte also includes an organic solvent, an electrolyte salt and a functional additive; The mass percentage of the organic solvent in the electrolyte is not higher than 80wt%; and / or the mass percentage of the electrolyte salt in the electrolyte is 12-18wt%; and / or the mass percentage of the functional additive in the electrolyte is 8-20wt%.