Low-resistivity sodium ferric pyrophosphate positive electrode material as well as preparation method and application thereof
By adjusting the defect content and sintering conditions of Na and Fe, a low-resistivity sodium iron pyrophosphate cathode material was prepared, which solved the problem of poor conductivity, achieved higher energy density and stability, and avoided environmental pollution.
Patent Information
- Application Number
- CN202411035629.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The poor conductivity of existing sodium-ion battery cathode materials leads to large energy losses, and the Fe-based cathode materials are environmentally unfriendly and unstable. It is necessary to develop low-resistivity sodium iron pyrophosphate cathode materials to replace them.
By adjusting the content of Na vacancies and Fe defects, controlling the band gap width and conductivity, ball milling, spray drying and sintering processes were used to prepare low resistivity Na4-xFe3-y(PO4)2(P2O7)/C materials. When unfriendly elements such as V and Mn are introduced, the heating rate and holding time are controlled to improve the conversion efficiency of phosphate and pyrophosphate and optimize the conductivity of the material.
A low-resistivity sodium ferric pyrophosphate cathode material has been realized, which reduces the Na ion diffusion barrier, widens the Na ion diffusion channel, increases the energy density, avoids the use of environmentally unfriendly elements, and improves the conductivity of the material. sex and stability.
Smart Images

Figure CN118790969A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium ion batteries, and in particular relates to a low-resistivity sodium iron pyrophosphate positive electrode material and a preparation method and application thereof. Background Art
[0002] Among the lithium batteries currently on the market, sodium (Na) ion batteries have attracted much attention due to the abundant reserves of Na elements and the close physical and chemical properties to Li, making sodium ion batteries (SIBs) an ideal substitute for lithium ion batteries. Most of the technical difficulties currently faced by sodium ion batteries are concentrated in the positive electrode materials. The current positive electrode materials are concentrated in vanadium (V)-based, iron (Fe)-based and manganese (Mn)-based positive electrode materials. Compared with some environmental unfriendly and unstable problems of V-based and Mn-based materials, Fe-based positive electrode materials will be a strong competitor for future Na ion battery positive electrode materials. Na4Fe3(PO4)2P2O7 has become one of the ideal choices for sodium ion battery positive electrode materials due to its low cost, green environmental protection, good structural stability and long cycle life. However, its poor conductivity causes large energy loss during use. Therefore, the development of low-resistivity sodium iron pyrophosphate positive electrode materials can provide a way of thinking for practical production applications. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a low resistivity sodium iron pyrophosphate positive electrode material and a preparation method and application thereof.
[0004] The first object of the present invention is to provide a low resistivity sodium iron pyrophosphate positive electrode material, the chemical formula of the low resistivity sodium iron pyrophosphate positive electrode material is Na 4-x Fe 3-y (PO4)2(P2O7) / C, 0≤x≤1, 0≤y≤1, x<y.
[0005] In one embodiment of the present invention, the band gap Eg of the low-resistivity sodium iron pyrophosphate positive electrode material is less than 2.7 eV.
[0006] In one embodiment of the present invention, the resistivity R of the low-resistivity sodium iron pyrophosphate positive electrode material satisfies the following relationship:
[0007] The second object of the present invention is to provide a method for preparing the low-resistivity sodium iron pyrophosphate positive electrode material, comprising the following steps: uniformly mixing a sodium source, an iron source, a phosphorus source, a carbon source and water, and obtaining the low-resistivity sodium iron pyrophosphate positive electrode material through ball milling, spray drying and sintering.
[0008] In one embodiment of the present invention, the sodium source is selected from one or more of sodium carbonate, sodium hydroxide, sodium sulfate and sodium dihydrogen phosphate; the iron source is selected from one or more of ferric acetate, ferric nitrate, ferrous oxalate, ferric oxide and ferric phosphate; the phosphorus source is selected from one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium dihydrogen phosphate and phosphorus pentoxide; the carbon source is selected from one or more of carbon black, graphite, acetylene black, activated carbon, citric acid, polyethylene glycol, sucrose and glucose.
[0009] In one embodiment of the present invention, the spray drying temperature is 100°C-140°C.
[0010] In one embodiment of the present invention, the sintering is carried out under a protective atmosphere and is divided into two stages; the first stage is to heat up to 300°C-350°C at a rate of 5°C / min-7°C / min and keep warm for 10min-30min; the second stage is to heat up to 600°C-750°C at a rate of 0.5°C / min-2°C / min and keep warm for 5h-10h.
[0011] In one embodiment of the present invention, the protective atmosphere is selected from nitrogen atmosphere or argon atmosphere.
[0012] The third object of the present invention is to provide a sodium ion battery positive electrode, comprising the low-resistivity sodium iron pyrophosphate positive electrode material or the low-resistivity sodium iron pyrophosphate positive electrode material prepared by the method described.
[0013] In one embodiment of the present invention, the sodium ion battery positive electrode further includes a conductive agent and a binder.
[0014] In one embodiment of the present invention, the conductive agent is selected from one or more of carbon nanotubes, acetylene black, conductive carbon black, conductive graphite, carbon fiber and graphene.
[0015] In one embodiment of the present invention, the amount of the conductive agent is ≤10wt%. It can be 0.01wt%-10wt%, 1wt%-10wt%, 2wt%-10wt%, 3wt%-10wt%, 4wt%-10wt%, 5wt%-10wt%, 6wt%-10wt%, 7wt%-10wt%, 8wt%-10wt%, 9wt%-10wt%. 0.01wt%, 0.05wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt%, 10wt%; or any amount between any two values.
[0016] In one embodiment of the present invention, the binder is selected from one or more of polyolefins, fluorine-containing resins, polypropylene resins and rubbers.
[0017] Furthermore, the binder is selected from one or more of polyvinylidene fluoride, styrene rubber, nitrile rubber, styrene butadiene rubber (SBR), polyacrylamide (PAA), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylonitrile (PAN), polyimide (PI), butadiene rubber, modified butadiene rubber, carboxyl-modified styrene butadiene rubber and modified polyorganosiloxane polymers.
[0018] In one embodiment of the present invention, the amount of the binder is ≤10wt%. It can be 0.01wt%-10wt%, 1wt%-10wt%, 2wt%-10wt%, 3wt%-10wt%, 4wt%-10wt%, 5wt%-10wt%, 6wt%-10wt%, 7wt%-10wt%, 8wt%-10wt%, 9wt%-10wt%. 0.01wt%, 0.05wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt%, 10wt%; or any amount between any two values.
[0019] A fourth object of the present invention is to provide a sodium ion battery, comprising the sodium ion battery positive electrode.
[0020] The technical solution of the present invention has the following advantages over the prior art:
[0021] (1) The preparation method of the present invention can effectively control the band gap width and further control the conductivity of the low-resistivity sodium iron pyrophosphate positive electrode material by adjusting the content of Na vacancies and Fe defects.
[0022] (2) The preparation method of the present invention regulates Na vacancies and Fe defects, and ensures that phosphate (PO4 3- ) and pyrophosphate (P2O7 4- ) conversion efficiency, making the material more electronegative and thus increasing the energy density.
[0023] (3) The low-resistivity sodium iron pyrophosphate positive electrode material described in the present invention reduces the energy gap between the valence band and the conduction band in the material by adjusting the number of Fe defects to be slightly larger than the number of Na vacancies without introducing environmentally unfriendly and unstable elements such as V and Mn, thereby reducing the Na ion diffusion barrier. A certain defect concentration widens the Na ion diffusion channel, thereby optimizing its conductive properties from the most fundamental material electronic structure layout. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:
[0025] Figure 1 The Na4Fe of Example 1 of the present invention 2.9 The first charge / discharge curve when (PO4)2(P2O7) / C is used as the positive electrode of sodium-ion battery;
[0026] Figure 2 The Na4Fe of Example 1 of the present invention 2.9 UV-visible diffuse reflectance curve of (PO4)2(P2O7) / C;
[0027] Figure 3 is Na of Example 2 of the present invention 3.9 Fe 2.8 The first charge / discharge curve when (PO4)2(P2O7) / C is used as the positive electrode of sodium-ion battery;
[0028] Figure 4 is Na of Example 2 of the present invention 3.9 Fe 2.8 UV-visible diffuse reflectance curve of (PO4)2(P2O7) / C;
[0029] Figure 5 is Na of Example 3 of the present invention 3.9 Fe 2.7 The first charge / discharge curve when (PO4)2(P2O7) / C is used as the positive electrode of sodium-ion battery;
[0030] Figure 6 is Na of Example 3 of the present invention 3.9 Fe 2.7 UV-visible diffuse reflectance curve of (PO4)2(P2O7) / C;
[0031] Figure 7 The Na of Comparative Example 1 of the present invention 3.9 Fe 2.9 The first charge / discharge curve when (PO4)2(P2O7) / C is used as the positive electrode of sodium-ion battery;
[0032] Figure 8 The Na of Comparative Example 2 of the present invention 3.9 First charge / discharge curves of Fe3(PO4)2(P2O7) / C used as the positive electrode of a sodium-ion battery. DETAILED DESCRIPTION
[0033] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. It should be understood that the specific embodiments are only used to explain the present invention, but the embodiments are not intended to limit the present invention.
[0034] In the present invention, unless otherwise explained, technical and scientific terms used in the present invention have the same meanings as commonly understood by those skilled in the art to which the present invention belongs.
[0035] In the present invention, unless otherwise stated, the term "and / or" used in the present invention includes any and all combinations of one or more of the associated listed items.
[0036] In the present invention, unless otherwise stated, the experimental methods used in the embodiments of the present invention are conventional methods unless otherwise stated, and the materials, reagents, etc. used are all commercially available unless otherwise stated.
[0037] Example 1
[0038] The low-resistivity sodium iron pyrophosphate positive electrode material of the present invention and its preparation method and application specifically include the following steps:
[0039] 15.4 g of sodium carbonate, 54.2 g of ferric phosphate dihydrate, 17.2 g of sodium dihydrogen phosphate dihydrate, 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of deionized water were mixed together for ball milling, spray dried at 120 ° C after ball milling, and the powder obtained by grinding was placed in a tube furnace for sintering. In a nitrogen atmosphere, the temperature was first increased to 325 ° C at a rate of 5 ° C / min, and kept warm for 20 min, and then increased to 650 ° C at a rate of 1 ° C / min, kept warm for 8 h, and cooled to obtain a low resistivity sodium iron pyrophosphate positive electrode material Na4Fe 2.9 (PO4)2(P2O7) / C.
[0040] Example 2
[0041] The low-resistivity sodium iron pyrophosphate positive electrode material of the present invention and its preparation method and application specifically include the following steps:
[0042] 14.3 g of sodium carbonate, 52.3 g of ferric phosphate dihydrate, 18.7 g of sodium dihydrogen phosphate dihydrate, 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of deionized water were mixed together for ball milling, spray dried at 120 ° C after ball milling, and the ground powder was placed in a tube furnace for sintering. In a nitrogen atmosphere, the temperature was first increased to 325 ° C at a rate of 6 ° C / min, and the temperature was kept for 20 min, and then the temperature was increased to 650 ° C at a rate of 1 ° C / min, and the temperature was kept for 8 h, and the low resistivity sodium iron pyrophosphate positive electrode material Na 3.9 Fe 2.8 (PO4)2(P2O7) / C.
[0043] Example 3
[0044] The low-resistivity sodium iron pyrophosphate positive electrode material of the present invention and its preparation method and application specifically include the following steps:
[0045] 15.4 g of sodium carbonate, 50.4 g of ferric phosphate dihydrate, 17.2 g of sodium dihydrogen phosphate dihydrate, 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of deionized water were mixed together for ball milling, and then spray dried at 120 ° C. The ground powder was placed in a tube furnace for sintering, and heated to 325 ° C at a rate of 7 ° C / min in a nitrogen atmosphere, and kept warm for 20 min, and then heated to 650 ° C at a rate of 1 ° C / min, kept warm for 8 h, and cooled to obtain a low resistivity sodium iron pyrophosphate positive electrode material Na 3.9 Fe 2.7 (PO4)2(P2O7) / C.
[0046] Example 4
[0047] The low-resistivity sodium iron pyrophosphate positive electrode material of the present invention and its preparation method and application specifically include the following steps:
[0048] 15.4 g of sodium carbonate, 54.2 g of ferric phosphate dihydrate, 17.2 g of sodium dihydrogen phosphate dihydrate, 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of deionized water were mixed together for ball milling, spray dried at 120 ° C after ball milling, and the ground powder was placed in a tube furnace for sintering. In a nitrogen atmosphere, the temperature was first raised to 300 ° C at a rate of 5 ° C / min, and kept warm for 20 min, then raised to 650 ° C at a rate of 1 ° C / min, kept warm for 8 h, and cooled to obtain a low resistivity sodium iron pyrophosphate positive electrode material Na4Fe 2.9 (PO4)2(P2O7) / C.
[0049] Example 5
[0050] The low-resistivity sodium iron pyrophosphate positive electrode material of the present invention and its preparation method and application specifically include the following steps:
[0051] 15.4 g of sodium carbonate, 54.2 g of ferric phosphate dihydrate, 17.2 g of sodium dihydrogen phosphate dihydrate, 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of deionized water were mixed together for ball milling, spray dried at 120 ° C after ball milling, and the ground powder was placed in a tube furnace for sintering. In a nitrogen atmosphere, the temperature was first increased to 350 ° C at a rate of 5 ° C / min, and kept warm for 20 min, and then increased to 650 ° C at a rate of 1 ° C / min, kept warm for 8 h, and cooled to obtain a low resistivity sodium iron pyrophosphate positive electrode material Na4Fe 2.9 (PO4)2(P2O7) / C.
[0052] Comparative Example 1 is basically the same as Example 1, except that the ratio of sodium to iron
[0053] 14.8 g of sodium carbonate, 54.2 g of ferric phosphate dihydrate, 17.2 g of sodium dihydrogen phosphate dihydrate, 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of deionized water were mixed together for ball milling, spray dried at 120 ° C after ball milling, and the powder obtained by grinding was placed in a tube furnace for sintering. The temperature was first increased to 325 ° C at a rate of 5 ° C / min in a nitrogen atmosphere, and kept warm for 20 min, and then increased to 650 ° C at a rate of 1 ° C / min, kept warm for 8 h, and cooled to obtain the sodium iron pyrophosphate positive electrode material Na 3.9 Fe 2.9 (PO4)2(P2O7) / C.
[0054] Comparative Example 2 is basically the same as Example 1, except that the ratio of sodium to iron
[0055] 15.4 g of sodium carbonate, 56.0 g of ferric phosphate dihydrate, 15.6 g of sodium dihydrogen phosphate dihydrate, 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of deionized water were mixed together for ball milling, spray dried at 120 ° C after ball milling, and the ground powder was placed in a tube furnace for sintering. The temperature was first raised to 325 ° C at a rate of 5 ° C / min in a nitrogen atmosphere, and kept warm for 20 min, and then raised to 650 ° C at a rate of 1 ° C / min, kept warm for 8 h, and cooled to obtain the sodium iron pyrophosphate positive electrode material Na 3.9 Fe3(PO4)2(P2O7) / C.
[0056] Comparative Example 3 is basically the same as Example 1, except that the heating rate in the first stage of sintering is
[0057] 15.4 g of sodium carbonate, 54.2 g of ferric phosphate dihydrate, 17.2 g of sodium dihydrogen phosphate dihydrate, 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of deionized water were mixed together for ball milling, spray dried at 120 ° C after ball milling, and the ground powder was placed in a tube furnace for sintering. In a nitrogen atmosphere, the temperature was first increased to 325 ° C at a rate of 3 ° C / min, and kept warm for 20 min, and then increased to 650 ° C at a rate of 1 ° C / min, kept warm for 8 h, and cooled to obtain the sodium iron pyrophosphate positive electrode material Na4Fe 2.9 (PO4)2(P2O7) / C.
[0058] Comparative Example 4 is basically the same as Example 1, except that the heating rate in the first stage of sintering is
[0059] 15.4 g of sodium carbonate, 54.2 g of ferric phosphate dihydrate, 17.2 g of sodium dihydrogen phosphate dihydrate, 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of deionized water were mixed together for ball milling, and then spray dried at 120 ° C. The ground powder was placed in a tube furnace for sintering, and heated to 325 ° C at a rate of 8 ° C / min in a nitrogen atmosphere, and kept warm for 20 min, and then heated to 650 ° C at a rate of 1 ° C / min, kept warm for 8 h, and cooled to obtain sodium iron pyrophosphate positive electrode material Na4Fe 2.9 (PO4)2(P2O7) / C.
[0060] Comparative Example 5 is basically the same as Example 1, except that the sintering temperature in the first stage of sintering is
[0061] 15.4 g of sodium carbonate, 54.2 g of ferric phosphate dihydrate, 17.2 g of sodium dihydrogen phosphate dihydrate, 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of deionized water were mixed together for ball milling, spray dried at 120 ° C after ball milling, and the ground powder was placed in a tube furnace for sintering. In a nitrogen atmosphere, the temperature was first increased to 275 ° C at a rate of 5 ° C / min, and kept warm for 20 min, and then increased to 650 ° C at a rate of 1 ° C / min, kept warm for 8 h, and cooled to obtain the sodium iron pyrophosphate positive electrode material Na4Fe 2.9 (PO4)2(P2O7) / C.
[0062] Comparative Example 6 is basically the same as Example 1, except that the sintering temperature in the first stage of sintering is
[0063] 15.4 g of sodium carbonate, 54.2 g of ferric phosphate dihydrate, 17.2 g of sodium dihydrogen phosphate dihydrate, 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of deionized water were mixed together for ball milling, spray dried at 120 ° C after ball milling, and the powder obtained by grinding was placed in a tube furnace for sintering. In a nitrogen atmosphere, the temperature was first increased to 400 ° C at a rate of 5 ° C / min, and kept warm for 20 min, and then increased to 650 ° C at a rate of 1 ° C / min, kept warm for 8 h, and cooled to obtain the sodium iron pyrophosphate positive electrode material Na4Fe 2.9 (PO4)2(P2O7) / C.
[0064] Comparative Example 7 is basically the same as Example 1, except that the holding time of the first stage of sintering is
[0065] 15.4 g of sodium carbonate, 54.2 g of ferric phosphate dihydrate, 17.2 g of sodium dihydrogen phosphate dihydrate, 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of deionized water were mixed together for ball milling, and then spray dried at 120 ° C. The ground powder was sintered in a tube furnace, and heated to 325 ° C at a rate of 5 ° C / min in a nitrogen atmosphere, and kept warm for 5 min, and then heated to 650 ° C at a rate of 1 ° C / min, kept warm for 8 h, and cooled to obtain sodium iron pyrophosphate positive electrode material Na4Fe 2.9 (PO4)2(P2O7) / C.
[0066] Comparative Example 8 is basically the same as Example 1, except that the holding time of the first stage of sintering is
[0067] 15.4 g of sodium carbonate, 54.2 g of ferric phosphate dihydrate, 17.2 g of sodium dihydrogen phosphate dihydrate, 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of deionized water were mixed together for ball milling, and then spray dried at 120 ° C. The ground powder was sintered in a tube furnace, and heated to 325 ° C at a rate of 5 ° C / min in a nitrogen atmosphere, and kept warm for 45 min, and then heated to 650 ° C at a rate of 1 ° C / min, kept warm for 8 h, and cooled to obtain sodium iron pyrophosphate positive electrode material Na4Fe 2.9 (PO4)2(P2O7) / C.
[0068] Verification Example
[0069] According to the relationship between the resistivity R and x and y of the sodium iron pyrophosphate positive electrode materials of Examples 1-5 and Comparative Examples 1-8, data fitting was performed to obtain the following relationship: The function shows that when x=0.076, y=0.144, the resistivity is the lowest, which is 1674Ω·cm. This is verified:
[0070] 14.52g sodium carbonate, 52.3g ferric phosphate dihydrate, 17.46g sodium dihydrogen phosphate dihydrate, 7.0g glucose, 1.7g polyethylene glycol and 120.0g deionized water were mixed together for ball milling, spray dried at 120°C after ball milling, and the powder obtained by grinding was placed in a tube furnace for sintering, and heated to 325°C at a rate of 5°C / min in a nitrogen atmosphere, and kept warm for 20min, and then heated to 650°C at a rate of 1°C / min, kept warm for 8h, and cooled to obtain a low resistivity sodium iron pyrophosphate positive electrode material Na 3.924 Fe 2.856 (PO4)2(P2O7) / C.
[0071] Test Example: Battery production and performance testing based on the sodium iron pyrophosphate positive electrode materials of Examples 1-5 and Comparative Examples 1-8
[0072] Sodium ion battery production:
[0073] Positive electrode sheet: The sodium iron pyrophosphate positive electrode materials of Examples 1-5 and Comparative Examples 1-8, super P and polyvinylidene fluoride were mixed at a mass ratio of 8:1:1, N-methylpyrrolidone was added and stirred to obtain a positive electrode active slurry, the positive electrode active slurry was evenly coated on the surface of the aluminum foil current collector, and a 200 μm blade coating was performed to prepare a pole sheet, and a positive electrode sheet was obtained after drying and cold pressing. The mass loading of the active material was about 2.5 mg / cm 2 ;
[0074] Negative electrode: metallic sodium sheet;
[0075] Separator: PE separator with a thickness of 9 μm;
[0076] Electrolyte: Sodium hexafluorophosphate was dissolved in ethylene carbonate at a concentration of 1 mol / L;
[0077] Sodium ion battery assembly: Arrange the positive electrode sheet, separator, negative electrode sheet and separator in sequence, and use winding as the assembly method.
[0078] Performance Test:
[0079] Charge / discharge test: The battery is charged / discharged at a rate of 0.1C in the voltage range of 1.5V-4.2V.
[0080] Band gap Eg (eV) test: The band gap width (band gap) of the obtained sodium titanium phosphate composite material can be calculated by UV-visible diffuse reflection test, and the band gap can be calculated by the intercept method, Eg (eV) = hc / λg = 1240 / λg (nm).
[0081] Resistivity R (Ω·cm) test: The ST2742C automatic powder resistivity tester was used to measure the powder resistivity of the sodium titanium phosphate composite material. Under the condition of the same carbon content, the electronic conductivity of the sodium titanium phosphate composite material can be directly reflected, and the curve between pressure (MPa) and resistivity (Ω·cm) is recorded. The resistivity at a pressure of 60MPa is used as a comparison between different samples.
[0082] Figure 1-Figure 8 Table 1 shows the relevant performance parameters finally measured:
[0083] Table 1
[0084]
[0085]
[0086] from Figure 1-Figure 8 As can be seen from Table 1, by adjusting the number and relationship of Fe defects and Na vacancies, while ensuring that the number of Fe defects is slightly larger than the number of Na vacancies, and combining appropriate heating rate, holding temperature and holding time, the phosphate (PO4 3- ) and pyrophosphate (P2O7 4- ) conversion efficiency, the band gap Eg of the sodium iron pyrophosphate positive electrode material can be achieved to be less than 2.7eV, and the resistivity is less than 2000Ω·cm. Under the optimal sintering conditions, the formula with the lowest resistivity is deduced through the relationship between x, y and the powder resistivity in the example, and verified. The deviation between the result of the verification example and the predicted value is only 1.25%, which can judge the accuracy of this prediction method.
[0087] It can be seen from Examples 1-3 and Comparative Examples 1-2 that the chemical formula Na 4-x Fe 3-y When x<y in (PO4)2(P2O7) / C, it can ensure that the material has a certain amount of Fe defects and Na vacancies, and the number of Fe defects is slightly greater than the number of Na vacancies, which is beneficial to reduce the Na ion diffusion barrier and widen the Na ion diffusion channel; the appropriate heating rate makes the phosphate (PO4 3- ) and pyrophosphate (P2O7 4- ) is more completely converted, while the completely converted pyrophosphate (P2O7 4- ) has a higher electronegativity, thereby increasing the energy density. When x ≥ y, a Na-poor structure will be formed during the sintering process, and the Fe element will be excessive, forming a large amount of pyrophosphate phase NaFePO4, which has a large band gap and low conductivity, resulting in an excessively large overall band gap of the material.
[0088] It can be seen from Example 1 and Comparative Examples 3-4 that even if the material ratio satisfies x<y, when the heating rate of the first stage is lower than 5°C / min, FePO4 is converted into inactive glass phase FePO4 during the sintering process, and ultimately active sodium iron pyrophosphate cannot be generated, resulting in a sharp decrease in the specific capacity of the material; when the heating rate of the first stage is higher than 7°C / min, phosphate (PO4 3- ) is not able to be converted into pyrophosphate (P2O7 4- ), a large amount of NaFePO4 phase with olivine structure and no electrochemical activity will be generated, resulting in a decrease in specific capacity.
[0089] It can be seen from Examples 1, 4-5 and Comparative Examples 5-6 that the sintering temperature of the first stage is the thermodynamic basis for determining whether phase formation can occur. When the sintering temperature of the first stage is lower than 300°C, acid radical (PO4 3- ) to pyrophosphate (P2O7 4- ) will generate the NaFePO4 phase with no electrochemical activity, and the specific capacity will decrease; when the sintering temperature of the first stage is greater than 350℃, the pyrophosphate will continue to dehydrate to generate polymetaphosphoric acid with a ring structure, which cannot react with Na and Fe elements to generate active substances.
[0090] It can be seen from Example 1 and Comparative Examples 7-8 that the first stage of the heat preservation time is also an important parameter index, and it is related to the acid radical (PO4 3- ) to pyrophosphate (P2O7 4- ) is closely related to the conversion amount. The insulation time is a necessary condition to ensure sufficient diffusion inside the material. Even if the temperature is appropriate, it is difficult to complete the conversion of acid radical (PO4 3- ) to pyrophosphate (P2O7 4- ) conversion, so the specific capacity of comparative example 7 is lower; when the insulation time is too long, the pyrophosphate will continue to dehydrate to form a cyclic polymetaphosphoric acid, and the cyclic polymetaphosphoric acid cannot react with Na and Fe elements to form active substances.
[0091] Therefore, the ratio of Na and Fe and the sintering conditions in the first stage are two indicators that restrict and influence each other and need to be considered comprehensively to achieve the best performance.
[0092] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A low resistivity sodium iron pyrophosphate positive electrode material, characterized in that: The chemical formula of the low resistivity sodium iron pyrophosphate positive electrode material is Na 4-x Fe 3-y (PO4)2(P2O7) / C, 0≤x≤1, 0≤y≤1, x<y.
2. The low resistivity sodium iron pyrophosphate positive electrode material according to claim 1, characterized in that: The band gap Eg of the low-resistivity sodium iron pyrophosphate positive electrode material is less than 2.7 eV.
3. The low resistivity sodium iron pyrophosphate positive electrode material according to claim 1, characterized in that: The resistivity R of the low-resistivity sodium iron pyrophosphate positive electrode material satisfies the following relationship: 0≤x≤1, 0≤y≤1, x<y.
4. A method for preparing the low resistivity sodium iron pyrophosphate positive electrode material according to any one of claims 1 to 3, characterized in that: The following steps are involved: The sodium source, iron source, phosphorus source, carbon source and water are uniformly mixed, and the low resistivity sodium iron pyrophosphate positive electrode material is obtained through ball milling, spray drying and sintering.
5. The method for preparing the low resistivity sodium iron pyrophosphate positive electrode material according to claim 4, characterized in that: The sodium source is selected from one or more of sodium carbonate, sodium hydroxide, sodium sulfate and sodium dihydrogen phosphate; the iron source is selected from one or more of ferric acetate, ferric nitrate, ferrous oxalate, ferric oxide and ferric phosphate; the phosphorus source is selected from one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium dihydrogen phosphate and phosphorus pentoxide; the carbon source is selected from one or more of carbon black, graphite, acetylene black, activated carbon, citric acid, polyethylene glycol, sucrose and glucose.
6. The method for preparing the low resistivity sodium iron pyrophosphate positive electrode material according to claim 4, characterized in that: The spray drying temperature is 100°C-140°C.
7. The method for preparing the low resistivity sodium iron pyrophosphate positive electrode material according to claim 4, characterized in that: The sintering is carried out under a protective atmosphere and is divided into two stages; the first stage is to heat up to 300°C-350°C at a rate of 5°C / min-7°C / min and keep warm for 10min-30min; the second stage is to heat up to 600°C-750°C at a rate of 0.5°C / min-2°C / min and keep warm for 5h-10h.
8. The method for preparing the low resistivity sodium iron pyrophosphate positive electrode material according to claim 7, characterized in that: The protective atmosphere is selected from a nitrogen atmosphere or an argon atmosphere.
9. A sodium ion battery positive electrode, characterized in that: The invention comprises the low-resistivity sodium iron pyrophosphate positive electrode material according to any one of claims 1 to 3 or the low-resistivity sodium iron pyrophosphate positive electrode material prepared by the method according to any one of claims 4 to 8.
10. A sodium ion battery, characterized in that: Including the sodium ion battery positive electrode as described in claim 9.
Citation Information
Patent Citations
Na4Fe3-x(PO4)2P2O7 / C sodium ion battery positive electrode material as well as preparation method and application thereof
CN112768673A
Sodium-ion battery positive electrode material and preparation method thereof
CN115986080A
Carbon-coated ferric sodium pyrophosphate positive electrode material as well as preparation method and application thereof
CN116230923A
Sodium-rich sodium ferric phosphate positive electrode material and preparation method and application thereof
CN116332144A
Carbon composite pyrophosphoric acid and sodium ferric phosphate composite material, preparation thereof and application of composite material in sodium ion battery
CN116487545A
Cited By
Sodium-supplementing Na4Fe3-a (PO4) 2P2O7 composite positive electrode material, preparation thereof and application of sodium-supplementing Na4Fe3-a (PO4) 2P2O7 composite positive electrode material in sodium ion battery
CN120072931A
In-situ doped composite sodium ferric phosphate positive electrode material, preparation method thereof and sodium ion battery
CN120288732A
Sodium ferric phosphate pyrophosphate positive electrode material and preparation method thereof
CN121202102A
Sodium ferric phosphate pyrophosphate positive electrode material cooperatively regulated by using defects of Na3PO4 and Fe3 (PO4) 2 and preparation method of sodium ferric phosphate pyrophosphate positive electrode material
CN121269670A
Low-band-gap ferric sodium pyrophosphate positive electrode material as well as preparation method and application thereof
CN121376950A