High-strength heat-treatment-free aluminum alloy of regenerated aluminum alloy and preparation method thereof
By precisely controlling the element content in the aluminum alloy and using the vacuum high-pressure casting process, the problems of traditional aluminum alloy heat treatment deformation risks and insufficient performance are solved, and a high-strength, high-toughness and environmentally friendly heat-free aluminum alloy is prepared.
Patent Information
- Application Number
- CN202411110756.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The risk of deformation of large-scale integrated die-cast parts caused by traditional aluminum alloy heat treatment processes is difficult to meet the industry's strict requirements for dimensional accuracy and shape integrity, and the performance of existing heat-treatable aluminum alloys is insufficient to meet increasingly stringent application requirements.
By precisely controlling the content and proportion of Si, Fe, Mn, Mg, Cu, V, Ti, Sr, Ce and other elements, Al-Ti-B is used for grain refinement, combined with the modification treatment of Al-Sr and Al-Ce. , using vacuum high-pressure casting method to prepare high-strength heat-free aluminum alloy, forming Mg2Si phase and spherical crystals to improve mechanical properties.
Aluminum alloys with high tensile strength, high yield strength and high elongation are achieved, which avoids deformation problems caused by heat treatment, while reducing preparation costs and having the advantages of low carbon, environmental protection and energy saving.
Smart Images

Figure BDA0004992120790000051 
Figure BDA0004992120790000052 
Figure BDA0004992120790000061
Abstract
Description
Technical Field
[0001] The invention relates to the field of aluminum alloy manufacturing, and in particular to a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy and a preparation method thereof. Background Art
[0002] In the traditional aluminum alloy processing process, in order to give the material the necessary strength and hardness characteristics, the heat treatment step (covering solution treatment, quenching and aging treatment) is indispensable. However, for large-scale integrated die-cast parts, the heat treatment process is often accompanied by a significant risk of deformation, which makes it difficult to meet the industry's strict requirements for dimensional accuracy and shape integrity. Against this background, heat-treatment-free aluminum alloy technology came into being. It cleverly bypasses the complex heat treatment process and directly exhibits excellent mechanical properties after die-casting, thereby effectively avoiding the deformation problem that may be caused by heat treatment. In order to broaden the application scope of heat-treatment-free aluminum alloys and meet increasingly stringent performance requirements, it is urgently necessary to develop a new type of heat-treatment-free aluminum alloy with higher strength and toughness. Summary of the invention
[0003] In view of the shortcomings of the prior art, the first object of the present invention is to provide a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy. The high-strength heat-treatment-free aluminum alloy provided by the present invention has high tensile strength, high yield strength and high elongation. The present invention accurately controls and optimizes the content and proportion of added elements such as Si, Fe, Mn, Mg, Cu, V, Ti, Sr, Ce, etc., so that the addition of each element is more easily controlled, so that the obtained aluminum alloy has high tensile strength, high yield strength and high elongation.
[0004] The second object of the present invention is to provide a method for preparing a high-strength heat-treatment-free aluminum alloy of recycled aluminum alloy.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] The invention provides a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy. The high-strength heat-treatment-free aluminum alloy has the following compositions by mass percentage: Si: 8.1-9%; Mg: 0.38-0.45%; Ti: 0.15-0.17%; Ce: 0.01-0.03%; Fe: 0.14-0.2%; Mn: 0.58-0.6%; Cu: 0.1-0.14%; V: 0.01-0.02%; Sr: 0.025-0.028%; and the rest is aluminum and unavoidable impurities.
[0007] The high-strength heat-treatment-free aluminum alloy provided by the present invention has high tensile strength, high yield strength and high elongation by controlling the ratio of each element within the scope of the present invention. In the present invention, it is very important to control the content of each element within the scope of the present invention. For example, if the Fe content is too high and the Mn content is too low, β-Fe will have a serious splitting effect on the matrix, affecting the mechanical properties of the alloy. If only one rare earth alloy is added, or the added amount is too much or too little, the size of α-Al will become larger and the dendrites will not be completely transformed into spherical crystals, thereby affecting the performance.
[0008] As a further solution of the present invention: the high-strength heat-treatment-free aluminum alloy has the following composition, calculated by mass percentage: Si: 8.5-9%; Mg: 0.4-0.45%; Ti: 0.15-0.16%; Ce: 0.02-0.03%; Fe: 0.14-0.17%; Mn: 0.58-0.6%; Cu: 0.11-0.14%; V: 0.01-0.02%; Sr: 0.025-0.026%; the rest is aluminum and unavoidable impurities.
[0009] In the present invention, the impurity content of the high-strength heat-treatment-free aluminum alloy provided is less than 0.02%.
[0010] The present invention also provides a method for preparing a high-strength heat-treatment-free aluminum alloy of recycled aluminum alloy: placing an aluminum source in a smelting furnace to melt to obtain an aluminum melt, then adding other intermediate alloy raw materials into the smelting furnace according to a designed proportion to melt to obtain an aluminum alloy melt, refining and degassing the aluminum alloy melt; then adding Al-Ti-B to refine the grains, and then adding Al-Sr and Al-Ce to perform a modification treatment to obtain an aluminum alloy liquid, and finally hydraulically casting the aluminum alloy into a mold.
[0011] The preparation method of the present invention obtains a high-strength aluminum alloy that does not require heat treatment by first performing grain refinement using Al-Ti-B after refining, then performing modification treatment using a mixed rare earth master alloy, and finally performing vacuum high-pressure casting, wherein the grain refinement of eutectic silicon by Al-Ti-B makes it granular; the modification using the mixed rare earth master alloy transforms α-Al from dendrites into spherical crystals with directionality; Mg and Si form a Mg2Si phase, which is dispersion strengthened after aging precipitation; and in coordination with other aluminum alloy strengthening elements, the high-strength aluminum alloy that does not require heat treatment finally obtained has high tensile strength, high yield strength and high elongation.
[0012] The inventors have found that only by using two aluminum rare earth intermediate alloys, Al-Sr and Al-Ce, can α-Al be completely transformed from dendrites to spherical crystals. If only Al-Sr is added without Al-Ce, the size of α-Al will increase and the transformation of dendrites into spherical crystals will be incomplete.
[0013] As a further solution of the present invention: the aluminum source is recycled A356 aluminum alloy prepared from waste aluminum.
[0014] The recycled A356 aluminum alloy provided in the present invention has the following composition by mass percentage: Si: 6.83%; Fe: 0.14%; Mg: 0.319%; Ti: 0.113%; Sn: 0.0203%; the rest is aluminum and inevitable impurities. It should be pointed out here that due to the low content of Sn, after further forming a high-strength heat-treatment-free aluminum alloy, the content below 0.01% is negligible. By using recycled aluminum alloy as an aluminum source, the preparation cost of the high-strength heat-treatment-free aluminum alloy is greatly reduced, low-carbon and environmentally friendly; energy saving.
[0015] As a further solution of the present invention: placing an aluminum source in a smelting furnace and melting it at 715-725° C. to obtain an aluminum melt.
[0016] As a further solution of the present invention, other master alloy raw materials are preheated to 220°C-250°C, and then added to the melting furnace and heated to 750-760°C for melting to obtain aluminum alloy melt. By preheating the master alloy raw materials, the quality of the aluminum alloy melt can be improved.
[0017] As a further solution of the present invention: the order of adding the other intermediate alloy raw materials is: first add the silicon source, manganese source, iron source, copper source, and vanadium source; and then add the magnesium source 4-6 minutes before refining.
[0018] The inventors found that by adding a magnesium source 4-6 minutes before refining, Mg can be prevented from being easily gasified at high temperatures, thereby ensuring that Mg meets the composition ratio and subsequently forms a Mg2Si phase dispersion with Si to strengthen the aluminum alloy.
[0019] More preferably, the manganese source is selected from Al-Mn, the iron source is selected from Al-Fe, the vanadium source is selected from Al-V, the silicon source is selected from Al-Si, the copper source is selected from Al-Cu, and the magnesium source is selected from pure magnesium.
[0020] As a further solution of the present invention: when the temperature of the aluminum alloy melt is 710-730°C, a refining agent is added to the smelting furnace for refining. In the present invention, the refining agent can be conventional in the prior art, such as ordinary refining agent 1#MJH-204, Pyrotech imported refining agent, 4032 special high-efficiency refining agent.
[0021] As a further solution of the present invention: the degassing process is to introduce a protective atmosphere into the aluminum alloy melt, control the pressure of the protective atmosphere to 0.25-0.4Mpa, and stir to degas.
[0022] As a further solution of the present invention: the aluminum alloy melt is refined and degassed under stirring, then allowed to stand for the first time, and then Al-Ti-B is added and stirred for grain refinement. After 4-6 minutes, Al-Sr and Al-Ce are added for modification treatment, and allowed to stand for the second time to obtain aluminum alloy liquid.
[0023] As a further solution of the present invention: the first standing time and the second standing time are both 15-30 minutes.
[0024] As a further solution of the present invention: the Al-Ti-B, Al-Sr, and Al-Ce are all preheated to 220°C-250°C and then added to the aluminum alloy melt.
[0025] As a further solution of the present invention, the die-casting method is vacuum high-pressure casting, and the pressure of the vacuum high-pressure casting is 8-12MPa. Vacuum high-pressure casting can eliminate pores and shrinkage cavities, improve casting quality, and improve casting accuracy.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The present invention reasonably designs the composition of each element so that Fe, Mn, Cu, Mg, Ti and Sr can be maintained at a relatively high proportion, so that the addition of each element is more easily controlled, so that the obtained aluminum alloy has high tensile strength, high yield strength and high elongation.
[0028] The preparation method of the present invention obtains a high-strength aluminum alloy that does not require heat treatment by first performing grain refinement using Al-Ti-B after refining, then performing modification treatment using a mixed rare earth master alloy, and finally performing vacuum high-pressure casting, wherein the grain refinement of eutectic silicon by Al-Ti-B makes it granular; the modification using the mixed rare earth master alloy transforms α-Al from dendrites into spherical crystals with directionality; Mg and Si form a Mg2Si phase, which is dispersion strengthened after aging precipitation; and in coordination with other aluminum alloy strengthening elements, the high-strength aluminum alloy that does not require heat treatment finally obtained has high tensile strength, high yield strength and high elongation. DETAILED DESCRIPTION
[0029] In the traditional aluminum alloy processing process, in order to give the material the necessary strength and hardness characteristics, the heat treatment step (covering solution treatment, quenching and aging treatment) is indispensable. However, for large-scale integrated die-cast parts, the heat treatment process is often accompanied by a significant risk of deformation, which makes it difficult to meet the industry's strict requirements for dimensional accuracy and shape integrity. Against this background, heat-treatment-free aluminum alloy technology came into being. It cleverly bypasses the complex heat treatment process and directly exhibits excellent mechanical properties after die-casting, thereby effectively avoiding the deformation problem that may be caused by heat treatment. In order to broaden the application scope of heat-treatment-free aluminum alloys and meet increasingly stringent performance requirements, it is urgently necessary to develop a new type of heat-treatment-free aluminum alloy with higher strength and toughness.
[0030] The present invention reasonably designs the composition of each element so that Fe, Mn, Cu, Mg, Ti and Sr can be maintained at a relatively high proportion, so that the addition of each element is more easily controlled, so that the obtained aluminum alloy has high tensile strength, high yield strength and high elongation.
[0031] The invention uses vacuum high-pressure casting without heat treatment to make the obtained aluminum alloy have high tensile strength, high yield strength and high elongation.
[0032] Example 1
[0033] A method for preparing a high-strength heat-treatment-free aluminum alloy of recycled aluminum alloy, wherein the aluminum alloy comprises the following elements in weight percentage: Si: 9%; Mg: 0.4%; Ti: 0.15%; Ce: 0.03%; Fe: 0.15%; Mn: 0.6%; Cu: 0.13%; V: 0.02%; Sr: 0.025%; and the rest are aluminum and unavoidable impurities.
[0034] The recycled A356 aluminum alloy prepared from waste aluminum is placed in a furnace and melted at 720°C to form aluminum liquid; Al-Mn, Al-Fe, Al-V, Al-Si, and Al-Cu weighed in mass percentage are added and the temperature is raised to 760°C, and the mixture is fully stirred and mixed. Pure magnesium is added before refining for 5 minutes, and then when the temperature of the aluminum alloy melt is cooled to 720°C, a refining agent is added into the smelting furnace for refining, and then argon gas is introduced into the aluminum alloy melt, and the pressure of the argon gas is controlled to be 0.3Mpa. The mixture is kept warm and allowed to stand for 30 minutes, and then Al-Ti-B is added and stirred for 5 minutes for grain refinement, and then Al-Sr and Al-Ce are added for modification treatment, and the mixture is allowed to stand for 30 minutes to obtain aluminum alloy liquid. The obtained aluminum alloy liquid is subjected to vacuum high-pressure casting at a pressure of 10MPa to obtain a high-strength heat-treatment-free aluminum alloy.
[0035] According to the above preparation method, 6 groups of high-strength heat-treatment-free aluminum alloys were prepared, and their properties are shown in Table 1:
[0036] Table 1 Performance indicators of the high-strength heat-treatment-free aluminum alloy in Example 1.
[0037]
[0038] Example 2
[0039] A method for manufacturing a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy. The aluminum alloy ingot includes the following elements in weight percentage: Si: 9%; Mg: 0.4%; Ti: 0.15%; Ce: 0.03%; Fe: 0.2%; Mn: 0.6%; Cu: 0.13%; V: 0.02%; Sr: 0.025%; the rest is aluminum and unavoidable impurities.
[0040] The recycled A356 aluminum alloy prepared from waste aluminum is placed in a furnace and melted at 720°C to form aluminum liquid; Al-Mn, Al-Fe, Al-V, Al-Si, and Al-Cu are weighed according to mass percentage and heated to 760°C, and fully stirred and mixed. Pure magnesium is added before refining for 5 minutes, and then when the temperature of the aluminum alloy melt is cooled to 720°C, the refining agent is added to the smelting furnace for refining, and then argon gas is introduced into the aluminum alloy melt, and the pressure of the argon gas is controlled to be 0.3Mpa, and the heat is kept and allowed to stand for 30 minutes; then Al-Ti-B is added, stirred for 5 minutes for grain refinement, and Al-Sr and Al-Ce are added for modification treatment, and the mixture is allowed to stand for 30 minutes to obtain aluminum alloy liquid, and the obtained aluminum alloy liquid is subjected to vacuum high-pressure casting at a pressure of 10MPa to obtain a high-strength heat-treatment-free aluminum alloy.
[0041] According to the above preparation method, 6 groups of high-strength heat-treatment-free aluminum alloys were prepared, and their properties are shown in Table 2:
[0042] Table 2 Performance indicators of the high-strength heat-treatment-free aluminum alloy in Example 2.
[0043]
[0044]
[0045] Comparative Example 1
[0046] A method for manufacturing a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy. The aluminum alloy ingot includes the following elements in weight percentage: Si: 9%; Mg: 0.4%; Ti: 0.15%; Ce: 0.04%; Fe: 0.15%; Mn: 0.4%; Cu: 0.1%; V: 0.04%; Sr: 0.04%; the rest is aluminum and unavoidable impurities.
[0047] The recycled A356 aluminum alloy prepared from waste aluminum is placed in a furnace and melted at 720°C to form aluminum liquid; Al-Mn, Al-Fe, Al-V, Al-Si, and Al-Cu are weighed according to mass percentage and heated to 760°C, and fully stirred and mixed. Pure magnesium is added before refining for 5 minutes, and then when the temperature of the aluminum alloy melt is cooled to 720°C, the refining agent is added to the smelting furnace for refining, and then argon gas is introduced into the aluminum alloy melt, and the pressure of the argon gas is controlled to be 0.3Mpa, and the heat is kept and allowed to stand for 30 minutes; then Al-Ti-B is added, stirred for 5 minutes for grain refinement, and Al-Sr and Al-Ce are added for modification treatment, and the mixture is allowed to stand for 30 minutes to obtain aluminum alloy liquid, and the obtained aluminum alloy liquid is subjected to vacuum high-pressure casting at a pressure of 10MPa to obtain a high-strength heat-treatment-free aluminum alloy.
[0048] According to the above preparation method, 6 groups of high-strength heat-treatment-free aluminum alloys were prepared. The modification effect of the comparative example was weakened due to excessive addition of rare earth, and the transformation of α-Al from dendrites to spheroidal crystals was incomplete. The properties are shown in Table 3:
[0049] Table 3 Performance indicators of the high-strength heat-treatment-free aluminum alloy in Comparative Example 1.
[0050]
[0051]
[0052] Comparative Example 2
[0053] A method for manufacturing a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy. The aluminum alloy ingot includes the following elements in weight percentage: Si: 9%; Mg: 0.4%; Ti: 0.15%; Ce: 0.01%; Fe: 0.6%; Mn: 0.2%; Cu: 0.1%; V: 0.01%; Sr: 0.05%; the rest is aluminum and unavoidable impurities.
[0054] The recycled A356 aluminum alloy prepared from waste aluminum is placed in a furnace and melted at 720°C to form aluminum liquid; Al-Mn, Al-Fe, Al-V, Al-Si, and Al-Cu are weighed according to mass percentage and heated to 760°C, and fully stirred and mixed. Pure magnesium is added before refining for 5 minutes, and then when the temperature of the aluminum alloy melt is cooled to 720°C, the refining agent is added to the smelting furnace for refining, and then argon gas is introduced into the aluminum alloy melt, and the pressure of the argon gas is controlled to be 0.3Mpa, and the heat is kept and allowed to stand for 30 minutes; then Al-Ti-B is added, stirred for 5 minutes for grain refinement, and Al-Sr and Al-Ce are added for modification treatment, and the mixture is allowed to stand for 30 minutes to obtain aluminum alloy liquid, and the obtained aluminum alloy liquid is subjected to vacuum high-pressure casting at a pressure of 10MPa to obtain a high-strength heat-treatment-free aluminum alloy.
[0055] According to the above preparation method, 6 groups of high-strength heat-treatment-free aluminum alloys were prepared. Due to the excessively high Fe content and the low Mn content, β-Fe produced a serious splitting effect on the matrix, which affected the mechanical properties of the alloy. The properties are shown in Table 4:
[0056] Table 4 Performance indicators of the high-strength heat-treatment-free aluminum alloy in Comparative Example 1.
[0057]
[0058] Comparative Example 3
[0059] A method for preparing a high-strength heat-treatment-free recycled aluminum alloy, wherein the aluminum alloy comprises the following elements in weight percentage: Si: 9%; Mg: 0.4%; Ti: 0.15%; Fe: 0.15%; Mn: 0.6%; Cu: 0.13%; V: 0.02%; Sr: 0.025%; and the rest are aluminum and unavoidable impurities. The recycled A356 aluminum alloy prepared from waste aluminum is placed in a furnace and melted at 720°C to form aluminum liquid; Al-Mn, Al-Fe, Al-V, Al-Si, and Al-Cu are weighed according to mass percentage and heated to 760°C, and fully stirred and mixed. Pure magnesium is added before refining for 5 minutes, and then when the temperature of the aluminum alloy melt is cooled to 720°C, the refining agent is added to the smelting furnace for refining, and then argon gas is introduced into the aluminum alloy melt, and the pressure of the argon gas is controlled to be 0.3Mpa, and the heat is kept and allowed to stand for 30 minutes; then Al-Ti-B is added, stirred for 5 minutes for grain refinement, and Al-Sr is added for modification treatment, and allowed to stand for 30 minutes to obtain aluminum alloy liquid, and the obtained aluminum alloy liquid is subjected to vacuum high-pressure casting at a pressure of 10MPa to obtain a high-strength heat-treatment-free aluminum alloy.
[0060] According to the above preparation method, 6 groups of high-strength heat-treatment-free aluminum alloys were prepared. In this comparative example, Al-Ce was not added, and the modification effect was not good. The size of α-Al became large and the dendrites were not completely transformed into spherical crystals. The properties are shown in Table 5:
[0061] Table 5 Performance indicators of the high-strength heat-treatment-free aluminum alloy in Comparative Example 1.
[0062]
[0063] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A high-strength heat-treatment-free aluminum alloy of recycled aluminum alloy, Features: The high-strength heat-treatment-free aluminum alloy has the following composition by mass percentage: Si: 8.1-9%; Mg: 0.38-0.45%; Ti: 0.15-0.17%; Ce: 0.01-0.03%; Fe: 0.14-0.2%; Mn: 0.58-0.6%; Cu: 0.1-0.14%; V: 0.01-0.02%; Sr: 0.025-0.028%; the rest is aluminum and inevitable impurities.
2. The high-strength heat-treatment-free aluminum alloy of the recycled aluminum alloy according to claim 1, Features: The high-strength heat-treatment-free aluminum alloy has the following composition by mass percentage: Si: 8.5-9%; Mg: 0.4-0.45%; Ti: 0.15-0.16%; Ce: 0.02-0.03%; Fe: 0.14-0.17%; Mn: 0.58-0.6%; Cu: 0.11-0.14%; V: 0.01-0.02%; Sr: 0.025-0.026%; the rest is aluminum and inevitable impurities.
3. A method for preparing a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy according to claim 1 or 2, Features: An aluminum source is placed in a smelting furnace to melt to obtain an aluminum melt, and then other intermediate alloy raw materials are added into the smelting furnace according to the designed proportion to melt to obtain an aluminum alloy melt, and the aluminum alloy melt is refined and degassed; then Al-Ti-B is added for grain refinement, and then Al-Sr and Al-Ce are added for modification to obtain an aluminum alloy liquid, and finally the aluminum alloy is hydraulically cast into a mold.
4. The method for preparing a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy according to claim 3, Features: The aluminum source is recycled A356 aluminum alloy prepared from waste aluminum; The aluminum source is placed in a smelting furnace and melted at 715-725° C. to obtain an aluminum melt.
5. The method for preparing a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy according to claim 3, Features: The other master alloy raw materials are preheated to 220°C-250°C, and then added into a melting furnace and heated to 750-760°C for melting to obtain an aluminum alloy melt.
6. A method for preparing a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy according to claim 3 or 5, Features: The order of adding the other master alloy raw materials is: first add silicon source, manganese source, iron source, copper source, and vanadium source; then add magnesium source 4-6 minutes before refining; The manganese source is selected from Al-Mn, the iron source is selected from Al-Fe, the vanadium source is selected from Al-V, the silicon source is selected from Al-Si, the copper source is selected from Al-Cu, and the magnesium source is selected from pure magnesium.
7. The method for preparing a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy according to claim 3, Features: When the temperature of the aluminum alloy melt is 710-730°C, a refining agent is added into the smelting furnace for refining; The degassing process is to introduce a protective atmosphere into the aluminum alloy melt, control the pressure of the protective atmosphere to 0.25-0.4Mpa, and stir to degas.
8. The method for preparing a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy according to claim 3, Features: The aluminum alloy melt is refined and degassed under stirring, then allowed to stand for the first time, and then Al-Ti-B is added and stirred for grain refinement. After 4-6 minutes, Al-Sr and Al-Ce are added for modification, and allowed to stand for the second time to obtain aluminum alloy liquid.
9. The method for preparing a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy according to claim 8, Features: The first and second resting times are both 15-30 minutes; The Al-Ti-B, Al-Sr and Al-Ce are all preheated to 220° C.-250° C. and then added into the aluminum alloy melt.
10. The method for preparing a high-strength heat-treatment-free aluminum alloy of a recycled aluminum alloy according to claim 3, Features: The die-casting method is vacuum high-pressure casting, and the pressure of the vacuum high-pressure casting is 8-12 MPa.
Citation Information
Patent Citations
Non-heat-treatment reinforced high-strength and high-toughness die-casting aluminum-silicon alloy and preparation method thereof
CN114411020A
Heat-treatment-free high-toughness cast aluminum alloy as well as preparation method and application thereof
CN115287506A
Die-casting aluminum alloy and preparation method thereof
CN117965968A
Low-cost heat-treatment-free high-toughness die-casting aluminum alloy and preparation method thereof
CN117987697A
Cited By
Preparation method of heat-treatment-free secondary aluminum-silicon alloy
CN120536763A
Preparation method of tough A356 regenerated aluminum alloy with high iron content and regenerated aluminum alloy