Sodium-ion battery sulfate positive electrode material, preparation method thereof and sodium-ion battery
By regulating the metal element ratio and octahedral vacancies in the phosphorite structure, the problem of poor conductivity of sodium-ion battery cathode materials is solved, the electrochemical performance and cycle stability are improved, and it is suitable for large-scale application and reduces costs.
Patent Information
- Application Number
- CN202310386783.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-18
AI Technical Summary
Existing sodium-ion battery cathode materials have problems such as poor conductivity, poor air stability, unstable cycle performance and poor rate performance, which limits their large-scale application.
By forming a unique phosphorite structure, regulating the element ratio of M1 and M2, controlling the vacancies of metal elements in the M1O6 or M2O6 octahedron, reducing the energy barrier of sodium ions in the channel, and improving the conductivity of the ions.
It significantly improves the conductivity and electrochemical properties of sodium ions, improves the cycle stability and rate performance of the material, and is suitable for large-scale industrial preparation with low cost.
Smart Images

Figure CN118800903A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of manufacturing positive electrode materials for sodium ion batteries, and relates to a sodium ion battery sulfate positive electrode material and a preparation method thereof, and a sodium ion battery. Background Art
[0003] Lithium-ion batteries have attracted widespread attention and achieved great success due to their high energy density, high power density, and stable and efficient voltage output. However, the continuous expansion of the lithium battery market will eventually exhaust the existing lithium resources and inevitably lead to higher costs. Since sodium and lithium belong to the same main group elements, sodium-ion batteries have similar operating voltages, similar electrochemical properties and working principles as lithium-ion batteries. Although the energy density is slightly lacking, the content of sodium in the earth's crust is much higher than that of lithium, and it has broad prospects in large-scale energy storage. Since the working principle of sodium-ion batteries is similar to that of lithium-ion batteries, the development of sodium-ion batteries can draw on the mature principles of lithium-ion battery systems. The key lies in finding suitable positive and negative electrode materials. In order to reduce costs and restrict the excessive rise in lithium ore prices, the development of positive electrode materials for sodium-ion batteries is an urgent problem that needs to be solved.
[0004] Unlike lithium-ion batteries, which have ternary materials and lithium iron phosphate, the mainstream route of sodium-ion batteries has not yet been fully confirmed. At present, relatively mature positive electrode materials include layered oxides and polyanion materials. However, layered oxides face problems such as poor air stability, high rate performance and cycle performance are not as good as polyanion materials, and the production cost is relatively expensive. Although polyanion phosphates have good cycle stability, they have poor conductivity and low operating voltage, and the V, F and other elements doped in them also face problems such as toxicity and high prices.
[0005] Thanks to the high electronegativity of sulfur, polyanionic sulfate cathode materials have advantages such as high operating voltage comparable to lithium-ion batteries, good theoretical specific capacity and low preparation cost. As polyanionic materials, they also have high ionic conductivity and broad prospects. However, polyanionic sulfate cathode materials also face problems such as low intrinsic electronic conductivity and poor air stability, which limit the capacity of the material, and also lead to unstable cycle performance and poor rate performance, which restricts their large-scale practical application.
[0006] In view of the above-mentioned shortcomings of the prior art, there is an urgent need to provide a sodium ion battery positive electrode material with a convenient synthesis route and excellent conductivity. Summary of the invention
[0007] In view of the problems existing in the prior art, the present invention provides a sodium ion battery sulfate positive electrode material and a preparation method thereof and a sodium ion battery. The sodium ion battery sulfate positive electrode material provided by the present invention forms a unique sodium manganese phosphate structure, and the electrochemical performance of the material is improved by adjusting the element ratio of M1 and M2; by controlling the M1O 6 or M2O 6 The vacancies of metal elements in the octahedron effectively reduce the energy barrier for the transmission of sodium ions in the channel and improve the conductivity of the ions.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a sodium ion battery sulfate positive electrode material, wherein the chemical formula of the sodium ion battery sulfate positive electrode material is Na a M1 b M2 c (SO 4 ) 3 , wherein M1 and M2 are metal elements, 1.8≤a≤2.2, for example, it can be 1.8, 1.9, 2, 2.1 or 2.2, 0<b≤2, for example, it can be 0.1, 0.5, 1, 1.5 or 2, 0<c≤2, for example, it can be 0.1, 0.5, 1, 1.5 or 2, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0010] The sodium ion battery sulfate positive electrode material provided by the present invention forms a unique sodium phosphate manganese sodium structure, and the electrochemical performance of the material is improved by adjusting the element ratio of M1 and M2; 6 or M2O 6 The vacancies of metal elements in the octahedron effectively reduce the energy barrier for the transmission of sodium ions in the channel and improve the conductivity of the ions.
[0011] The control of metal element vacancies is caused by different element ratios, for example, when there is no vacancy, it is Na 2 Fe 2 (SO 4 ) 3 , when the element ratio is Na 2.2 Fe 1.9 (SO 4 ) 3 When FeO is present 6 Octahedron vacancy.
[0012] Preferably, the M1 includes any one of Fe, Ni or Co or a combination of at least two thereof. Typical but non-limiting combinations include a combination of Fe and Ni, a combination of Ni and Co, a combination of Fe and Co, or a combination of Fe, Ni and Co.
[0013] Preferably, M2 includes any one of Fe, Ni, Co, Al, Mn, Cu or V, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of Fe and Ni, a combination of Ni and Co, a combination of Co and Al, a combination of Al and Mn, a combination of Mn and Cu, a combination of Cu and V, a combination of Fe, Ni and Co, a combination of Ni, Co and Al, a combination of Co, Al and Mn, a combination of Al, Mn and Cu, and a combination of Mn, Cu and V.
[0014] Preferably, the structure of the sodium ion battery sulfate positive electrode material is composed of MO 6 Octahedron and SO 4 Tetrahedron, wherein M is one of M1 or M2. M refers to M1 and / or M2.
[0015] Preferably, in the structure of the sodium ion battery sulfate positive electrode material, adjacent MO 6 Octahedron edge-sharing, MO 6 The vertices of the octahedron and SO 4 The vertices of the tetrahedron are connected.
[0016] Preferably, in the structure of the sodium ion battery sulfate positive electrode material, sodium ions are embedded in the MO 6 Octahedron and SO 4 In a tunnel made of tetrahedrons.
[0017] Preferably, the sodium ion battery sulfate positive electrode material is in the shape of secondary particles composed of primary particles.
[0018] Preferably, the particle size of the primary particles is in the range of 50 to 100 nm, for example, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, the particle size of the secondary particles is in the range of 1 to 10 μm, for example, 1 μm, 3 μm, 5 μm, 7 μm, 9 μm or 10 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] In a second aspect, the present invention provides a method for preparing the sodium ion battery sulfate positive electrode material according to the first aspect, the preparation method comprising the following steps:
[0021] (1) mixing sodium sulfate, M1 salt, M2 salt and a solvent to obtain a mixed solution;
[0022] (2) drying the obtained mixed solution to obtain a precursor powder;
[0023] (3) calcining the obtained precursor powder to obtain the sodium ion battery sulfate positive electrode material.
[0024] Preferably, the M1 salt in step (1) is sulfate of M1.
[0025] Preferably, the M2 salt in step (1) is sulfate of M2.
[0026] Preferably, the molar amounts of sodium sulfate, M1 salt and M2 salt in step (1) are as follows: a M1 b M2 c (SO 4 ) d Mix in proportion.
[0027] Preferably, the solvent in step (1) comprises deionized water.
[0028] Preferably, the mixing in step (1) is followed by stirring until a clear solution is obtained.
[0029] Preferably, after the mixing in step (1), the process further comprises supplementing a sodium source and a reducing agent.
[0030] In the present invention, a sodium source is additionally added, which reduces the generation of sodium-deficient phase impurities during the preparation process, thereby improving the purity of the product and further improving the capacity of the material.
[0031] Preferably, the sodium source comprises a sodium salt.
[0032] Preferably, the molar amount of the sodium salt is 10 to 30 mol% of the molar amount of sodium sulfate, for example, it can be 10 mol%, 15 mol%, 20 mol%, 25 mol% or 30 mol%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, the reducing agent comprises glucose and / or ascorbic acid.
[0034] The supplementary reducing agent in the present invention provides reducing agents for the preparation process on the one hand, avoiding oxidation of elements such as divalent iron, and at the same time, reducing agents such as glucose and / or ascorbic acid are introduced as carbon sources and can be in-situ coated during the sintering process, which helps to improve the conductivity and structural stability of the material.
[0035] Preferably, the mass of the reducing agent is 10 to 30 wt% of the mass of the sodium ion battery sulfate positive electrode material, for example, it can be 10 wt%, 15 wt%, 20 wt%, 25 wt% or 30 wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] Preferably, the pH of the mixed solution in step (1) is 2 to 6, for example, 2, 2.5, 3, 4, 5, 5.5 or 6, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0037] Preferably, the drying in step (2) comprises any one of evaporative drying, spray drying or condensation drying, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of evaporative drying and spray drying, a combination of spray drying and condensation drying, a combination of evaporative drying and condensation drying, and a combination of evaporative drying, spray drying and condensation drying.
[0038] Preferably, the heating temperature of the evaporative drying is 100-200°C, for example, 100°C, 120°C, 140°C, 160°C, 180°C or 200°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0039] Preferably, the evaporative drying process is accompanied by stirring until the solvent is completely evaporated.
[0040] Preferably, the calcination in step (3) is carried out in a hydrogen-argon mixed gas.
[0041] Preferably, the volume ratio of hydrogen to argon in the hydrogen-argon mixture is (3-6):(97-94), for example, 3:97, 4:96, 5:95, 5.5:94.5 or 6:94, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] Preferably, the calcination temperature in step (3) is 320-380°C, for example, 320°C, 340°C, 360°C, 370°C or 380°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0043] Preferably, the calcination time in step (3) is 10 to 30 hours, for example, 10 hours, 15 hours, 20 hours, 25 hours or 30 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0044] Preferably, the calcination in step (3) is followed by grinding.
[0045] Preferably, the grinding time is 5 to 15 minutes, for example, 5 minutes, 8 minutes, 10 minutes, 12 minutes or 15 minutes, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0046] As a preferred technical solution of the preparation method described in the second aspect of the present invention, the preparation method comprises the following steps:
[0047] (1) According to Na a M1 b M2 c (SO 4 ) d Sodium sulfate, sulfate of M1, sulfate of M2 and deionized water are mixed in a ratio of , and after mixing, sodium salt and reducing agent are added, and stirred to a clear solution to obtain a mixed solution with a pH of 2 to 6; the molar amount of the sodium salt is 10 to 30 mol% of the molar amount of the sodium sulfate; the mass of the reducing agent is 10 to 30 wt% of the mass of the sulfate positive electrode material of the sodium ion battery;
[0048] (2) drying the obtained mixed solution to obtain a precursor powder; the drying includes any one of evaporative drying, spray drying or condensation drying, or a combination of at least two of them;
[0049] The evaporative drying method is to heat the obtained mixed solution to a temperature of 100 to 200° C. and stir until the solvent is completely evaporated;
[0050] (3) calcining the obtained precursor powder at 320-380° C. for 10-30 h in a hydrogen-argon mixed gas with a volume ratio of (3-6):(97-94), and then grinding for 5-15 min to obtain the sodium ion battery sulfate positive electrode material.
[0051] The liquid phase synthesis method provided by the present invention optimizes the pretreatment process of raw materials, is suitable for large-scale industrial preparation, has low cost and high product purity.
[0052] In a third aspect, the present invention provides a sodium ion battery, wherein the sodium ion battery contains the sodium ion battery sulfate positive electrode material as described in the first aspect.
[0053] According to the above technical scheme, the beneficial effects of the present invention are as follows:
[0054] The sodium ion battery sulfate positive electrode material provided by the present invention forms a unique sodium phosphate manganese sodium structure, and the electrochemical performance of the material is improved by adjusting the element ratio of M1 and M2; 6 or M2O 6 The vacancies of metal elements in the octahedron effectively reduce the energy barrier for the transmission of sodium ions in the channel and improve the conductivity of the ions. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 This is a SEM image of the sodium ion battery sulfate positive electrode material described in Example 1.
[0056] Figure 2This is a SEM image of the sodium ion battery sulfate positive electrode material described in Example 2. DETAILED DESCRIPTION
[0057] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0058] Example 1
[0059] This embodiment provides a sodium ion battery sulfate positive electrode material (SEM as Figure 1 As shown), the chemical formula of the sodium ion battery sulfate positive electrode material is Na 2 FeNi(SO 4 ) 3 The structure of the sodium ion battery sulfate cathode material is composed of MO 6 Octahedron and SO 4 Tetrahedral structure, adjacent MO 6 Octahedron edge-sharing, MO 6 The vertices of the octahedron and SO 4 The vertices of the tetrahedron are connected, and the sodium ions are embedded in the MO 6 Octahedron and SO 4 In the tunnel formed by tetrahedrons; the shape of the sodium ion battery sulfate positive electrode material is secondary particles composed of primary particles, the particle size of the primary particles is 75nm, and the particle size of the secondary particles is 5μm.
[0060] The method for preparing the sodium ion battery sulfate positive electrode material comprises the following steps:
[0061] (1) According to Na 2 FeNi(SO 4 ) 3 Sodium sulfate, ferrous sulfate, nickel sulfate and deionized water are mixed in a ratio of 1:1, and CH 3 COONa and glucose, stirred to a clear solution, and a mixed solution with a pH of 5 was obtained by adding sulfuric acid; the CH 3 The molar amount of COONa is 20 mol% of the molar amount of sodium sulfate; the mass of the glucose is 20 wt% of the mass of the sulfate positive electrode material of the sodium ion battery;
[0062] (2) heating the obtained mixed solution to a temperature of 130° C. and stirring until the solvent is completely evaporated to obtain a precursor powder;
[0063] (3) In a hydrogen-argon mixed gas with a volume ratio of 5:95, the obtained precursor powder was calcined at 350° C. for 15 hours, and then ground for 10 minutes to obtain the sodium ion battery sulfate positive electrode material.
[0064] Example 2
[0065] This embodiment provides a sodium ion battery sulfate positive electrode material (SEM as Figure 2 As shown), the chemical formula of the sodium ion battery sulfate positive electrode material is Na 2.2 FeNi 0.9 (SO 4 ) 3 The structure of the sodium ion battery sulfate cathode material is composed of MO 6 Octahedron and SO 4 Tetrahedral structure, adjacent MO 6 Octahedron edge-sharing, MO 6 The vertices of the octahedron and SO 4 The vertices of the tetrahedron are connected, and the sodium ions are embedded in the MO 6 Octahedron and SO 4 In the tunnel formed by tetrahedrons; the shape of the sodium ion battery sulfate positive electrode material is a secondary particle composed of primary particles, the particle size of the primary particles is 50nm, and the particle size of the secondary particles is 1μm.
[0066] The method for preparing the sodium ion battery sulfate positive electrode material comprises the following steps:
[0067] (1) According to Na 2.2 FeNi 0.9 (SO 4 ) 3 Sodium sulfate, ferrous sulfate, nickel sulfate and deionized water are mixed in a ratio of 1:1, and CH 3 COONa and ascorbic acid, stirred to a clear solution, and a mixed solution with a pH of 2 was obtained by adding sulfuric acid; the CH 3 The molar amount of COONa is 10 mol% of the molar amount of sodium sulfate; the mass of the ascorbic acid is 10 wt% of the mass of the sulfate positive electrode material of the sodium ion battery;
[0068] (2) heating the obtained mixed solution to a temperature of 100° C. and stirring until the solvent is completely evaporated to obtain a precursor powder;
[0069] (3) In a hydrogen-argon mixed gas with a volume ratio of 5:95, the obtained precursor powder was calcined at 320° C. for 30 hours, and then ground for 15 minutes to obtain the sodium ion battery sulfate positive electrode material.
[0070] Example 3
[0071] This embodiment provides a sodium ion battery sulfate positive electrode material (SEM as Figure 2 As shown), the chemical formula of the sodium ion battery sulfate positive electrode material is Na2.2 Fe 0.9 Ni 0.9 Cu 0.1 (SO 4 ) 3 The structure of the sodium ion battery sulfate cathode material is composed of MO 6 Octahedron and SO 4 Tetrahedral structure, adjacent MO 6 Octahedron edge-sharing, MO 6 The vertices of the octahedron and SO 4 The vertices of the tetrahedron are connected, and the sodium ions are embedded in the MO 6 Octahedron and SO 4 In the tunnel formed by tetrahedrons; the shape of the sodium ion battery sulfate positive electrode material is a secondary particle composed of primary particles, the particle size of the primary particles is 100nm, and the particle size of the secondary particles is 10μm.
[0072] The method for preparing the sodium ion battery sulfate positive electrode material comprises the following steps:
[0073] (1) According to Na 2.2 Fe 0.9 Ni 0.9 Cu 0.1 (SO 4 ) 3 Sodium sulfate, ferrous sulfate, nickel sulfate, copper sulfate and deionized water are mixed in a ratio of 1:1, and CH 3 COONa and ascorbic acid, stirred to a clear solution, and a mixed solution with a pH of 6 was obtained by adding sulfuric acid; the CH 3 The molar amount of COONa is 30 mol% of the molar amount of sodium sulfate; the mass of the ascorbic acid is 30 wt% of the mass of the sulfate positive electrode material of the sodium ion battery;
[0074] (2) heating the obtained mixed solution to a temperature of 200° C. and stirring until the solvent is completely evaporated to obtain a precursor powder;
[0075] (3) In a hydrogen-argon mixed gas with a volume ratio of 5:95, the obtained precursor powder was calcined at 380° C. for 10 hours, and then ground for 5 minutes to obtain the sodium ion battery sulfate positive electrode material.
[0076] Example 4
[0077] This embodiment provides a sodium ion battery sulfate positive electrode material, which is different from Embodiment 1 in that the evaporative drying in step (2) of the preparation method is replaced by a spray drying method.
[0078] Example 5
[0079] This embodiment provides a sodium ion battery sulfate positive electrode material, which is different from the embodiment 1 in that CH is not added in step (1). 3 COONa.
[0080] Example 6
[0081] This embodiment provides a sodium ion battery sulfate positive electrode material, which is different from the embodiment 1 in that: the CH 3 The molar amount of COONa was 5 mol% of the molar amount of sodium sulfate.
[0082] Example 7
[0083] This embodiment provides a sodium ion battery sulfate positive electrode material, which is different from the embodiment 1 in that: the CH 3 The molar amount of COONa was 35 mol% of the molar amount of sodium sulfate.
[0084] Example 8
[0085] This embodiment provides a sodium ion battery sulfate positive electrode material, which is different from Embodiment 1 in that glucose is not added in step (1).
[0086] Example 9
[0087] This embodiment provides a sodium ion battery sulfate positive electrode material, which is different from Embodiment 1 in that the mass of the glucose in step (1) is 5wt% of the mass of the sodium ion battery sulfate positive electrode material.
[0088] Example 10
[0089] This embodiment provides a sodium ion battery sulfate positive electrode material, which is different from Embodiment 1 in that the mass of the glucose in step (1) is 35 wt % of the mass of the sodium ion battery sulfate positive electrode material.
[0090] Comparative Example 1
[0091] This comparative example provides a sodium ion battery sulfate positive electrode material, which is different from Example 1 in that the chemical formula is Na 2 Fe 2 (SO 4 ) 3 .
[0092] Comparative Example 2
[0093] This comparative example provides a sodium ion battery sulfate positive electrode material, which is different from Example 1 in that the chemical formula is Na 2 Ni 2 (SO 4 ) 3 .
[0094] The sodium ion battery sulfate positive electrode material obtained above was assembled into a sodium ion battery and subjected to electrochemical testing. The test results are shown in Table 1.
[0095] Table 1
[0096] Test No. capacity Cycle performance Rate performance Example 1 107mAh / g 500 laps 5C / 1C=90% Example 2 105mAh / g 350 laps 5C / 1C=86% Example 3 98mAh / g 400 laps 5C / 1C=84% Example 4 110mAh / g 600 laps 5C / 1C=92% Example 5 89mAh / g 230 laps 5C / 1C=84% Example 6 96mAh / g 300 laps 5C / 1C=85% Example 7 79mAh / g 200 laps 5C / 1C=81% Example 8 84mAh / g 300 laps 5C / 1C=79% Example 9 96mAh / g 450 laps 5C / 1C=82% Example 10 98mAh / g 400 laps 5C / 1C=85% Comparative Example 1 98mAh / g 400 laps 5C / 1C=85% Comparative Example 2 --- --- ---
[0097] In summary, the sodium ion battery sulfate positive electrode material provided by the present invention forms a unique sodium phosphate manganese ore structure, and the electrochemical performance of the material is improved by adjusting the element ratio of M1 and M2; 6 or M2O 6 The vacancies of metal elements in the octahedron effectively reduce the energy barrier for the transmission of sodium ions in the channel and improve the conductivity of the ions.
[0098] The present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A sodium ion battery sulfate positive electrode material, characterized in that: The chemical formula of the sodium ion battery sulfate positive electrode material is Na a M1 b M2 c (SO4)3, wherein M1 and M2 are metal elements, 1.8≤a≤2.2, 0<b≤2, 0<c≤2.
2. The sodium ion battery sulfate positive electrode material according to claim 1, characterized in that: The M1 includes any one of Fe, Ni or Co or a combination of at least two; Preferably, M2 includes any one of Fe, Ni, Co, Al, Mn, Cu or V, or a combination of at least two of them.
3. The sodium ion battery sulfate positive electrode material according to claim 1 or 2, characterized in that: The structure of the sodium ion battery sulfate positive electrode material is composed of MO6 octahedron and SO4 tetrahedron, wherein M is one of M1 or M2; Preferably, in the structure of the sodium ion battery sulfate positive electrode material, adjacent MO6 octahedra are connected by sharing edges, and the vertices of the MO6 octahedron are connected to the vertices of the SO4 tetrahedron; Preferably, in the structure of the sodium ion battery sulfate positive electrode material, sodium ions are embedded in tunnels formed by MO6 octahedrons and SO4 tetrahedrons; Preferably, the sodium ion battery sulfate cathode material is in the shape of secondary particles composed of primary particles; Preferably, the particle size of the primary particles is in the range of 50 to 100 nm; Preferably, the secondary particles have a particle size range of 1 to 10 μm.
4. A method for preparing the sodium ion battery sulfate positive electrode material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) mixing sodium sulfate, M1 salt, M2 salt and a solvent to obtain a mixed solution; (2) drying the obtained mixed solution to obtain a precursor powder; (3) calcining the obtained precursor powder to obtain the sodium ion battery sulfate positive electrode material.
5. The preparation method according to claim 4, characterized in that: The M1 salt in step (1) is a sulfate of M1; Preferably, the M2 salt in step (1) is a sulfate of M2; Preferably, the molar amounts of sodium sulfate, M1 salt and M2 salt in step (1) are as follows: a M1 b M2 c (SO4) d Mix in proportion; Preferably, the solvent in step (1) comprises deionized water; Preferably, the mixing in step (1) is followed by stirring until a clear solution is obtained.
6. The preparation method according to claim 4 or 5, characterized in that: After the mixing in step (1), the step further comprises supplementing a sodium source and a reducing agent; Preferably, the sodium source comprises a sodium salt; Preferably, the molar amount of the sodium salt is 10 to 30 mol% of the molar amount of sodium sulfate; Preferably, the reducing agent comprises glucose and / or ascorbic acid; Preferably, the mass of the reducing agent is 10-30wt% of the mass of the sodium ion battery sulfate positive electrode material; Preferably, the pH of the mixed solution in step (1) is 2-6.
7. The preparation method according to any one of claims 4 to 6, characterized in that: The drying in step (2) includes any one of evaporative drying, spray drying or condensation drying, or a combination of at least two thereof; Preferably, the heating temperature of the evaporative drying is 100-200°C; Preferably, the evaporative drying process is accompanied by stirring until the solvent is completely evaporated.
8. The preparation method according to any one of claims 4 to 7, characterized in that: The calcination in step (3) is carried out in a hydrogen-argon mixed gas; Preferably, the volume ratio of hydrogen to argon in the hydrogen-argon mixture is (3-6):(97-94); Preferably, the calcination temperature in step (3) is 320-380°C; Preferably, the calcination time in step (3) is 10 to 30 hours; Preferably, the calcination in step (3) is followed by grinding; Preferably, the grinding time is 5 to 15 minutes.
9. The preparation method according to any one of claims 4 to 8, characterized in that: The preparation method comprises the following steps: (1) According to Na a M1 b M2 c (SO4) d Sodium sulfate, sulfate of M1, sulfate of M2 and deionized water are mixed in a ratio of , and after mixing, sodium salt and reducing agent are added, and stirred to a clear solution to obtain a mixed solution with a pH of 2 to 6; the molar amount of the sodium salt is 10 to 30 mol% of the molar amount of the sodium sulfate; the mass of the reducing agent is 10 to 30 wt% of the mass of the sulfate positive electrode material of the sodium ion battery; (2) drying the obtained mixed solution to obtain a precursor powder; the drying includes any one of evaporative drying, spray drying or condensation drying, or a combination of at least two of them; The evaporative drying method is to heat the obtained mixed solution to a temperature of 100 to 200° C. and stir until the solvent is completely evaporated; (3) calcining the obtained precursor powder at 320-380° C. for 10-30 h in a hydrogen-argon mixed gas with a volume ratio of (3-6):(97-94), and then grinding for 5-15 min to obtain the sodium ion battery sulfate positive electrode material.
10. A sodium ion battery, characterized in that: The sodium ion battery contains the sodium ion battery sulfate positive electrode material according to any one of claims 1 to 3.