Pettringite self-assembly ordered material, preparation and application of ettringite self-assembly ordered material
Preparing ettringite bulk materials through a self-assembly method solves the problems of low application efficiency and powdery state of ettringite materials, achieves lightweight, high strength and high energy storage density, expands application scenarios, and plays an important role in phase change energy storage. Materials exhibit excellent properties.
Patent Information
- Application Number
- CN202410723167.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-18
AI Technical Summary
The existing ettringite materials have low application efficiency, are mostly in powder state, lack deep processing, have no mechanical functional properties, and have limited application scenarios.
Preparation of ettringite self-assembled ordered materials through self-assembly method, using aluminum sulfate octahydrate and calcium hydroxide powder to stir in deionized water to form nano ettringite, and dried in a mold into a bulk material with a temperature of more than 10MPa Compressive strength and high phase change energy storage density.
It has achieved the lightweight, high-strength, and high energy storage density characteristics of the vanadium material, expanded its application scope, and demonstrated good interfacial compatibility and energy storage performance in phase change energy storage materials and concrete.
Smart Images

Figure CN118791241A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of phase-change energy storage materials, and in particular to an ordered self-assembled calcium vanadium material, and its preparation and application. Background Art
[0002] Calcium vanadate (trisulfur hydrated calcium sulfoaluminate) is widely present in natural minerals and various cement-based materials. Its chemical expression is 3CaO·Al2O3·3CaSO4·32H2O, and it mostly exists in the form of needle-shaped crystals. The existence of calcium vanadate is greatly affected by environmental factors and is sensitive to temperature, humidity, solution ion conditions, etc. When the ambient temperature is higher than 70°C, the morphology of calcium vanadate crystals becomes fine, unstable and easy to decompose. When it is higher than 95°C, there are documents showing that calcium vanadate no longer exists in the cement environment. The study of the morphological transformation and stability of calcium vanadate is of great significance to many building materials, and the phase transition behavior of calcium vanadate at low temperature (50-150°C) can also be used in phase change energy storage materials, mainly using sulfoaluminate cement to prepare cement-based materials containing calcium vanadate products as energy storage carriers. For example, in patent CN114777543 A, a block with calcium vanadate as the main hydration product was prepared by sulfoaluminate cement and gypsum as an energy storage sheet, which was applied to a civil thermal storage system based on phase change thermal storage. Patent CN 114804790 A uses sulphoaluminate cement as raw material to prepare an ettringite-based energy storage foam lightweight soil, which is applied to road energy storage to melt ice and snow.
[0003] In addition to the calcium vanadate generated in nature or cement, there are also artificial synthetic methods to form calcium vanadate for research and application, including the use of a single ore for hydration reaction or solution reaction method. The single ore reaction method usually uses calcium aluminate or calcium sulfoaluminate to react in the presence of gypsum. The solution reaction method is to react with Ca(OH)2 plus Al2(SO4)3·18H2O, or Ca(OH)2 plus Al2(OH)3 plus gypsum. Regardless of the method of generation, the calcium vanadate obtained after drying is in a powder state or a suspension state, which can be used in cement-based materials, sewage or solid waste treatment and other fields. Patent CN 115305574 A uses phosphogypsum and brine to quickly prepare calcium vanadate whiskers. Patent CN116041016 A uses calcium sulfoaluminate cement to generate calcium vanadate whiskers, which are added to anti-seepage inorganic spray materials to promote silicate hydration. Patent CN 114751701A uses ettringite whiskers and polyvinyl alcohol fibers in combination to improve the toughness of cement-based materials.
[0004] At present, the application of ettringite as the main component has the following two limitations: 1. With cement concrete as the main body, ettringite as a hydration product is only used as a partial component, and the efficiency is limited. For example, in patent CN 114777543 A, ettringite as an energy storage material accounts for <50% of the total material. 2. Products using pure ettringite materials as applications are all powder materials, such as patents CN113213803A and CN113277809A, etc., and no further deep processing has been seen, and no ettringite blocks have been seen, making it difficult to prepare functional devices, and the application scenarios are limited.
[0005] Ordering the material can significantly enhance the various properties of the material, such as excellent mechanical strength or thermoelectric properties, and enable the material to achieve the designed target form. Patent CN 117447844 A uses a magnetic field to prepare a highly ordered asphalt-based chopped carbon fiber composite material with excellent vertical thermal conductivity. Patent CN115839031A prepares a conductive polymer composite electrode material with an ordered array structure through electropolymerization self-catalytic growth, which greatly improves the structural stability of the electrode. However, there is currently no ordered treatment of calcium vanadium materials. Summary of the invention
[0006] Technical issues:
[0007] In view of the technical problems in the prior art such as low application efficiency of calcium vanadate materials, mostly in powder state, lack of deep processing, no mechanical functional characteristics, and limited application scenarios, the purpose of the present invention is to provide a calcium vanadate self-assembled ordered material, a preparation method and its application. Among them, the calcium vanadate material is ordered by self-assembly to make the calcium vanadate material have the characteristics of light weight, high strength and high energy storage density, which greatly expands its application range. And based on the prepared ordered calcium vanadate material, it is applied to many scenarios such as high-density phase change energy storage materials and phase change aggregates.
[0008] Technical solution:
[0009] In order to achieve the above-mentioned purpose, the present invention is implemented by the following technical solutions:
[0010] A self-assembled ordered material of calcium vanadate, which is formed by stacking ordered calcium vanadate crystal particles. It is a white low-density block, hard, with a compressive strength of more than 10MPa. The size and shape can be designed as needed. The maximum diameter of the block ranges from 1mm to 50mm. It has a high phase transition energy storage density and high adaptability to cement-based materials.
[0011] The method for preparing the calcium vanadium self-assembled ordered material comprises the following steps:
[0012] (1) Add aluminum sulfate 18hydrate and calcium hydroxide powder into deionized water and stir thoroughly;
[0013] (2) centrifuging the product obtained in the previous step, removing the supernatant to obtain a milky white suspension or a milky white paste, and washing it twice with deionized water, centrifuging to remove the supernatant each time, and finally obtaining a milky white suspension or paste, which is nano-ettringite (containing water);
[0014] (3) The nano-ettringite (containing water) is placed in a mold and dried. After the mass remains unchanged and the material is completely dried, an ordered self-assembled ettringite material is formed. The material is a block material with white color and hard texture. The size and shape can be determined by the mold as needed. The maximum diameter of the block ranges from 1 mm to 200 mm.
[0015] In step (1), aluminum sulfate 18hydrate and calcium hydroxide powder are reacted in a mass ratio of 3:2 under the condition of a water-to-solid ratio of 30-100.
[0016] The stirring speed of step (1) is 200-500 r / min, and the reaction is carried out in a water bath environment at 20-30° C. for 24 hours to 48 hours.
[0017] Step (3) drying is carried out by natural drying, forced air drying or vacuum drying at 20-70°C.
[0018] The application of the calcium vanadium self-assembled ordered material in phase change energy storage materials.
[0019] The calcium vanadium self-assembled ordered material is directly encapsulated and processed and used as an energy storage module in the energy storage system.
[0020] The phase change concrete is prepared by adding the ordered self-assembled calcium vanadium material as a phase change component to replace part of the aggregate, and the adding amount is 10-40% of the original volume of the aggregate.
[0021] Beneficial effects:
[0022] (1) This application realizes the ordered morphology of ettringite for the first time through self-assembly, and the ordered ettringite block material obtained thereby makes the use of pure ettringite break through the application form of powder.
[0023] (2) The self-assembled ordered material of calcium vanadium is light and high-strength, and the size and shape of the block material can be freely designed according to the mold; it is easy to produce and process, and can be produced using industrial-grade products at a low cost.
[0024] (3) Calcium vanadium self-assembled ordered materials have the characteristics of high energy storage density. Compared with ordinary calcium vanadium materials, the storable phase change energy density is higher, and they have good application in phase change energy storage materials.
[0025] (4) The self-assembled ordered material of calcium vanadium has very good interfacial compatibility with cement-based materials, and is effective in replacing aggregates. The prepared phase change energy storage mortar or concrete has no loss in strength.
[0026] (5) When calcium vanadium self-assembled ordered materials are used as blocks to replace aggregates to prepare energy storage mortar or concrete, phase change energy storage can be accurately calculated and designed, which is conducive to the preparation of refined and customized products, and is also conducive to the systematic design of phase change energy storage. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Table 1 shows the compressive strength and density of the calcium vanadium self-assembled ordered material block.
[0028] Table 2 shows the heat transfer and storage performance of the calcium vanadium self-assembled ordered material block.
[0029] Figure 1 This is a photo of a self-assembled ordered block of calcium vanadium.
[0030] Figure 2 This is a magnified electron microscope photo of the self-assembled ordered material of calcium vanadium.
[0031] Figure 3 Phase transition enthalpy measurements for self-assembled ordered materials as calcium vanadium.
[0032] Figure 4 This is the 28d strength effect diagram of mortar using calcium vanadium self-assembled ordered materials as alternative aggregate. DETAILED DESCRIPTION
[0033] The technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. In this application, unless otherwise specified, all percentage contents are mass percentages.
[0034] A self-assembled ordered ettringite material, which is formed by stacking ordered ettringite crystal particles, is blocky, hard, and has a compressive strength of more than 10MPa.
[0035] A method for preparing a self-assembled ordered material of calcium vanadium comprises the following steps:
[0036] (1) Aluminum sulfate 18hydrate and calcium hydroxide powder are added into deionized water at a mass ratio of 3:2, and stirred in a reactor with a stirring paddle driven by a motor at a water-to-solid ratio of 30-100 at a stirring speed of 200-500 r / min, and reacted in a water bath environment at 20-30° C. for 24 hours to 48 hours;
[0037] (2) centrifuging the product obtained in the previous step at a speed of 2000-9000 r / min, removing the supernatant to obtain a milky white suspension or a milky white paste, and washing it twice with deionized water, centrifuging to remove the supernatant each time, and finally obtaining a milky white suspension or paste, which is nano-ettringite (containing water);
[0038] (3) The nano-ettringite (containing water) is placed in a mold and dried naturally, by forced air drying or by vacuum drying at 20-70° C. After being thoroughly dried without changing its quality, an ettringite self-assembled ordered material is formed, which is a block material with white color and hard texture. The size and shape can be determined by the mold as needed, and the maximum diameter of the block ranges from 1 mm to 200 mm.
[0039] Applications of a calcium vanadium self-assembled ordered material include but are not limited to:
[0040] (1) High-density phase change energy storage material: The obtained calcium vanadium self-assembled ordered block material can be made into a specified size according to demand and can be directly used as an energy storage module in the energy storage system
[0041] (2) Phase change concrete: The obtained calcium vanadium self-assembled ordered block material is made into continuous particle size particles of 0.15-5 mm as needed to replace the fine aggregate in sulphoaluminate, silicate concrete or mortar to prepare phase change energy storage concrete or phase change energy storage mortar.
[0042] Embodiment 1:
[0043] (1) Aluminum sulfate 18hydrate and calcium hydroxide powder are added into deionized water at a mass ratio of 3:2, and stirred in a reactor with a stirring paddle driven by a motor at a water-to-solid ratio of 30-100 at a stirring speed of 200-500 r / min, and reacted in a water bath environment at 20-30° C. for 24 hours to 48 hours;
[0044] (2) centrifuging the product obtained in the previous step at a speed of 2000-5000 r / min, removing the supernatant to obtain a milky white suspension or a milky white paste, and washing it twice with deionized water, centrifuging to remove the supernatant each time, and finally obtaining a milky white suspension or paste, which is nano-ettringite (containing water);
[0045] (3) The nano-ettringite (containing water) is placed into 40*40*40mm and 300mm*200mm*40mm molds, and is dried naturally, by forced air drying or by vacuum drying at 20-70°C. After being thoroughly dried without changing the quality, an ettringite self-assembled ordered material is formed, which is a block material with white color and hard texture, and a maximum length of about 200mm.
[0046] The calcium vanadium self-assembled ordered material obtained above was further trimmed to obtain a 20*20*20 cubic block.
[0047] Embodiment 2:
[0048] (1) Aluminum sulfate 18hydrate and calcium hydroxide powder are added into deionized water at a mass ratio of 3:2, and stirred in a reactor with a stirring paddle driven by a motor at a water-to-solid ratio of 30-100 at a stirring speed of 200-500 r / min, and reacted in a water bath environment at 20-30° C. for 24 hours to 48 hours;
[0049] (2) centrifuging the product obtained in the previous step at a speed of 2000-5000 r / min, removing the supernatant to obtain a milky white suspension or a milky white paste, and washing it twice with deionized water, centrifuging to remove the supernatant each time, and finally obtaining a milky white suspension or paste, which is nano-ettringite (containing water);
[0050] (3) The nano-ettringite (containing water) is placed into a 20*20*20 mm cubic mold, and is dried naturally, by forced air drying or by vacuum drying at 20-70° C. After being thoroughly dried without changing its quality, an ettringite self-assembled ordered material is formed, which is a block material with white color and hard texture, and a maximum length of about 8 mm.
[0051] The obtained calcium vanadium self-assembled ordered material was crushed and sieved using a mortar, and passed through a 200-mesh sieve to obtain a powder.
[0052] Embodiment 3:
[0053] (1) Aluminum sulfate 18hydrate and calcium hydroxide powder are added into deionized water at a mass ratio of 3:2, and stirred in a reactor with a stirring paddle driven by a motor at a water-to-solid ratio of 30-100 at a stirring speed of 200-500 r / min, and reacted in a water bath environment at 20-30° C. for 24 hours to 48 hours;
[0054] (2) centrifuging the product obtained in the previous step at a speed of 2000-5000 r / min, removing the supernatant to obtain a milky white suspension or a milky white paste, and washing it twice with deionized water, centrifuging to remove the supernatant each time, and finally obtaining a milky white suspension or paste, which is nano-ettringite (containing water);
[0055] (3) The nano-ettringite (containing water) is placed into a 40*40*40 mm cubic mold, and is dried naturally, by forced air drying or by vacuum drying at 20-70° C. After being thoroughly dried without changing its quality, an ettringite self-assembled ordered material is formed, which is a block material with white color and hard texture, and a maximum length of about 25 mm.
[0056] The obtained calcium vanadium self-assembled ordered material is crushed and sieved to obtain an irregular block material with a continuous gradation of 0.15-5 mm.
[0057] Test Example 1: Morphological characteristics, density and compressive strength test of calcium vanadium self-assembled ordered materials
[0058] The large block material in Example 1 was observed to be a white, light, hard block with a maximum size of about 200 mm. Figure 1 .
[0059] The density and compressive strength of the block material in Example 1 were tested, and the crushed samples were sprayed with gold and observed by scanning electron microscope. The results are shown in Table 1 and Figure 2 .
[0060] Table 1 Appearance and physical and mechanical properties of calcium vanadium self-assembled ordered materials
[0061] Appearance Compressive strength density White block 10.5±0.3MPa <![CDATA[0.79g / cm 3 ]]>
[0062] From Appendix 1, it can be seen that the density of the calcium vanadium self-assembled ordered material is 0.79 g / cm3, and the compressive strength is 10.5±0.3 MPa. It is light and high-strength, and fully meets the conditions for further processing of bulk materials.
[0063] By the attached Figure 2 It can be observed that the ettringite crystals have formed an ordered structure through the self-assembly process, so that they can have sufficient interaction force to become a bulk material. At present, no other materials that have been processed to order the ettringite crystals have been found, nor have ettringite bulk materials been found.
[0064] Test Example 2: Thermal Conductivity and Heat Storage Performance Test of Calcium Vanadium Self-Assembled Ordered Materials
[0065] The heat transfer performance of the bulk material in Example 2 was tested. The thermal conductivity and specific heat capacity of the calcium vanadium self-assembled ordered material were tested using a multifunctional rapid thermal conductivity tester. The results are shown in Appendix 2.
[0066] Table 2 Thermal properties of calcium vanadium self-assembled ordered materials
[0067] Thermal conductivity Specific heat 0.22W / (m*K) 1.43KJ / (Kg*K)
[0068] The powder material in Example 2 was tested for its heat storage performance. The phase transition enthalpy of the calcium vanadium self-assembled ordered material between 50 and 150 °C was tested by differential scanning calorimetry. Figure 3As shown, it is 595.2J / g, the energy storage density of the bulk material is 166Wh / kg, and the power density is about 1kW / kg. Because the material is composed of pure calcium vanadate, the heat storage and heat release performance is better than the calcium vanadate energy storage related patents CN 114804790 A and CN 114777543 A, and the energy storage density is close to the level of lithium-ion monomer batteries ("Lithium-ion Battery Industry Standard Conditions (2021 Edition)" Energy storage battery energy density ≥ 145Wh / kg). This data shows that calcium vanadate self-assembled ordered materials have excellent phase change energy storage potential. And because its phase change is a solid-solid phase change, the bulk morphology can be maintained before and after the phase change, and it can be used in a wide range of scenarios.
[0069] Test Example 3: Calcium vanadate self-assembled ordered materials for phase change aggregate testing
[0070] The block material in Example 3 was substituted for the aggregate in the original mortar at a replacement rate of 30%. The mortar strength was measured 28 days after the mortar was formed. The results are shown in the attached Figure 4 As shown. It can be seen that although the strength of the calcium vanadium self-assembled ordered material itself is lower than that of the standard sand aggregate, due to the good interface characteristics, the 28d strength is similar to or even slightly improved from the control group. Compared with the phase change aggregates in the existing patents, there is no need for high-priced organic phase change materials such as paraffin (CN115594433A) and fatty acid ternary eutectic (CN116354635A), no need for complex impregnation and encapsulation processes (CN116119959A, CN115594433A, CN113185181A), no need to consider the leakage of phase change materials caused by stirring (CN107379244A), and no need to worry about weak interface problems (CN116119959A). The calculated phase change heat storage capacity of this mortar is about 130 J / g, which is higher than the existing phase change mortars such as CN116119959A (15.3 J / g) and CN115594433A (phase change aggregate 40-70 J / g). This example shows that it is completely feasible to prepare phase change mortar or concrete using calcium vanadium self-assembled ordered materials as phase change aggregates.
[0071] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A self-assembled ordered material of calcium vanadium, characterized in that: The material is made of ordered stacked calcium sulfonate crystal particles. It is a white, low-density block that is hard and has a compressive strength of more than 10MPa. The size and shape can be designed as needed. The maximum diameter of the block ranges from 1mm to 50mm. It has a high phase change energy storage density and is highly compatible with cement-based materials.
2. The method for preparing a self-assembled ordered calcium vanadium material according to claim 1, characterized in that: The method comprises the following steps: (1) adding aluminum sulfate 18hydrate and calcium hydroxide powder into deionized water and stirring them thoroughly; (2) centrifuging the product obtained in the previous step, removing the supernatant to obtain a milky white suspension or a milky white paste, and washing it twice with deionized water, centrifuging to remove the supernatant each time, and finally obtaining a milky white suspension or paste, which is nano-ettringite (containing water); (3) The nano-ettringite (containing water) is placed in a mold and dried. After the mass remains unchanged and the material is completely dried, an ordered self-assembled ettringite material is formed. The material is a block material with white color and hard texture. The size and shape can be determined by the mold as needed. The maximum diameter of the block ranges from 1 mm to 200 mm.
3. The method for preparing a self-assembled ordered material of calcium vanadium according to claim 2, characterized in that: In step (1), aluminum sulfate 18hydrate and calcium hydroxide powder are reacted in a mass ratio of 3:2 under the condition of a water-to-solid ratio of 30-100.
4. The method for preparing a self-assembled ordered material of calcium vanadium according to claim 2, characterized in that: The stirring speed of step (1) is 200-500 r / min, and the reaction is carried out in a water bath environment at 20-30° C. for 24 hours to 48 hours.
5. The method for preparing a self-assembled ordered material of calcium vanadium according to claim 2, characterized in that: Step (3) drying is carried out by natural drying, forced air drying or vacuum drying at 20-70°C.
6. Use of the calcium vanadium self-assembled ordered material according to claim 1 in phase change energy storage materials.
7. The use according to claim 6, characterized in that: The calcium vanadium self-assembled ordered material is directly encapsulated and processed and used as an energy storage module in the energy storage system.
8. The use according to claim 6, characterized in that: The phase change concrete is prepared by adding the ordered self-assembled calcium vanadium material as a phase change component to replace part of the aggregate, and the adding amount is 10-40% of the original volume of the aggregate.