Flame-retardant composite diaphragm, preparation method thereof and lithium ion battery

By applying a flame-retardant coating of decabromodiphenylethane and antimony trioxide on the lithium-ion battery separator, the problem of thermal runaway and combustion of lithium-ion batteries under abnormal conditions is solved, and the safety performance and electrochemistry of the battery are improved. performance.

CN118783033AInactive Publication Date: 2024-10-15NIO BATTERY TECH (ANHUI) CO LTD

Patent Information

Application Number
CN202310361497.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Lithium-ion batteries are prone to thermal runaway and combustion under abnormal conditions such as overcharge, high temperature, or internal short circuit. Existing separator materials cannot effectively prevent battery core combustion, leading to the risk of electric vehicle explosions or fire accidents.

Method used

A flame-retardant composite separator is used, including a base film and a flame-retardant coating on the surface of the base film. The flame-retardant coating is composed of decabromodiphenylethane and antimony trioxide as the main components, supplemented by adhesives and additives. , applied to the separator through micro-gravure roller coating or spraying technology to form a thickness of 1 to 20 μm.

Benefits of technology

When the battery core catches fire, the SbBr3 produced by the decomposition of the flame retardant blocks oxygen, and the bromine radicals capture the burning free radicals, effectively terminating the combustion reaction, improving the safety performance of the lithium-ion battery, and maintaining appropriate thermal shrinkage and electrochemical performance. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118783033A_ABST
    Figure CN118783033A_ABST
Patent Text Reader

Abstract

The invention relates to a flame-retardant composite diaphragm, a preparation method thereof and a lithium ion battery. The flame-retardant composite membrane comprises a base membrane and a flame-retardant coating arranged on at least one surface of the base membrane, wherein the flame-retardant coating layer comprises a flame retardant, and the flame retardant comprises decabromodiphenyl ethane and antimony trioxide; according to the flame-retardant composite diaphragm provided by the invention, when a battery cell is on fire, the flame retardant coating is decomposed at a high temperature to generate SbBr3, oxygen can be isolated, and meanwhile, the bromine free radicals capture H and HO free radicals generated by combustion, so that the free radical chain reaction of combustion is relieved or terminated, and the safety performance of the ternary battery is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of lithium battery materials, and in particular to a flame retardant composite diaphragm, a method for preparing the flame retardant composite diaphragm, and a lithium ion battery comprising the flame retardant composite diaphragm. Background Art

[0002] With the development of energy technology, new energy electric vehicles have become more and more popular and recognized by consumers. Lithium-ion batteries are widely used in electric vehicle power sources due to their high specific energy density and stable cycle performance. The performance of lithium-ion batteries directly affects the cruising range and safety performance of electric vehicles. With the continuous improvement of cruising range, safety performance will be affected to some extent. When the lithium-ion battery cell is in abnormal conditions such as overcharge, high temperature, internal short circuit (such as acupuncture), the active oxygen and oxygen generated by the decomposition of the positive electrode material at high temperature react strongly with the electrolyte and the negative electrode to release a large amount of heat, causing the battery to rise sharply in temperature, and further causing the electrolyte, diaphragm, etc. to burn, resulting in thermal runaway of the battery. Thermal runaway of a single cell can easily cause heat spread and cause the entire module cell to catch fire, thereby causing accidents such as explosions and fires in electric vehicles. The modification of positive and negative electrode materials and electrolyte materials in terms of safety has a great impact on electrochemical performance. For example, flame-retardant electrolytes can greatly shorten the flame burning time, but flame-retardant electrolytes will greatly increase the internal resistance of the battery and reduce the battery cycle performance.

[0003] Relatively speaking, the modification of the diaphragm material has the least effect on the overall performance. Therefore, it is very important to improve the safety performance of the diaphragm, especially the flame retardant performance. The diaphragm material in the prior art is mainly polyolefin material. In order to improve the safety performance of the diaphragm, ceramic coating or polymer coating is usually applied on the polyolefin base film to improve the thermal shrinkage performance of the diaphragm. However, when the battery cell is out of control and catches fire, the diaphragm cannot prevent the battery cell from burning. The main flame retardants at present are inorganic flame retardants, halogen flame retardants and phosphorus flame retardants. Inorganic flame retardants absorb heat by losing water when the flame retardant is heated, thereby alleviating or terminating the heating process of the main material. The flame retardant efficiency of such flame retardants is extremely low; phosphorus flame retardants decompose phosphoric acid liquid film and strong dehydrating agent polymetaphosphoric acid through phosphorus compounds, so that the polymer is dehydrated and carbonized to form a carbonized layer, isolating combustibles, and its efficiency is general; halogen flame retardants effectively capture active free radicals through halogen free radicals, thereby alleviating or terminating the radical chain reaction of combustion, and generating non-flammable gases at the same time, thereby isolating oxygen, and its efficiency is relatively high. Summary of the invention

[0004] In view of at least one of the problems existing in the prior art, the present disclosure provides a flame retardant composite diaphragm, the flame retardant composite diaphragm comprising:

[0005] A base film and a flame retardant coating disposed on at least one surface of the base film; wherein the flame retardant coating comprises a flame retardant, and the flame retardant comprises decabromodiphenylethane and antimony trioxide.

[0006] In one aspect of the present disclosure, the flame retardant coating includes decabromodiphenylethane, antimony trioxide, a binder, and an auxiliary agent, wherein the auxiliary agent includes at least one of a dispersant, a wetting agent, a thickener, and a defoaming agent.

[0007] In one aspect of the present disclosure, the flame retardant coating has a thickness of 1 to 20 μm.

[0008] In one aspect of the present disclosure, in the flame retardant, the mass ratio of decabromodiphenylethane to antimony trioxide is (2-5):1.

[0009] In one aspect of the present disclosure, in the flame retardant, the mass ratio of decabromodiphenylethane to antimony trioxide is (2.5-3.5):1.

[0010] In one aspect of the present disclosure, the flame retardant coating further comprises: an adhesive and an auxiliary agent, the weight of the adhesive is 2 to 10% of the weight of the flame retardant, and the weight of the auxiliary agent is 2 to 10% of the weight of the flame retardant.

[0011] In one aspect of the present disclosure, the auxiliary agent includes: a dispersant, a wetting agent, a thickener and a defoaming agent; wherein the weight of the dispersant is 0.1 to 2% of the weight of the flame retardant, the weight of the wetting agent is 0.4 to 5% of the weight of the flame retardant, the weight of the thickener is 0.5 to 3% of the weight of the flame retardant, and the weight of the defoaming agent is 0 to 0.5% of the weight of the flame retardant.

[0012] In one aspect of the present disclosure, the material of the base film includes at least one of polyethylene, polypropylene, PP / PE / PP, polyethylene terephthalate, polyimide, and aramid.

[0013] In one aspect of the present disclosure, the thickness of the base film is selected from 5 to 20 μm, preferably 5 to 12 μm.

[0014] In one aspect of the present disclosure, a ceramic layer is coated on one surface or on two opposite surfaces of the base membrane, and the material of the ceramic layer includes at least one of aluminum oxide, boehmite, magnesium hydroxide, aluminum hydroxide, garnet, silicon dioxide and an oxide solid electrolyte.

[0015] In one aspect of the present disclosure, the thickness of the ceramic layer is selected from 1 to 5 μm, preferably 2.5 to 3.5 μm.

[0016] In one aspect of the present disclosure, the binder includes at least one of carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, polyacrylate, polyvinyl alcohol, and polyvinylidene fluoride.

[0017] In one aspect of the present disclosure, the dispersant includes at least one of polyacrylic acid copolymers, sodium polyacrylate, ammonium polyacrylate, carboxylates, and sulfonates.

[0018] In one aspect of the present disclosure, the wetting agent is selected from at least one of fluorocarbon surfactants, polyoxyethylene ethers, sodium dodecyl sulfate, sodium dodecyl sulfonate, and polyether-modified polydimethylsilane.

[0019] In one aspect of the present disclosure, the thickener is selected from at least one of sodium carboxymethyl cellulose, carboxyethyl cellulose, sodium alginate, polyacrylamide and polyvinyl alcohol.

[0020] In one aspect of the present disclosure, the defoaming agent is selected from polyether-modified polydimethylsilane.

[0021] The present disclosure also provides a method for preparing the flame-retardant composite diaphragm, comprising the following steps:

[0022] Step 1: Add a dispersant and a flame retardant to a solvent in sequence, mix them, and obtain a dispersion A;

[0023] Step 2: mixing the dispersion A with a thickener, and grinding the mixture to obtain a dispersion B; mixing the dispersion B with a wetting agent and a binder to obtain a coating slurry;

[0024] Step 3: Apply the coating slurry on at least one surface of the base film.

[0025] In one aspect of the present disclosure, the mixing process may be uniform stirring, but is not limited thereto.

[0026] In one aspect of the present disclosure, the method satisfies at least one of the following conditions:

[0027] (1) In step 1, the solvent is selected from water, a mixture of water and ethanol, and N-methylpyrrolidone;

[0028] (2) in step 1, adding a defoaming agent when adding the flame retardant;

[0029] (3) In step 2, the grinding process is performed using a sand mill;

[0030] (4) In step 3, the coating is selected from micro-concave roller coating, transfer coating, gravure coating or spray coating.

[0031] In one aspect of the present disclosure, the flame retardant coating is disposed on two opposing surfaces of the base film.

[0032] In the present disclosure, the thickness of the flame retardant coating layer is the thickness of the flame retardant coating layer provided on one surface of the base film.

[0033] In one aspect of the present disclosure, the single-side thickness of the flame retardant coating is 2-5 μm.

[0034] In one aspect of the present disclosure, the mass ratio of decabromodiphenylethane to antimony trioxide is 3:1.

[0035] In one aspect of the present disclosure, among the auxiliary agents, the wetting agent is selected from at least one of fluorocarbon surfactants, polyoxyethylene ethers, sodium dodecyl sulfate, sodium dodecyl sulfonate, polysiloxane and polyether-modified polydimethylsilane, but is not limited thereto.

[0036] In one aspect of the present disclosure, among the auxiliary agents, the thickener is selected from at least one of sodium carboxymethyl cellulose, carboxyethyl cellulose, sodium alginate, polyacrylamide and polyvinyl alcohol, but is not limited thereto.

[0037] In one aspect of the present disclosure, among the auxiliary agents, the defoaming agent is selected from polyether-modified polydimethylsilane, but is not limited thereto.

[0038] The present disclosure also provides a lithium-ion battery, which includes: a positive electrode, a negative electrode, an electrolyte, and the flame-retardant composite diaphragm or the flame-retardant composite diaphragm prepared by the method.

[0039] In the present disclosure, when the battery cell catches fire, the flame retardant material decomposes at high temperature to produce SbBr 3 It can isolate oxygen and extinguish flames. At the same time, bromine free radicals capture H and HO free radicals produced by combustion, thereby alleviating or terminating the free radical chain reaction of combustion, effectively improving the safety performance of ternary batteries.

[0040] Beneficial effects:

[0041] By using the flame-retardant film provided by the present invention, oxygen can be isolated and the flame can be extinguished when the battery cell catches fire, thereby alleviating or terminating the free radical chain reaction of combustion, and effectively improving the safety performance of the ternary battery; the flame-retardant film provided by the present invention has a small thermal shrinkage rate at high temperature and has suitable air permeability; and, compared with lithium batteries using films of the prior art, lithium batteries using the flame-retardant film provided by the present invention do not show a decline in electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1The schematic diagram of the structure of the flame-retardant composite diaphragm prepared in Example 1 is shown.

[0043] Figure 2 A flow chart of preparing a flame-retardant composite diaphragm in Example 1 is shown. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solution and advantages of the present disclosure clearer, the technical solution of the present disclosure will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present disclosure, rather than all the embodiments. The relevant embodiments described herein are illustrative and are used to provide a basic understanding of the present disclosure. The embodiments of the present disclosure should not be interpreted as limiting the present disclosure.

[0045] the term:

[0046] For simplicity, only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.

[0047] In this article, the terms "comprises", "comprising" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device that includes a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of more restrictions, an element defined by the sentence "comprising a ..." does not exclude the presence of other identical elements in the process, method, article or device that includes the element.

[0048] In this document, it is necessary to understand that the orientations or positional relationships indicated by terms such as “upper”, “lower”, “top”, “bottom”, “inside” and “outside” are based on the orientations or positional relationships shown in the accompanying drawings and are only for the convenience of describing the present invention and simplifying the description. They do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0049] In the description herein, unless otherwise specified, “above” and “below” include the number.

[0050] Unless otherwise specified, the terms used in this disclosure have the commonly known meanings generally understood by those skilled in the art. Unless otherwise specified, the numerical values ​​of the various parameters mentioned in this disclosure can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the embodiments of this disclosure).

[0051] The term "about" is used to describe and illustrate small changes. When used in conjunction with an event or situation, the term may refer to an example in which the event or situation occurs precisely and an example in which the event or situation occurs very approximately. For example, when used in conjunction with a numerical value, the term may refer to a range of variation of less than or equal to ±10% of the numerical value, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%. In addition, amounts, ratios, and other numerical values ​​are sometimes presented in this article in a range format. It should be understood that such a range format is for convenience and simplicity, and should be flexibly understood to include not only numerical values ​​explicitly designated as range limits, but also all individual numerical values ​​or subranges encompassed within the range, as if each numerical value and subrange were explicitly designated.

[0052] A list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.

[0053] The present disclosure is further described below in conjunction with specific embodiments. It should be understood that these specific embodiments are only used to illustrate the present disclosure and are not used to limit the scope of the present disclosure.

[0055] negative electrode:

[0056] In some embodiments of the present disclosure, the negative electrode includes a negative electrode plate, and the negative electrode plate includes a current collector and a negative electrode active material layer disposed on the current collector. The specific types of negative electrode active materials are not subject to specific restrictions and can be selected according to needs. Specifically, the negative electrode active material is selected from natural graphite, artificial graphite, mesophase microcarbon beads (abbreviated as MCMB), hard carbon, soft carbon, silicon, silicon-oxygen composites, silicon-carbon composites, Li-Sn alloys, Li-Sn-O alloys, Sn, SnO, SnO 2 , spinel-structured lithiated TiO 2 -Li 4 Ti 5 O 12 , Li-Al alloy. Non-limiting examples of carbon materials include crystalline carbon, amorphous carbon and mixtures thereof. Crystalline carbon can be amorphous or flake-shaped, platelet-shaped, spherical or fibrous natural graphite or artificial graphite. Amorphous carbon can be soft carbon, hard carbon, mesophase pitch carbide, calcined coke, etc.

[0057] In some embodiments of the present disclosure, the negative electrode active material layer may include a binder and optionally a conductive material. The binder improves the bonding between the negative electrode active material particles and the bonding between the negative electrode active material and the current collector.

[0058] In some embodiments of the present disclosure, non-limiting examples of binders include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber, acrylated styrene-butadiene rubber, polyacrylic acid, polyacrylate, acrylonitrile multipolymers, and the like.

[0059] In some embodiments of the present disclosure, the negative electrode active material layer includes a conductive material so that the electrode has conductivity. The conductive material may include any conductive material as long as it does not cause chemical changes. Non-limiting examples of conductive materials include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.), metal-based materials (e.g., metal powder, metal fiber, etc., such as copper, nickel, aluminum, silver, etc.), conductive polymers (e.g., polyphenylene derivatives) and mixtures thereof.

[0060] In some embodiments of the present disclosure, the negative electrode sheet of the present disclosure includes a negative electrode active material, a binder and a conductive agent.

[0061] In some embodiments of the present disclosure, the negative electrode active material of the present disclosure may also be selected from other materials that can electrochemically absorb and release metal ions such as lithium ions. Specifically, it can be selected from carbonaceous materials, silicon materials, alloy materials, lithium-containing metal oxide materials, etc. They can be used alone or in any combination of two or more.

[0062] In some embodiments of the present disclosure, the negative electrode current collector may be selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.

[0063] positive electrode:

[0064] In some embodiments of the present disclosure, the positive electrode includes a positive electrode sheet, the positive electrode sheet includes a current collector and a positive electrode active material layer disposed on the current collector. The positive electrode active material includes a compound that reversibly embeds and deintercalates lithium ions. The positive electrode active material may include a composite oxide containing lithium and at least one element selected from cobalt, manganese and nickel. The specific types of positive electrode active materials are not subject to specific restrictions and can be selected according to needs. The positive electrode active material is optionally selected from lithium cobalt oxide LiCoO 2 At least one of (LCO), lithium nickel manganese cobalt ternary material (NCM), lithium iron phosphate, and lithium manganate. These may be used alone or in any combination of two or more.

[0065] In some embodiments of the present disclosure, the positive electrode active material may have a coating layer on the surface, or may be mixed with another compound having a coating layer.

[0066] In some embodiments of the present disclosure, the coating may include at least one coating element compound selected from an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, and a hydroxycarbonate of a coating element. The compound for the coating may be amorphous or crystalline. The coating element contained in the coating may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The coating may be applied by any method as long as the method does not adversely affect the performance of the positive active material. For example, the method may include any coating method well known to those of ordinary skill in the art, such as spraying, dipping, etc.

[0067] In some embodiments of the present disclosure, the positive electrode active material layer further includes a binder, and optionally also includes a conductive material. The binder improves the bonding between the positive electrode active material particles and also improves the bonding between the positive electrode active material and the current collector.

[0068] In some embodiments of the present disclosure, non-limiting examples of the binder include polyvinylidene fluoride, polytetrafluoroethylene, polyvinylidene fluoride, polyacrylonitrile, and the like.

[0069] In some embodiments of the present disclosure, the positive electrode active material layer includes a conductive material to impart conductivity to the electrode. The conductive material may include any conductive material as long as it does not cause chemical changes. Non-limiting examples of conductive materials include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.), metal-based materials (e.g., metal powder, metal fiber, etc., including, for example, copper, nickel, aluminum, silver, etc.), conductive polymers (e.g., polyphenylene derivatives) and mixtures thereof.

[0070] In some embodiments of the present disclosure, the positive electrode current collector may be aluminum (Al), but is not limited thereto.

[0071] Diaphragm:

[0072] In some embodiments of the present disclosure, the lithium-ion battery and electrochemical device of the present disclosure are provided with a separator between the positive electrode and the negative electrode to prevent short circuit, and the separator is the flame-retardant composite separator provided by the present disclosure.

[0073] In some embodiments of the present disclosure, the flame retardant composite membrane includes a base film and a flame retardant coating coated on at least one surface of the base film; the flame retardant coating provided by the present disclosure includes a flame retardant, and the flame retardant includes decabromodiphenylethane and antimony trioxide.

[0074] In some embodiments of the present disclosure, the single-sided thickness of the flame-retardant coating in the flame-retardant composite diaphragm is 1-20 μm. Specifically, the single-sided thickness may be 1 μm, 2 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm or 20 μm.

[0075] In some embodiments of the present disclosure, in the flame retardant, the mass ratio of decabromodiphenylethane to antimony trioxide is (2-5): 1. Specifically, the mass ratio of decabromodiphenylethane to antimony trioxide can be 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1 or 5:1.

[0076] In some preferred embodiments of the present disclosure, in the flame retardant, the mass ratio of decabromodiphenylethane to antimony trioxide is (2.5-3.5): 1. Specifically, the mass ratio of decabromodiphenylethane to antimony trioxide can be 2.5:1, 2.8:1, 3:1, 3.2:1 or 3.5:1.

[0077] In some embodiments of the present disclosure, the flame retardant coating further comprises an adhesive and an auxiliary agent; the weight of the adhesive is 2-10% of the weight of the flame retardant, and the weight of the auxiliary agent is 2-10% of the weight of the flame retardant. Specifically, the weight of the adhesive is 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10% of the weight of the flame retardant. Specifically, the weight of the auxiliary agent is 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10% of the weight of the flame retardant.

[0078] In some embodiments of the present disclosure, the auxiliary agent includes: a dispersant, a wetting agent, a thickener and a defoaming agent; wherein the weight of the dispersant is 0.1-2% of the weight of the flame retardant, the weight of the wetting agent is 0.4-5% of the weight of the flame retardant, the weight of the thickener is 0.5-3% of the weight of the flame retardant, and the weight of the defoaming agent is 0-0.5% of the weight of the flame retardant. Specifically, the weight of the dispersant is 0.1%, 0.2%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8% or 2% of the weight of the flame retardant. Specifically, the weight of the wetting agent is 0.4%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5% of the weight of the flame retardant. Specifically, the weight of the thickener is 0.5%, 0.8%, 1%, 1.5%, 1.8%, 2%, 2.5%, 2.8% or 3% of the weight of the flame retardant. Specifically, the weight of the defoamer is 0.01%, 0.1%, 0.2%, 0.3%, 0.4% or 0.5% of the weight of the flame retardant.

[0079] In some embodiments of the present disclosure, the material of the base film includes at least one of polyethylene, polypropylene, PP / PE / PP (polypropylene / polyethylene / polypropylene), polyethylene terephthalate, polyimide and aramid.

[0080] In some embodiments of the present disclosure, the thickness of the base film is selected from 5 to 20 μm. Specifically, the thickness of the base film may be 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm or 20 μm.

[0081] In some preferred embodiments of the present disclosure, the thickness of the base film is selected from 5 to 12 μm. Specifically, the thickness of the base film can be 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm or 12 μm.

[0082] In some embodiments of the present disclosure, a ceramic layer is coated on one surface or on two opposite surfaces of the base film, and the material of the ceramic layer includes at least one of aluminum oxide, boehmite, magnesium hydroxide, aluminum hydroxide, garnet, silicon dioxide and an oxide solid electrolyte, but is not limited thereto.

[0083] In some embodiments of the present disclosure, the thickness of the ceramic layer is selected from 1 to 5 μm. Specifically, the thickness of the ceramic layer may be 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm or 5 μm.

[0084] In some embodiments of the present disclosure, the binder includes at least one of carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, polyacrylate, polyvinyl alcohol, and polyvinylidene fluoride, but is not limited thereto.

[0085] In some embodiments of the present disclosure, the dispersant includes at least one of polyacrylic acid copolymers, sodium polyacrylate, ammonium polyacrylate, carboxylates, and sulfonates, but is not limited thereto.

[0086] In some embodiments of the present disclosure, the wetting agent is selected from at least one of fluorocarbon surfactants, polyoxyethylene ethers, sodium dodecyl sulfate, sodium dodecyl sulfonate, and polyether-modified polydimethylsilane, but is not limited thereto.

[0087] In some embodiments of the present disclosure, the thickener is selected from at least one of sodium carboxymethyl cellulose, carboxyethyl cellulose, sodium alginate, polyacrylamide and polyvinyl alcohol, but is not limited thereto.

[0088] In some embodiments of the present disclosure, the defoaming agent is selected from polyether-modified polydimethylsilane, but is not limited thereto.

[0089] In some embodiments of the present disclosure, the flame retardant composite diaphragm provided by the present disclosure is prepared by the following method:

[0090] Step 1: Add a dispersant and a flame retardant to a solvent in sequence, mix them, and obtain a dispersion A;

[0091] Step 2: mixing the dispersion A with a thickener, and grinding the mixture to obtain a dispersion B; mixing the dispersion B with a wetting agent and a binder to obtain a coating slurry;

[0092] Step 3: Apply the coating slurry on at least one surface of the base film.

[0093] In one aspect of the present disclosure, the mixing process may be uniform stirring, but is not limited thereto.

[0094] In one aspect of the present disclosure, the solvent is selected from one of water, a mixture of water and ethanol, and N-methylpyrrolidone.

[0095] In one aspect of the present disclosure, in step 1, a defoaming agent is added when the flame retardant is added.

[0096] In one aspect of the present disclosure, in step 2, the grinding process is performed using a sand mill.

[0097] In one aspect of the present disclosure, in step 3, the coating is selected from one of micro-concave roller coating, transfer coating, gravure coating or spray coating.

[0098] In one aspect of the present disclosure, the flame retardant coating is disposed on two opposing surfaces of the base film.

[0099] In the present disclosure, the thickness of the flame retardant coating layer is the thickness of the flame retardant coating layer provided on one surface of the base film.

[0100] In one aspect of the present disclosure, the single-sided thickness of the flame retardant coating is 2-5 μm. Specifically, the single-sided thickness of the flame retardant coating may be 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm or 5 μm.

[0101] In one aspect of the present disclosure, the mass ratio of decabromodiphenylethane to antimony trioxide is 3:1.

[0102] In one aspect of the present disclosure, among the auxiliary agents, the wetting agent is selected from at least one of fluorocarbon surfactants, polyoxyethylene ethers, sodium dodecyl sulfate, sodium dodecyl sulfonate, polysiloxane and polyether-modified polydimethylsilane, but is not limited thereto.

[0103] In one aspect of the present disclosure, among the auxiliary agents, the thickener is selected from at least one of sodium carboxymethyl cellulose, carboxyethyl cellulose, sodium alginate, polyacrylamide and polyvinyl alcohol, but is not limited thereto.

[0104] In one aspect of the present disclosure, among the auxiliary agents, the defoaming agent is selected from polyether-modified polydimethylsilane, but is not limited thereto.

[0105] The present disclosure also provides a lithium-ion battery, which includes: a positive electrode, a negative electrode, an electrolyte, and the flame-retardant composite diaphragm or the flame-retardant composite diaphragm prepared by the method.

[0106] In the present disclosure, when the battery cell catches fire, the flame retardant material decomposes at high temperature to produce SbBr 3It can isolate oxygen and cut off the flame, while bromine free radicals capture H and HO free radicals produced by combustion, thereby alleviating or terminating the free radical chain reaction of combustion, and effectively improving the safety performance of ternary batteries. By using the flame-retardant film provided by the present disclosure, oxygen can be isolated and the flame can be cut off when the battery cell catches fire, thereby alleviating or terminating the free radical chain reaction of combustion, and effectively improving the safety performance of ternary batteries; the flame-retardant film provided by the present disclosure has a small thermal shrinkage rate at high temperature and has suitable air permeability; and, compared with lithium batteries using films of the prior art, lithium batteries using the flame-retardant film provided by the present disclosure do not show a decrease in electrochemical performance.

[0107] Electrolyte:

[0108] The lithium-ion batteries and electrochemical devices of the present disclosure also include an electrolyte.

[0109] In some embodiments of the present disclosure, the electrolyte includes a lithium salt and a solvent.

[0110] In some embodiments of the present disclosure, the lithium salt includes at least one of an organic lithium salt or an inorganic lithium salt. In some embodiments, the lithium salt includes, but is not limited to: lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium difluorophosphate (LiPO 2 F 2 ), bis(trifluoromethanesulfonyl)imide lithium LiN (CF 3 SO 2 ) 2 (LiTFSI), lithium bis(fluorosulfonyl)imide Li(N(SO 2 F) 2 )(LiFSI), LiB(C 2 O 4 ) 2 (LiBOB) or lithium difluorooxalatoborate LiBF 2 (C 2 O 4 In some embodiments, the concentration of the lithium salt in the electrolyte is about 0.5 mol / L to 3 mol / L, about 0.5 mol / L to 2 mol / L, or about 0.8 mol / L to 1.5 mol / L.

[0111] In some embodiments of the present disclosure, the solvent may be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0112] In some embodiments of the present disclosure, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, additives that improve battery low temperature performance, etc.

[0113] Lithium-ion battery:

[0114] In some embodiments of the present disclosure, the lithium-ion battery involved in the present disclosure includes the above-mentioned positive electrode plate, negative electrode plate, flame-retardant composite separator, electrolyte, etc., but is not limited thereto.

[0115] In some embodiments of the present disclosure, the lithium ion battery involved in the present disclosure may include an outer package, which may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer package of the secondary battery may also be a soft package, such as a pouch-type soft package.

[0116] In some embodiments of the present disclosure, the lithium ion battery involved in the present disclosure is a cylindrical battery.

[0117] In some embodiments of the present disclosure, the present disclosure further provides a battery module. The battery module includes the above-mentioned lithium-ion battery. The battery module of the present disclosure uses the above-mentioned lithium-ion battery, and therefore has at least the same advantages as the lithium-ion battery. The number of lithium-ion batteries contained in the battery module of the present disclosure can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module.

[0118] In some embodiments of the present disclosure, the present disclosure further provides a battery pack, which includes the above-mentioned battery module. The number of battery modules included in the battery pack can be adjusted according to the application and capacity of the battery pack.

[0119] Device:

[0120] The present disclosure also provides a device, which includes at least one of the above-mentioned lithium-ion battery, battery module or battery pack.

[0121] In some embodiments of the present disclosure, the device includes, but is not limited to: electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, power storage systems, etc. In order to meet the device's requirements for high power and high energy density of lithium-ion batteries, a battery pack or battery module may be used.

[0122] In some embodiments of the present disclosure, the device may be a mobile phone, a tablet computer, a laptop computer, etc. The device is usually required to be light and thin, and a lithium-ion battery may be used as a power source.

[0123] The present disclosure is further described below in conjunction with the examples. It should be understood that these examples are only used to illustrate the present disclosure and are not used to limit the scope of the present disclosure.

[0124] Example

[0125] Test method:

[0126] 1. Thermal shrinkage test: Cut a 100mm×100mm flame-retardant composite diaphragm in the longitudinal direction of the film roll, clamp it horizontally with a plywood, and then place it in a 130℃ oven for 1 hour. Measure the transverse and longitudinal dimensions after baking, and then calculate the transverse and longitudinal shrinkage according to the formula: shrinkage = (100-size after baking) / 100.

[0127] 2. Air permeability test: Under a pressure of 1.21KPa, 100mL of air passes through an area of ​​6.45cm 2 The time required for flame retardant composite diaphragm.

[0128] 3. Flame retardant test: Take a 100mm×15mm flame retardant composite diaphragm specimen, burn it vertically, and test the flame self-extinguishing time.

[0129] 4. Cycle performance test: In order to accelerate the cycle test, a 45°C cycle test, 0.5C charge / 1C discharge, and a rated capacity of 3.7Ah were used.

[0130] Embodiment 1:

[0131] (1) Preparation of flame retardant composite diaphragm:

[0132] In the preparation of the flame-retardant composite diaphragm, the components are added according to the following weight percentages: 100 parts of flame retardant; 4 parts of adhesive; 0.5 parts of dispersant; 0.5 parts of wetting agent; and 1.5 parts of thickener.

[0133] Add 3.5 grams of polyacrylic acid copolymer dispersant into 2000 grams of water, stir and disperse evenly to obtain a mixed solution; then add 650 grams of flame retardant in a ratio of 3:1 of decabromodiphenylethane: antimony trioxide into the mixed solution, stir and disperse evenly, and grind with a sand mill for 1 hour to obtain a dispersion with a particle size D50 less than 2μm; mix the obtained dispersion with CMC thickener, polyacrylate adhesive and polyether modified siloxane wetting agent, stir well for 2 hours with a stirrer to obtain a coating slurry; apply the coating slurry on a 9μm PE base film by micro-gravure coating, wherein the coating thickness is 5μm on both sides. The structure of the flame-retardant composite diaphragm prepared in Example 1 is as follows: Figure 1 shown.

[0134] (2) Preparation of lithium-ion batteries:

[0135] Positive electrode preparation: The binder PVDF is dispersed in NMP solvent to obtain PVDF glue, and then the positive electrode ternary high nickel active material Ni90 and conductive carbon black are added to the PVDF glue at a mass ratio of positive electrode material: conductive agent: binder of 97.5:1.5:1.0, and the positive electrode slurry is obtained after being fully stirred. The positive electrode slurry is evenly coated on both sides of the aluminum foil, and after drying, calendering and vacuum drying, the positive electrode sheet, also called the positive electrode, is obtained;

[0136] Negative electrode preparation: Sodium carboxymethyl cellulose (CMC) is dispersed in deionized water in advance, stirred evenly to obtain CMC glue, and then 30% silicon-oxygen doped graphite material, conductive carbon black, binder (styrene-butadiene rubber, polyacrylic acid copolymer) and sodium carboxymethyl cellulose glue are mixed in a mass ratio of 96.0:1.0:2.4:0.6 to obtain negative electrode slurry, and the negative electrode slurry is coated on both sides of the copper foil, and after drying, calendering and vacuum drying, a negative electrode sheet, also called a negative electrode, is obtained;

[0137] Preparation of battery cells: A flame-retardant composite separator is placed between the positive electrode and the negative electrode, and then the structure consisting of the positive electrode, the flame-retardant composite and the negative electrode is stacked to obtain a battery cell with a battery cell capacity of 3.7Ah.

[0138] Embodiment 2:

[0139] The steps in Example 2 are the same as those in Example 1, except that in Example 2, the coating slurry is coated on a 9+3 (9 μm PE base film + a single-sided 3 μm Al 2 O 3 The flame retardant coating is coated on the opposite side of the ceramic layer, and the coating thickness is 5 μm on a single side.

[0140] Embodiment 3:

[0141] The steps in Example 3 are the same as those in Example 2, except that the coating thickness in Example 3 is 3 μm on a single side.

[0142] Embodiment 4:

[0143] The method for preparing the flame retardant composite diaphragm in Example 4 is the same as that in Example 3, except that the DBDPE (decabromodiphenylethane) / Sb 2 O 3 The ratio is adjusted to 1:1.

[0144] Embodiment 5:

[0145] The method for preparing the flame-retardant composite diaphragm in Example 5 is the same as that in Example 3, the only difference being that the amount of adhesive used is 10%.

[0146] Comparative Example 1:

[0147] The steps in Comparative Example 1 are the same as those in Example 1, except that a commercially available ceramic-coated PE base film is used in Comparative Example 1. The thickness of the PE base film is 9 μm, and both sides of the PE base film are coated with 3 μm thick Al 2 O 3 The ceramic layer replaces the flame-retardant composite diaphragm prepared in Example 1.

[0148] Comparative Example 2:

[0149] The steps in Comparative Example 2 are the same as those in Example 3, except that the flame retardant used in Comparative Example 2 contains only decabromodiphenylethane and does not contain antimony trioxide.

[0150] Comparative Example 3:

[0151] The steps in Comparative Example 3 are the same as those in Example 3, except that the flame retardant used in Comparative Example 3 only contains antimony trioxide and does not contain decabromodiphenylethane.

[0152] Performance Test:

[0153] Examples 1-5 and Comparative Examples 1-3 were subjected to heat shrinkage test, air permeability test and flame retardancy test, respectively. The test results are as follows, wherein the longitudinal direction refers to the direction of mechanical stretching, and the transverse direction refers to the direction perpendicular to the mechanical stretching:

[0154] Table 1

[0155]

[0156] It can be seen that compared with Comparative Example 1 using the film of the prior art, Examples 1-5 still maintain good electrochemical performance, and their capacity retention rate has not decreased; and compared with Comparative Example 1 using the film of the prior art, Comparative Example 2 using only decabromodiphenylethane, and Comparative Example 3 using only antimony trioxide, Examples 1-3 and Example 5 show excellent flame retardant properties, which are non-flammable in the flame retardant test and have suitable air permeability; compared with Comparative Examples 2 and 3, Examples 1-5 also have smaller thermal shrinkage at 130°C. In addition, in Example 4, decabromodiphenylethane and Sb in the flame retardant are 2 O 3 The ratio is 1:1, relative to the mass ratio of decabromodiphenylethane and antimony trioxide in the flame retardant is (2-5):1, in Example 4, antimony trioxide is added in excess, resulting in a decrease in flame retardant efficiency.

[0157] Although illustrative embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present disclosure, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present disclosure.

Claims

1. A flame retardant composite diaphragm, It is characterized in that The flame retardant composite diaphragm comprises: A base film and a flame retardant coating disposed on at least one surface of the base film; Wherein, the flame retardant coating comprises a flame retardant, and the flame retardant comprises decabromodiphenylethane and antimony trioxide.

2. The flame retardant composite diaphragm according to claim 1, It is characterized in that The thickness of the flame retardant coating is 1 to 20 μm.

3. The flame retardant composite diaphragm according to claim 1, It is characterized in that In the flame retardant, the mass ratio of decabromodiphenylethane to antimony trioxide is (2-5):

1.

4. The flame retardant composite diaphragm according to claim 3, It is characterized in that In the flame retardant, the mass ratio of decabromodiphenylethane to antimony trioxide is (2.5-3.5):

1.

5. The flame retardant composite diaphragm according to claim 1, It is characterized in that The flame retardant coating further comprises: The weight of the adhesive and the auxiliary agent is 2-10% of the weight of the flame retardant, and the weight of the auxiliary agent is 2-10% of the weight of the flame retardant.

6. The flame retardant composite diaphragm according to claim 5, It is characterized in that The auxiliary agent includes: Dispersants, wetting agents, thickeners and defoamers; The weight of the dispersant is 0.1-2% of the weight of the flame retardant, the weight of the wetting agent is 0.4-5% of the weight of the flame retardant, the weight of the thickener is 0.5-3% of the weight of the flame retardant, and the weight of the defoaming agent is 0-0.5% of the weight of the flame retardant.

7. The flame retardant composite diaphragm according to claim 6, It is characterized in that The material of the base film includes at least one of polyethylene, polypropylene, PP / PE / PP, polyethylene terephthalate, polyimide and aramid; and / or The thickness of the base film is selected from 5 to 20 μm; and / or A ceramic layer is coated on one surface or two opposite surfaces of the base film, wherein the material of the ceramic layer includes at least one of aluminum oxide, boehmite, magnesium hydroxide, aluminum hydroxide, garnet, silicon dioxide and oxide solid electrolyte, and the thickness of the ceramic layer is selected from 1 to 5 μm; and / or The binder comprises at least one of carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, polyacrylate, polyvinyl alcohol and polyvinylidene fluoride; and / or The dispersant comprises at least one of polyacrylic acid copolymers, sodium polyacrylate, ammonium polyacrylate, carboxylates and sulfonates; and / or The wetting agent is selected from at least one of fluorocarbon surfactants, polyoxyethylene ethers, sodium dodecyl sulfate, sodium dodecyl sulfonate and polyether-modified polydimethylsilane; and / or The thickener is selected from at least one of sodium carboxymethyl cellulose, carboxyethyl cellulose, sodium alginate, polyacrylamide and polyvinyl alcohol; and / or The defoaming agent is selected from polyether-modified polydimethylsilane.

8. A method for preparing the flame-retardant composite diaphragm according to any one of claims 1 to 7, It is characterized in that The following steps are involved: Step 1: Add a dispersant and a flame retardant to a solvent in sequence, mix them, and obtain a dispersion A; Step 2: mixing the dispersion A with a thickener, and grinding the mixture to obtain a dispersion B; mixing the dispersion B with a wetting agent and a binder to obtain a coating slurry; Step 3: Apply the coating slurry on at least one surface of the base film.

9. The method according to claim 8, It is characterized in that The method satisfies at least one of the following conditions: (1) In step 1, the solvent is selected from water, a mixture of water and ethanol, and N-methylpyrrolidone; (2) in step 1, adding a defoaming agent when adding the flame retardant; (3) In step 2, the grinding process is performed using a sand mill; (4) In step 3, the coating is selected from micro-concave roller coating, transfer coating, gravure coating or spray coating.

10. A lithium ion battery, It is characterized in that The lithium-ion battery comprises: A positive electrode, a negative electrode, an electrolyte, and a flame-retardant composite diaphragm according to any one of claims 1 to 7 or a flame-retardant composite diaphragm prepared by the method according to any one of claims 8 to 9.

Citation Information

Patent Citations

  • Flame-retardant cellulose membrane for lithium battery and preparation method of membrane

    CN103579562A

  • Light-weight high-flame-retardant polyphenyl ether modified material, new energy automobile flame-retardant battery shell upper cover and preparation method of upper cover

    CN109135248A

  • Flame-retardant composite diaphragm, preparation method thereof and lithium ion battery

    CN113078412A

  • Composite diaphragm, preparation method thereof and lithium ion battery

    CN114039171A

  • Lithium battery comprising composite flame retardant particles

    CN114649498A

Cited By

  • High-strength lithium battery microporous diaphragm produced by wet process and preparation method thereof

    CN119381699A