Optical fiber and optical fiber preparation method
By dividing the annular doping area in the optical fiber and rationally designing the refractive index, reducing local stress, and combining the high flexibility and high hardness coating design, the problem of coating peeling off of the polarization-maintaining optical fiber is solved, and the reliability and reliability of the optical fiber are improved. stability.
Patent Information
- Application Number
- CN202410774110.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-14
AI Technical Summary
When the existing polarization-maintaining optical fiber is wound and used, its outer coating is easy to fall off, affecting the performance of the optical fiber.
Design an optical fiber structure in which the core is wrapped in a cladding. The cladding is divided into multiple annular doped regions. The refractive index of the core and doped regions is reasonably designed to reduce local stress and avoid coating. fall off. The coating is made of acrylic resin, with the first coating having high flexibility and the second coating having high hardness to improve bonding strength.
Through uniform stress distribution and high-quality coating design, the reliability and service life of the optical fiber are improved, coating shedding is avoided, and the stability of the optical fiber and signal transmission quality are enhanced.
Smart Images

Figure CN118795593A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of optical fibers, and in particular to an optical fiber and a method for preparing the optical fiber. Background Art
[0002] The full name of polarization-maintaining fiber is polarization-maintaining fiber. Its principle is to maintain the polarization state of light transmission by artificially increasing stress birefringence. The main method is to artificially set a stress area in the optical fiber to increase the birefringence coefficient of the optical fiber to maintain the polarization state of light when it is transmitted in the optical fiber. Polarization-maintaining optical fiber can be divided into panda-type, butterfly-type, bow-tie-type, elliptical core-type, etc. according to its structure.
[0003] In the prior art, polarization-maintaining optical fiber is usually used as an optical fiber gyroscope. The optical fiber needs to be wound before use. However, when the existing polarization-maintaining optical fiber is wound for use, its outer coating is prone to fall off. Summary of the invention
[0004] In order to solve at least one of the problems mentioned in the background technology, the present invention provides an optical fiber and an optical fiber preparation method, and the optical fiber coating is not easy to fall off.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] In a first aspect, the present invention provides an optical fiber, comprising a core, a cladding, a stress layer and a coating, wherein the cladding is coated on the outside of the core, the stress layer is embedded in the cladding, there are two stress layers, the two stress layers are evenly arranged around the periphery of the core, and the coating is coated on the outside of the cladding;
[0007] The radius a of the fiber core is 2.75 μm to 3.25 μm, and the relative refractive index difference Δn1 of the fiber core is 0.5% to 1%;
[0008] The radius b of the cladding is 39 μm to 41 μm. In the radial direction of the cladding, the cladding includes a plurality of annular doped regions in a concentric circle structure. The annular doped regions include a first annular region. The first annular region surrounds the outside of the fiber core. The relative refractive index difference Δn2 of the first annular region is -0.1% to 0.3%. The outer circle radius r2 of the first annular region and the inner circle outer diameter r1 of the first annular region satisfy the following relationship:
[0009] (r2-r1)≤3μm
[0010] The relative refractive index difference is the difference between the refractive index of the target area on the optical fiber and the refractive index of silica.
[0011] As an optional embodiment, the ratio of the distance r between the two stress layers to the core radius a is between 3 and 4, the stress layer is doped with B2O3 at a concentration of 17 mol% to 26 mol%, and the value range of (r+t) / b is between 0.7 and 0.85, where t is the diameter of the stress layer.
[0012] As an optional embodiment, the annular doped region further includes a second annular region and a third annular region, the second annular region surrounds the first annular region, the third annular region surrounds the second annular region, and the relative refractive index difference Δn of the second annular region is a Calculated by the following formula:
[0013]
[0014] Among them, Δn3 is the relative refractive index difference of the third annular zone, Δn3 is between -0.1% and -0.5%, r3 is the outer radius of the second annular zone, (r3-r2)≤2.5μm, r4 is the outer radius of the third annular zone, 2μm≤(r4-r3)≤6μm.
[0015] As an optional implementation, the annular doped region further includes a fourth annular region and a fifth annular region, the fourth annular region surrounds the third annular region, the fifth annular region surrounds the fourth annular region, and the relative refractive index difference Δn of the fourth annular region is b Calculated by the following formula:
[0016]
[0017] Among them, Δn4 is the relative refractive index difference of the fifth annular zone, Δn4 is between 0 and -0.2.5%, r5 is the outer circle radius of the fourth annular zone, (r5-r4)≤2.5μm, 1μm≤(r6-r5)≤2.5μm, and r6 is the outer circle radius of the fifth annular zone.
[0018] As an optional embodiment, the annular doped region further includes a sixth annular region, a seventh annular region and an eighth annular region, the sixth annular region surrounds the fifth annular region, the seventh annular region surrounds the sixth annular region, the eighth annular region surrounds the seventh annular region, and the relative refractive index difference Δn of the sixth annular region is c Calculated by the following formula:
[0019]
[0020] Wherein, Δn5 is -0.5% to -1.2%, r7 is the outer radius of the sixth annular zone, 6μm≤(r7-r6)≤12μm;
[0021] Relative refractive index difference Δn of the seventh annular zone d Calculated by the following formula:
[0022]
[0023] Among them, Δn6 is the relative refractive index difference of the eighth annular zone, the value of Δn6 is 0, r8 is the outer circle radius of the seventh annular zone, 7μm≤(r8-r7)≤13μm, 39μm≤(r9-r8)≤41μm, and r9 is the radius of the cladding.
[0024] As an optional implementation, the material of the coating is acrylic resin.
[0025] As an optional embodiment, the coating includes a first coating and a second coating, the first coating is coated outside the cladding, and the second coating is coated outside the first coating, and the first coating uses an acrylic resin with a Young's modulus less than 1.5 MPa and an elongation at break greater than or equal to 130%.
[0026] As an optional implementation, the second coating layer uses an acrylic resin with a Young's modulus of 900 MPa to 1500 MPa, an elongation at break greater than or equal to 10%, and a glass transition temperature of 70° C. to 150° C.
[0027] In a second aspect, the present invention further provides a method for preparing an optical fiber, which is applied to the optical fiber of the first aspect and comprises the following steps:
[0028] Melting the optical fiber preform at a temperature of 800° C. to 2000° C.;
[0029] Drawing the melted optical fiber preform into an optical fiber main body at a speed of 300m / min to 500m / min;
[0030] Applying the first coating to the surface of the optical fiber body at a temperature of 36°C to 44°C;
[0031] Applying the second coating layer on the surface of the first coating layer at a temperature of 25 to 33°C;
[0032] curing the first coating layer and the second coating layer to form an optical fiber;
[0033] Collect the optical fiber onto the fiber collection tray;
[0034] The curing degree of the first coating is 82% to 86%, and the curing degree of the second coating is 88% to 92%.
[0035] As an optional embodiment, before curing the first coating and the second coating to form an optical fiber, the method further includes: performing surface inspection on the optical fiber after the curing treatment, and coating the first coating on the surface of the optical fiber if the inspection fails.
[0036] The optical fiber provided by the present invention comprises a core, a cladding, a stress layer and a coating, wherein the cladding is coated on the outside of the core, the stress layer is embedded in the cladding, there are two stress layers, the two stress layers are evenly arranged around the periphery of the core, and the coating is coated on the outside of the cladding; the radius a of the core is 2.75 μm to 3.25 μm, and the relative refractive index difference Δn1 of the core is 0.5% to 1%; the radius b of the cladding is 39 μm to 41 μm, and in the radial direction of the cladding, the cladding comprises a plurality of annular doped regions in a concentric circle structure, the annular doped regions comprise a first annular region, the first annular region surrounds the outside of the core, the relative refractive index difference Δn2 of the first annular region is -0.1% to 0.3%, and the outer circle radius r2 of the first annular region and the inner circle outer diameter r1 of the first annular region satisfy the following relationship: (r2-r1)≤3 μm. The optical fiber provided by the present invention divides the cladding into a plurality of annular doped regions and reasonably designs the refractive indexes of the fiber core and the doped regions, so that the relative refractive index difference Δn1 between the fiber core and silica is 0.5% to 1%, and the relative refractive index difference Δn2 between the first annular region and silica is -0.1% to 0.3%, thereby making the stress inside the optical fiber more uniform, reducing local stress, avoiding the outer coating of the optical fiber from falling off due to excessive internal local stress and uneven stress distribution when the optical fiber is bent, and improving the reliability of the optical fiber. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0038] Figure 1 A schematic diagram of the structure of an optical fiber provided by an embodiment of the present invention;
[0039] Figure 2 for Figure 1 The enlarged view of point A in the middle;
[0040] Figure 3 A flow chart of a method for preparing an optical fiber provided in an embodiment of the present invention.
[0041] Reference numerals:
[0042] 100-fiber;
[0043] 110-fiber core;
[0044] 120-cladding;
[0045] 121 - first annular area;
[0046] 122 - second annular area;
[0047] 123-third annular area;
[0048] 124-the fourth annular area;
[0049] 125-Fifth Ring Area;
[0050] 126-sixth ring area;
[0051] 127-7th Ring Area;
[0052] 128-8th Ring Area;
[0053] 130-stress layer;
[0054] 140-first coating;
[0055] 150 - Second coating. DETAILED DESCRIPTION
[0056] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0057] Polarization-maintaining optical fiber is commonly used as a fiber optic gyroscope and needs to be wound before use. Usually, several hundred meters of optical fiber are wound into a gyroscope. If the coating falls off, the stripped fiber part will lose protection and be directly damaged, affecting the performance of the optical fiber. In the current traditional technical solutions, the coating of the optical fiber is easily affected by stress after curing, causing it to fall off.
[0058] In view of this, the present invention provides an optical fiber 100, which divides the cladding 120 into a plurality of annular doped regions and reasonably designs the refractive indexes of the core 110 and the doped regions, so that the relative refractive index difference Δn1 between the core 110 and silica is 0.5% to 1%, and the relative refractive index difference Δn2 between the first annular region 121 and silica is -0.1% to 0.3%, thereby making the stress inside the optical fiber 100 more uniform, reducing local stress, avoiding the outer coating of the optical fiber 100 from falling off due to excessive internal local stress and uneven stress distribution when the optical fiber 100 is bent, and improving the reliability of the optical fiber 100.
[0059] Figure 1 A schematic diagram of the structure of an optical fiber provided by an embodiment of the present invention; Figure 2 for Figure 1 The enlarged view of point A in the middle; Figure 3 A flowchart of a method for preparing an optical fiber provided by an embodiment of the present invention. Figure 1 and Figure 2 As shown, the present invention provides an optical fiber 100, including a core 110, a cladding 120, a stress layer 130 and a coating, wherein the cladding 120 is coated on the outside of the core 110, the stress layer 130 is embedded in the cladding 120, there are two stress layers 130, the two stress layers 130 are evenly arranged around the periphery of the core 110, and the coating is coated on the outside of the cladding 120;
[0060] The radius a of the fiber core 110 is 2.75 μm to 3.25 μm, and the relative refractive index difference Δn1 of the fiber core 110 is 0.5% to 1%;
[0061] The radius b of the cladding 120 is 39 μm to 41 μm. In the radial direction of the cladding 120, the cladding 120 includes a plurality of annular doped regions in a concentric circle structure. The annular doped regions include a first annular region 121. The first annular region 121 surrounds the outside of the core 110. The relative refractive index difference Δn2 of the first annular region 121 is -0.1% to 0.3%. The outer circle radius r2 of the first annular region 121 and the inner circle outer diameter r1 of the first annular region 121 satisfy the following relationship:
[0062] (r2-r1)≤3μm
[0063] The relative refractive index difference is the difference between the refractive index of the target area on the optical fiber 100 and the refractive index of silica.
[0064] The target area refers to the current area, and the target area may represent the fiber core 110, the first annular area 121, and the like.
[0065] It can be understood that the refractive index at different positions of the optical fiber 100 can be changed by doping the optical fiber 100 with elements such as germanium, phosphorus, boron, and fluorine. Among them, doping with germanium and phosphorus elements can increase the refractive index, and doping with boron and fluorine elements can reduce the refractive index. The embodiment of the present invention does not limit the type of doping elements as long as it meets the refractive index requirements.
[0066] The optical fiber 100 provided in the embodiment of the present invention divides the cladding 120 into a plurality of annular doped regions, and reasonably designs the refractive index of the core 110 and the doped regions, so that the relative refractive index difference Δn1 between the core 110 and silica is 0.5% to 1%, and the relative refractive index difference Δn2 between the first annular region 121 and silica is -0.1% to 0.3%, so that the stress inside the optical fiber 100 is more uniform, the local stress is reduced, and the external coating of the optical fiber 100 is prevented from falling off due to excessive internal local stress and uneven stress distribution when the optical fiber 100 is bent, thereby improving the reliability of the optical fiber 100. Among them, Δn1 and Δn2 that are too large or too small will cause excessive stress concentration when the optical fiber 100 is bent, thereby increasing the risk of the external coating of the optical fiber 100 falling off.
[0067] In the above embodiment, the ratio of the distance r between the two stress layers 130 and the radius a of the core 110 can be between 3 and 4, the stress layer 130 is doped with B2O3 at a concentration of 17 mol% to 26 mol%, and the value range of (r+t) / b is between 0.7 and 0.85, where t is the diameter of the stress layer 130. By doping the stress layer 130 with a proper amount of B2O3, the shrinkage coefficient of the stress layer 130 after being heated can be made higher than that of the cladding 120, thereby improving the adhesion between the stress layer 130 and the cladding 120, making the internal structure of the optical fiber 100 more compact and reliable.
[0068] In the above embodiment, the annular doped region may further include a second annular region 122 and a third annular region 123, wherein the second annular region 122 surrounds the first annular region 121, and the third annular region 123 surrounds the second annular region 122, and the relative refractive index difference Δn of the second annular region 122 is a Calculated by the following formula:
[0069]
[0070] Among them, Δn3 is the relative refractive index difference of the third annular zone 123, Δn3 is between -0.1% and -0.5%, r3 is the outer circle radius of the second annular zone 122, (r3-r2)≤2.5μm, r4 is the outer circle radius of the third annular zone 123, 2μm≤(r4-r3)≤6μm.
[0071] In the above embodiment, the annular doped region may further include a fourth annular region 124 and a fifth annular region 125, wherein the fourth annular region 124 surrounds the third annular region 123, and the fifth annular region 125 surrounds the fourth annular region 124, and the relative refractive index difference Δn of the fourth annular region 124 is b Calculated by the following formula:
[0072]
[0073] Among them, Δn4 is the relative refractive index difference of the fifth annular zone 125, Δn4 is between 0 and -0.2.5%, r5 is the outer circle radius of the fourth annular zone 124, (r5-r4)≤2.5μm, 1μm≤(r6-r5)≤2.5μm, and r6 is the outer circle radius of the fifth annular zone 125.
[0074] In the above embodiment, the annular doped region may further include a sixth annular region 126, a seventh annular region 127 and an eighth annular region 128, the sixth annular region 126 surrounds the fifth annular region 125, the seventh annular region 127 surrounds the sixth annular region 126, the eighth annular region 128 surrounds the seventh annular region 127, and the relative refractive index difference Δn of the sixth annular region 126 isc Calculated by the following formula:
[0075]
[0076] Wherein, Δn5 is -0.5% to -1.2%, r7 is the outer radius of the sixth annular region 126, and 6 μm ≤ (r7-r6) ≤ 12 μm;
[0077] The relative refractive index difference Δn of the seventh annular zone 127 d Calculated by the following formula:
[0078]
[0079] Wherein, Δn6 is the relative refractive index difference of the eighth annular zone 128, the value of Δn6 is 0, r8 is the outer radius of the seventh annular zone 127, 7μm≤(r8-r7)≤13μm, 39μm≤(r9-r8)
[0080] ≤41 μm, r9 is the radius of the cladding 120. By dividing the cladding 120 into a plurality of doping regions with different refractive indices, the internal structure of the optical fiber 100 can be made more stable, further preventing the coating from falling off, and improving the service life of the optical fiber 100.
[0081] In the above embodiment, the coating material can be acrylic resin. Among them, acrylic resin has the advantages of high transparency, good weather resistance, high hardness, good wear resistance, etc. These advantages can make the optical fiber 100 more stable during use and the quality of the transmitted signal higher. In addition, acrylic resin also has good flexibility and impact resistance, which makes the optical fiber 100 not easily damaged when subjected to external forces. In addition, acrylic resin also has good chemical corrosion resistance and can be used in harsh environments.
[0082] In the above embodiment, the coating may include a first coating 140 and a second coating 150, the first coating 140 is coated on the outside of the cladding 120, the second coating 150 is coated on the outside of the first coating 140, and the first coating 140 uses an acrylic resin with a Young's modulus less than 1.5 MPa and an elongation at break greater than or equal to 130%. Using the acrylic resin of the specification in this embodiment as the first coating 140 can improve the flexibility of the coating, make the first coating 140 more firmly combined with the cladding 120, and can withstand greater bending stress without falling off.
[0083] In the above embodiment, the second coating 150 uses an acrylic resin with a Young's modulus of 900MPa to 1500MPa, an elongation at break greater than or equal to 10%, and a glass transition temperature of 70°C to 150°C. Using the acrylic resin of the specification in this embodiment as the second coating 150 can improve the hardness of the coating and the wear resistance of the outer coating. Through this double-layer coating structure with a relatively soft inner layer and a relatively hard outer layer, the bonding force between the coating of the optical fiber 100 and the cladding 120 can be improved, the risk of its falling off can be reduced, and the wear resistance of the coating can be improved, thereby increasing its service life.
[0084] The optical fiber 100 provided in the embodiment of the present invention comprises a core 110, a cladding 120, a stress layer 130 and a coating. The cladding 120 is coated on the outside of the core 110, the stress layer 130 is embedded in the cladding 120, there are two stress layers 130, the two stress layers 130 are evenly arranged around the periphery of the core 110, and the coating is coated on the outside of the cladding 120; the radius a of the core 110 is 2.75 μm to 3.25 μm, and the relative refractive index difference Δn1 of the core 110 is 0.5% to 1%; the cladding 120 is coated on the outside of the core 110, and the stress layer 130 is embedded in the cladding 120. There are two stress layers 130, and the two stress layers 130 are evenly arranged around the periphery of the core 110, and the coating is coated on the outside of the cladding 120; the radius a of the core 110 is 2.75 μm to 3.25 μm, and the relative refractive index difference Δn1 of the core 110 is 0.5% to 1%; The radius b of 0 is 39μm~41μm. In the radial direction of the cladding 120, the cladding 120 includes a plurality of annular doped regions in a concentric circle structure. The annular doped regions include a first annular region 121. The first annular region 121 surrounds the outside of the core 110. The relative refractive index difference Δn2 of the first annular region 121 is -0.1%~0.3%. The outer circle radius r2 of the first annular region 121 and the inner circle outer diameter r1 of the first annular region 121 satisfy the following relationship: (r2-r1)≤3μm. The optical fiber 100 provided in the embodiment of the present invention divides the cladding 120 into a plurality of annular doped regions, and reasonably designs the refractive indices of the core 110 and the doped regions, so that the relative refractive index difference Δn1 between the core 110 and silica is 0.5% to 1%, and the relative refractive index difference Δn2 between the first annular region 121 and silica is -0.1% to 0.3%, thereby making the stress inside the optical fiber 100 more uniform, reducing local stress, and preventing the outer coating of the optical fiber 100 from falling off due to excessive internal local stress and uneven stress distribution when the optical fiber 100 is bent, thereby improving the reliability of the optical fiber 100.
[0085] In addition, an embodiment of the present invention further provides a method for preparing an optical fiber 100, which is applied to the optical fiber 100 in the above embodiment, and includes the following steps:
[0086] S100, melting the optical fiber preform at a temperature of 800°C to 2000°C.
[0087] The optical fiber preform is melted at high temperature, so that the preform is transformed from a solid state to an intermediate state between a solid state and a liquid state, which is convenient for subsequent thermal processing of the preform. The heating method of the optical fiber preform can be graphite heating or induction coil heating. The environment where the optical fiber preform is located is filled with a protective gas. The protective gas can be selected from helium, argon, or a mixed gas thereof, wherein the proportion of helium in the total can be less than 20%, the total gas flow rate is (10L-30L) / min, and the oxygen concentration is less than 50ppm.
[0088] S200, drawing the melted optical fiber preform into an optical fiber body at a speed of 300m / min to 500m / min.
[0089] It can be understood that the preform rod is heated and melted in the drawing furnace, and the heating temperature is correlated with the non-contact tension indication. At a certain speed, the higher the heating temperature, the smaller the non-contact tension. Taking the non-contact tension as the control standard, the heating temperature (or power) can meet the non-contact tension indication between 30g and 85g.
[0090] S300, applying the first coating 140 to the surface of the optical fiber body at a temperature of 36°C to 44°C.
[0091] S400, coating the second coating layer 150 on the surface of the first coating layer 140 at a temperature of 25-33°C.
[0092] Wherein, if the coating temperature of the first coating 140 and the second coating 150 is too high or too low, the coating quality will be affected.
[0093] S500 , curing the first coating 140 and the second coating 150 to form the optical fiber 100 , wherein the curing degree of the first coating 140 is 82% to 86%, and the curing degree of the second coating 150 is 88% to 92%.
[0094] Among them, after the curing is completed, the size of the optical fiber 100 can be made smaller than the target value by about 5μm (for example, if the target optical fiber 100 size is 135μm, then the size of the optical fiber 100 after curing is about 130μm), the coating curing can be carried out by ultraviolet curing or LED lamp curing, and the curing environment is isolated by one of nitrogen, helium, argon or a mixed gas. The gas flow rate of a single curing furnace is controlled at 5L~20L, and the oxygen content in the curing environment is less than 100ppm. During the curing process, the optical fiber 100 can be exposed to the air environment for no more than 0.02S when passing through different curing furnaces. After being cured in the curing furnace, the curing degree of the inner coating (first coating 140) of the optical fiber 100 is 88%~94%, and the curing degree of the outer coating (second coating 150) is 92%~98%.
[0095] S600, collecting the optical fiber 100 onto a fiber collection reel.
[0096] The strength of the optical fiber 100 may be tested before being wound onto the fiber winding drum, and the optical fiber 100 having a strength greater than or equal to 100 kpsi may be wound onto the optical fiber 100 drum.
[0097] In the above embodiment, before the first coating 140 and the second coating 150 are cured to form the optical fiber 100, the process further includes: performing a surface inspection on the optical fiber 100 after the curing treatment, and coating the surface of the optical fiber 100 with the first coating 140 when the inspection fails. This step is similar to coloring, and the selected coating is consistent with the material of the first coating 140. After this step, the damage caused to the coating of the optical fiber 100 due to various reasons during the preparation process can be repaired, thereby improving the quality of the optical fiber 100.
[0098] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An optical fiber, It is characterized in that It includes a fiber core, a cladding, a stress layer and a coating, wherein the cladding is coated on the outside of the fiber core, the stress layer is embedded in the cladding, there are two stress layers, the two stress layers are evenly arranged around the periphery of the fiber core, and the coating is coated on the outside of the cladding; The radius a of the fiber core is 2.75 μm to 3.25 μm, and the relative refractive index difference Δn of the fiber core is 1 0.5% to 1%; The radius b of the cladding is 39 μm to 41 μm. In the radial direction of the cladding, the cladding includes a plurality of annular doped regions in a concentric circle structure. The annular doped regions include a first annular region surrounding the outside of the fiber core. The relative refractive index difference Δn of the first annular region is 2 The outer radius of the first annular zone is -0.1% to 0.3%. 2 The inner diameter of the first annular zone is r 1 Satisfies the following relationship: (r 2 -r 1 )≤3μm The relative refractive index difference is the difference between the refractive index of the target area on the optical fiber and the refractive index of silica.
2. The optical fiber according to claim 1, It is characterized in that The ratio of the distance r between the two stress layers to the core radius a is between 3 and 4, and the stress layer is doped with B at a concentration of 17 mol% to 26 mol%. 2 O 3 , and the value range of (r+t) / b is 0.7 to 0.85, where t is the diameter of the stress layer.
3. The optical fiber according to claim 2, It is characterized in that The annular doping region further includes a second annular region and a third annular region, wherein the second annular region surrounds the first annular region, the third annular region surrounds the second annular region, and the relative refractive index difference Δn of the second annular region is a Calculated by the following formula: Among them, Δn 3 is the relative refractive index difference of the third annular zone, Δn 3 Between -0.1% and -0.5%, r 3 is the outer radius of the second annular zone, (r 3 -r 2 )≤2.5μm, r 4 is the outer radius of the third annular zone, 2μm≤(r 4 -r 3 )≤6μm.
4. The optical fiber according to claim 3, It is characterized in that The annular doping region further includes a fourth annular region and a fifth annular region, wherein the fourth annular region surrounds the third annular region, the fifth annular region surrounds the fourth annular region, and the relative refractive index difference Δn of the fourth annular region is b Calculated by the following formula: Among them, Δn 4 is the relative refractive index difference of the fifth annular zone, Δn 4 Between 0 and -0.2.5%, r 5 is the outer radius of the fourth annular zone, (r 5 -r 4 )≤2.5μm, 1μm≤(r 6 -r 5 )≤2.5μm, r 6 is the outer radius of the fifth annular area.
5. The optical fiber according to claim 4, It is characterized in that The annular doping region further includes a sixth annular region, a seventh annular region and an eighth annular region, wherein the sixth annular region surrounds the fifth annular region, the seventh annular region surrounds the sixth annular region, the eighth annular region surrounds the seventh annular region, and the relative refractive index difference Δn of the sixth annular region is c Calculated by the following formula: Among them, Δn 5 -0.5%~-1.2%, r 7 is the outer radius of the sixth annular zone, 6 μm≤(r 7 -r 6 )≤12μm; The relative refractive index difference Δn of the seventh annular zone d Calculated by the following formula: Among them, Δn6 is the relative refractive index difference of the eighth annular zone, the value of Δn6 is 0, r8 is the outer circle radius of the seventh annular zone, 7μm≤(r8-r7)≤13μm, 39μm≤(r9-r8)≤41μm, and r9 is the radius of the cladding.
6. The optical fiber according to any one of claims 1 to 5, It is characterized in that The material of the coating is acrylic resin.
7. The optical fiber according to claim 6, It is characterized in that The coating comprises a first coating and a second coating, wherein the first coating is coated on the outside of the cladding, and the second coating is coated on the outside of the first coating, and the first coating uses an acrylic resin with a Young's modulus less than 1.5 MPa and an elongation at break greater than or equal to 130%.
8. The optical fiber according to claim 7, It is characterized in that The second coating layer uses an acrylic resin with a Young's modulus of 900 MPa to 1500 MPa, a breaking elongation of 10% or more, and a glass transition temperature of 70° C. to 150° C.
9. A method for preparing an optical fiber, It is characterized in that The optical fiber according to claim 7 or 8 comprises the following steps: Melting the optical fiber preform at a temperature of 800° C. to 2000° C.; Drawing the melted optical fiber preform into an optical fiber body at a speed of 300m / min to 500m / min; Applying the first coating to the surface of the optical fiber body at a temperature of 36° C. to 44° C.; Applying the second coating layer on the surface of the first coating layer at a temperature of 25 to 33° C.; Curing the first coating layer and the second coating layer to form an optical fiber; Receiving the optical fiber onto a fiber receiving tray; The curing degree of the first coating is 82% to 86%, and the curing degree of the second coating is 88% to 92%.
10. The method for preparing an optical fiber according to claim 9, It is characterized in that Before curing the first coating and the second coating to form an optical fiber, the method further includes: performing a surface inspection on the optical fiber after the curing treatment, and coating the first coating on the surface of the optical fiber if the inspection fails.
Citation Information
Patent Citations
Annular stress region-birefringent polarization maintaining optical fiber and preparation method thereof
CN106646732A
Quasi-rectangular panda polarization maintaining fiber
CN108169845A
Polarization maintaining fiber
CN108845389A
Polarization maintaining optical fiber and preparation method thereof
CN110780377A
Polarization-maintaining three-layer coated optical fiber, coating method, optical fiber ring preparation method and application
CN114924346A