Dopamine carbon coated P2 type sodium ion battery layered oxide positive electrode material and preparation method and application thereof
The dopamine carbon coating technology improves the cycle stability of P2-type sodium-ion battery cathode materials, solves the problem of performance degradation caused by electrolyte erosion and transition metal dissolution in the existing technology during long-term use, and achieves better Battery performance is maintained.
Patent Information
- Application Number
- CN202410970333.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-25
Smart Images

Figure HDA0004952982600000011 
Figure HDA0004952982600000012 
Figure HDA0004952982600000021
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a dopamine carbon-coated P2 type sodium ion battery layered oxide positive electrode material, and a preparation method and application thereof. Background Art
[0002] Renewable energy is becoming increasingly important for sustainable development. Among various energy-saving storage systems, electrochemical energy technology is considered to be the most effective way. For example, lithium-ion batteries have been widely used in all aspects of social life due to their high energy density, environmental friendliness, and long cycle life. However, its further development is largely restricted by the shortage of lithium resources and rising costs. In order to solve the huge market demand problem at a low cost, sodium-ion batteries have attracted much attention due to their abundant reserves and similar chemical properties to lithium-ion batteries. In addition, the intercalation and deintercalation mechanisms of lithium-ion batteries and sodium-ion batteries are similar. Therefore, similar synthesis strategies and material development can also be applied to the development of sodium-ion battery electrode materials.
[0003] So far, the research and results on the positive electrode materials of sodium ion batteries have shown a straight upward trend. Prussian blue analogs, organic compounds, polyanion compounds and layered transition metal oxides are the main positive electrode materials of sodium ion batteries. Among them, layered metal oxides have the advantages of easy synthesis, large theoretical capacity and high working voltage. However, the poor cycle stability caused by the irreversible phase change during the charge and discharge process and the poor air stability themselves hinder their practical application in sodium ion batteries. Prussian blue compounds have attracted widespread attention due to their simple synthesis method, stable structure and rich and diverse active centers. However, the vacancies contained in their structure will increase the coordination number of water molecules and manganese ions, which will hinder the migration of sodium ions to a certain extent. At the same time, they often lead to the appearance of crystal water during synthesis, which will seriously affect the performance of the battery. Even if the crystal water is dissolved in the electrolyte, it will also threaten the safety of the battery. Polyanion compounds have good structural stability and cycle stability, but their relative molecular mass is large, resulting in a low energy density of the battery.
[0004] Sodium-based layered materials can be divided into two categories: P-type or O-type, in which the sodium ions are placed in prismatic or octahedral positions, respectively. Depending on the sodium stoichiometry and the synthesis temperature, Na xMO2 is further divided into three types: P2, P3 and O3 (O3: ABCABC stacking, P2: ABBA stacking, P3: ABBCCA stacking). Among P-type materials, the most studied are P2-type layered materials, while among O3-type materials, the most studied are O3-type layered materials. For the O3-type structure, since the sodium content is higher than that of the P2-type structure, it has a higher energy density than the P2-type structure in the full battery, but for the O3 structure, the migration of Na ions from one octahedral site to the adjacent octahedral site is slow, and it is necessary to overcome a high energy barrier, and phase changes and complex chemical changes will inevitably occur, resulting in structural damage and rapid decline in battery performance. In sharp contrast, P2-type materials have a lower diffusion barrier during the migration process because the sodium ions in P2-type materials occupy a wider triangular prism than O3-type materials, so they have better rate performance. In addition, P2-type materials only undergo one phase change (P-type to O-type) during the charge and discharge process, avoiding structural changes and thus having better stability. However, during long cycles, side reactions between the material and the electrolyte lead to the dissolution of transition metal ions and the generation of lattice cracks, which reduces battery performance and limits its practical application. 0.67 Co 0.5 Mn 0.5 O2 has attracted wide attention due to its high capacity and good rate performance. The P2-type Na 0.67 Co 0.5 Mn 0.5 At a rate of 0.1C, the discharge capacity of O2 can reach 141 mAh g -1 However, its capacity retention rate is not ideal. This may be due to the fact that when the P2-type layered material is charged to a high voltage range, the electrolyte corrodes the active material, the electrolyte decomposes on the electrode surface, and the transition metal in the material dissolves out. Summary of the invention
[0005] In order to overcome the shortcomings and deficiencies of the poor cycle performance of the layered positive electrode materials of ion batteries in the prior art, the primary purpose of the present invention is to provide a method for preparing a dopamine carbon-coated P2-type sodium ion battery layered oxide positive electrode material; in this method, the coating material is selected as dopamine, and the coating material can protect the interface on the surface of the positive electrode material and inhibit the decomposition of the electrolyte, thereby improving the P2-Na 0.67 Co 0.5 Mn 0.5 Cycling stability of layered oxide cathode materials for O2 sodium-ion batteries.
[0006] Another object of the present invention is to provide a dopamine carbon-coated P2 type sodium ion battery layered oxide positive electrode material prepared by the above preparation method.
[0007] Another object of the present invention is to provide an application of the above-mentioned dopamine carbon-coated P2 type sodium ion battery layered oxide positive electrode material.
[0008] The purpose of the present invention is achieved through the following technical solutions:
[0009] A method for preparing a dopamine carbon-coated P2-type sodium ion battery layered oxide positive electrode material comprises the following steps:
[0010] (1) According to the chemical formula Na 0.67 Co 0.5 Mn 0.5 O2 takes the corresponding amount of sodium source, cobalt source and manganese source and puts them into a corundum ball mill to obtain a precursor; the obtained precursor is placed in a tubular furnace, heated to 900°C at a heating rate of 5°C, and kept at this temperature for 12 hours for high-temperature sintering to obtain P2-Na 0.67 Co 0.5 Mn 0.5 O2 sodium-ion battery layered oxide cathode materials;
[0011] (2) P2-Na 0.67 Co 0.5 Mn 0.5 The layered oxide positive electrode material of the O2 sodium ion battery is dissolved in a Tris-HCL buffer solution of pH=8.5, and ultrasonic treatment is performed to uniformly disperse the positive electrode material in the buffer solution to obtain a dispersion;
[0012] (3) dissolving dopamine hydrochloride in the dispersion obtained in step (2), subjecting the mixture to ultrasonic treatment to uniformly disperse the dopamine hydrochloride in the buffer solution, and then placing the mixture on a magnetic stirrer and subjecting the mixture to magnetic stirring at 600 rpm for 24 h at room temperature to completely coat the cathode material with dopamine; filtering and washing the obtained mixed solution, and placing the mixture in a vacuum oven for drying to obtain a powder;
[0013] (4) The powder obtained in step (3) is placed in a corundum ark, and then placed in a muffle furnace for sintering, heated to 500°C at a heating rate of 5°C / min, kept warm for 6 hours, and then naturally cooled to room temperature and taken out for grinding to obtain a dopamine carbon-coated P2 type sodium ion battery layered oxide positive electrode material.
[0014] In step (1), the sodium source is one or more of sodium carbonate, sodium hydroxide, sodium acetate, sodium nitrate, and sodium citrate; the manganese source is one or more of manganese acetate, manganese dioxide, and manganese carbonate; and the cobalt source is one or more of cobalt acetate, cobalt oxide, and cobalt carbonate.
[0015] The rotation speed of the ball mill in step (1) is 500 r / min, the ball milling time is 10 h, and the ball-to-material mass ratio is 30:1.
[0016] The concentration of the buffer in step (2) is 10 mmol / L; the time of the ultrasonic treatment is 1 h.
[0017] In step (3), the mass ratio of dopamine hydrochloride to the positive electrode material in the dispersion is 0.01-0.05:1; the ultrasonic treatment time is 1 hour; the drying temperature of the drying treatment is 60°C-80°C, and the drying time is 18h-24h.
[0018] A dopamine carbon-coated P2-type sodium ion battery layered oxide positive electrode material prepared by the above-mentioned preparation method.
[0019] The application of the above-mentioned dopamine carbon-coated P2 type sodium ion battery layered oxide positive electrode material in the preparation of sodium ion battery positive electrode.
[0020] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0021] (1) The method for modifying the P2-type sodium ion battery layered oxide positive electrode material by carbon coating of dopamine proposed in the present invention has a simple implementation method and a simple process flow. The raw materials used can all be cheap, non-toxic, and pollution-free products, which has great cost and environmental advantages.
[0022] (2) In the present invention, dopamine is coated on the surface of the sodium ion battery layered positive electrode, and after sintering, a carbon-coated modified sodium ion battery layered positive electrode Na is obtained. 0.67 Co 0.5 Mn 0.5 O2@DA, the coating layer can isolate the direct contact between the positive electrode material and the electrolyte, avoid corrosion and failure of the positive electrode material, and effectively improve the cycle stability of the battery.
[0023] (3) The method for modifying the sodium ion battery layered positive electrode material by carbon coating of dopamine proposed in the present invention can control the thickness of the coating layer by adjusting the mass ratio of dopamine to the sodium ion battery layered positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is Na in Example 1 0.67 Co 0.5 Mn 0.5 O2 and Na 0.67 Co 0.5 Mn 0.5 XRD pattern of O2@DA-1%.
[0025] Figure 2 is Na in Example 1 0.67 Co 0.5 Mn 0.5SEM image of O2.
[0026] Figure 3 is Na in Example 1 0.67 Co 0.5 Mn 0.5 SEM image of O2@DA-1%.
[0027] Figure 4 is Na in Example 1 0.67 Co 0.5 Mn 0.5 The cycle life of O2 in the voltage range of 1.5-4.3V and the rate of 0.1C.
[0028] Figure 5 is Na in Example 1 0.67 Co 0.5 Mn 0.5 Cycle life diagram of O2@DA-1% in the voltage range of 1.5-4.3V and the rate of 0.1C. DETAILED DESCRIPTION
[0029] The present invention is further described below with reference to specific embodiments, but they should not be construed as limiting the present invention.
[0030] Embodiment 1:
[0031] Synthesis of 0.02 mol of P2-Na 0.67 Co 0.5 Mn 0.5 O2, according to the chemical formula Na 0.67 Co 0.5 Mn 0.5 Take the corresponding amount of sodium acetate (5% excess), manganese acetate and cobalt acetate, put them into a corundum ball mill, the ball-to-material ratio is 1:30, the rotation speed is 500r / min, after ball milling for 10h, put the obtained precursor into a tube furnace, heat it to 900℃ at a heating rate of 5℃, keep it warm for 12h for high temperature sintering, and obtain P2-Na 0.67 Co 0.5 Mn 0.5 O 22 Sodium ion battery layered oxide positive electrode material. 0.67 Co 0.5 Mn 0.5 O 22The layered oxide positive electrode material of the sodium ion battery is dissolved in a Tris-HCL buffer solution with a pH of 8.5, placed in a beaker, and ultrasonically treated for 1 hour to uniformly disperse the positive electrode material in the buffer solution to obtain a dispersion. 0.002 mol of dopamine hydrochloride is dissolved in the above dispersion solution and ultrasonically treated for 1 hour to uniformly disperse the dopamine hydrochloride in the buffer solution; a suitable rotor is placed in the beaker and placed on a magnetic stirrer, and stirred at room temperature at a speed of 600 rpm for 24 hours to ensure that dopamine is completely coated on the positive electrode material. The mixed solution obtained after magnetic stirring is filtered and washed, and placed in a vacuum oven for drying under vacuum conditions of 80°C. The powder obtained after drying is placed in a corundum ark, and then placed in a muffle furnace for sintering, heated to 500°C at a heating rate of 5°C / min, kept warm for 6 hours, and naturally cooled to room temperature before being taken out and ground to obtain Na 0.67 Co 0.5 Mn 0.5 O2@DA-1%.
[0032] The P2-Na 0.67 Co 0.5 Mn 0.5 O2 sodium ion battery layered oxide positive electrode material and coated modified positive electrode material Na 0.67 Co 0.5 Mn 0.5 O2@DA-1% was mixed with a conductive agent (Ketjen black) and a binder (PVDF) in a mass ratio of 7:2:1, and then an appropriate amount of N-methylpyrrolidone was added to form a slurry, which was evenly coated on an aluminum foil, and then placed in a vacuum oven and dried at 80°C for 8 hours under vacuum conditions. After drying, it was cut into a circular positive electrode sheet with a diameter of 10 mm using a cutting machine. The positive electrode sheet was assembled with a separator, a sodium sheet, a spring and a gasket using sodium perchlorate as the electrolyte to obtain a button cell, and XRD and electrochemical performance tests were performed.
[0033] Figure 1 The XRD diagram shown shows that the diffraction peaks of the synthesized sample are sharp, corresponding to the standard PDF card one by one, and there are no obvious impurity peaks, proving that Na 0.67 Co 0.5 Mn 0.5 O2 positive electrode material.
[0034] Figure 2 The Na 0.67 Co 0.5 Mn 0.5 The SEM image of O2 shows that the synthesized sample particles are uniform in size, have a layered structure, and have a smooth surface without obvious cracks.
[0035] Figure 3 The Na 0.67 Co 0.5Mn 0.5 The SEM image of O2@DA-1% shows that the synthesized sample particles are uniform in size, have a layered structure, and have an obvious coating layer on the surface, indicating that dopamine is successfully coated on the surface of the positive electrode material.
[0036] Figure 4 ShownNa 0.67 Co 0.5 Mn 0.5 The cycle life of O2 at 0.1C rate shows that the initial capacity is 141.62 mAh g -1 After about 40 cycles, the capacity is 87 mAh g -1 , the capacity retention rate is 61.4%.
[0037] Figure 5 ShownNa 0.67 Co 0.5 Mn 0.5 The cycle life of O2@DA-1% at 0.1C rate shows that the initial capacity is 155.61 mAh g -1 After about 40 cycles, the capacity is 104.24 mAh g -1 , the capacity retention rate is 67%, compared with the unmodified Na 0.67 Co 0.5 Mn 0.5 O2 has better cycle stability.
[0038] Embodiment 2:
[0039] Synthesis of 0.02 mol of P2-Na 0.67 Co 0.5 Mn 0.5 O2, according to the chemical formula Na 0.67 Co 0.5 Mn 0.5 Take the corresponding amount of sodium acetate (5% excess), manganese acetate and cobalt acetate, put them into a corundum ball mill, the ball-to-material ratio is 1:30, the rotation speed is 500r / min, after ball milling for 10h, put the obtained precursor into a tube furnace, heat it to 900℃ at a heating rate of 5℃, keep it warm for 12h for high temperature sintering, and obtain P2-Na 0.67 Co 0.5 Mn 0.5 O2 sodium ion battery layered oxide positive electrode material. 0.67 Co 0.5 Mn 0.5The layered oxide positive electrode material of the O2 sodium ion battery is dissolved in a Tris-HCL buffer solution with a pH of 8.5, placed in a beaker, and ultrasonically treated for 1 hour to uniformly disperse the positive electrode material in the buffer solution to obtain a dispersion. 0.006 mol of dopamine hydrochloride is dissolved in the above dispersion solution and ultrasonically treated for 1 hour to uniformly disperse the dopamine hydrochloride in the buffer solution; a suitable rotor is placed in the beaker and placed on a magnetic stirrer, and stirred at room temperature at a speed of 600 rpm for 24 hours to ensure that dopamine is completely coated on the positive electrode material. The mixed solution obtained after magnetic stirring is filtered and washed, and placed in a vacuum oven for drying under vacuum conditions at 80°C. The powder obtained after drying is placed in a corundum ark, and then placed in a muffle furnace for sintering, heated to 500°C at a heating rate of 5°C / min, kept warm for 6 hours, and naturally cooled to room temperature before being taken out and ground to obtain Na 0.67 Co 0.5 Mn 0.5 O2@DA-3%.
[0040] Embodiment 3:
[0041] Synthesis of 0.02 mol of P2-Na 0.67 Co 0.5 Mn 0.5 O 2, Sodium acetate (5% excess), manganese acetate and cobalt acetate were placed in a corundum ball mill in a certain proportion, with a ball-to-material ratio of 1:30 and a rotation speed of 500r / min. After ball milling for 10 hours, the obtained precursor was placed in a tubular furnace and heated to 900°C at a heating rate of 5°C. The temperature was kept for 12 hours for high-temperature sintering to obtain P2-Na 0.67 Co 0.5 Mn 0.5 O2 sodium ion battery layered oxide positive electrode material. 0.67 Co 0.5 Mn 0.5 The layered oxide positive electrode material of the O2 sodium ion battery is dissolved in a Tris-HCL buffer solution with a pH of 8.5, placed in a beaker, and ultrasonically treated for 1 hour to uniformly disperse the positive electrode material in the buffer solution to obtain a dispersion. 0.01 mol of dopamine hydrochloride is dissolved in the above dispersion solution and ultrasonically treated for 1 hour to uniformly disperse the dopamine hydrochloride in the buffer solution; a suitable rotor is placed in the beaker and placed on a magnetic stirrer, and stirred at room temperature at a speed of 600 rpm for 24 hours to ensure that dopamine is completely coated on the positive electrode material. The mixed solution obtained after magnetic stirring is filtered and washed, and placed in a vacuum oven for drying under vacuum conditions of 80°C. The powder obtained after drying is placed in a corundum ark, and then placed in a muffle furnace for sintering, heated to 500°C at a heating rate of 5°C / min, kept warm for 6 hours, and naturally cooled to room temperature before being taken out and ground to obtain Na 0.67 Co0.5 Mn 0.5 O2@DA-5%.
[0042] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a dopamine carbon-coated P2-type sodium ion battery layered oxide positive electrode material, characterized in that The following steps are involved: (1) According to the chemical formula Na 0.67 Co 0.5 Mn 0.5 O2 takes the corresponding amount of sodium source, cobalt source and manganese source and puts them into a corundum ball mill to obtain a precursor; the obtained precursor is placed in a tubular furnace, heated to 900°C at a heating rate of 5°C, and kept at this temperature for 12 hours for high-temperature sintering to obtain P2-Na 0.67 Co 0.5 Mn 0.5 O2 sodium-ion battery layered oxide cathode materials; (2) P2-Na 0.67 Co 0.5 Mn 0.5 The layered oxide positive electrode material of the O2 sodium ion battery is dissolved in a Tris-HCL buffer solution of pH=8.5, and ultrasonic treatment is performed to uniformly disperse the positive electrode material in the buffer solution to obtain a dispersion; (3) dissolving dopamine hydrochloride in the dispersion obtained in step (2), subjecting the mixture to ultrasonic treatment to uniformly disperse the dopamine hydrochloride in the buffer solution, and then placing the mixture on a magnetic stirrer and subjecting the mixture to magnetic stirring at 600 rpm for 24 h at room temperature to completely coat the cathode material with dopamine; filtering and washing the obtained mixed solution, and placing the mixture in a vacuum oven for drying to obtain a powder; (4) The powder obtained in step (3) is placed in a corundum ark, and then placed in a muffle furnace for sintering, heated to 500°C at a heating rate of 5°C / min, kept warm for 6 hours, and then naturally cooled to room temperature and taken out for grinding to obtain a dopamine carbon-coated P2 type sodium ion battery layered oxide positive electrode material.
2. The method for preparing a dopamine carbon-coated P2-type sodium ion battery layered oxide positive electrode material according to claim 1, characterized in that: In step (1), the sodium source is one or more of sodium carbonate, sodium hydroxide, sodium acetate, sodium nitrate, and sodium citrate; the manganese source is one or more of manganese acetate, manganese dioxide, and manganese carbonate; and the cobalt source is one or more of cobalt acetate, cobalt oxide, and cobalt carbonate.
3. The method for preparing a dopamine carbon-coated P2-type sodium ion battery layered oxide positive electrode material according to claim 1, characterized in that: The rotation speed of the ball mill in step (1) is 500 r / min, the ball milling time is 10 h, and the ball-to-material mass ratio is 30:
1.
4. The method for preparing a dopamine carbon-coated P2-type sodium ion battery layered oxide positive electrode material according to claim 1, characterized in that: The concentration of the buffer in step (2) is 10 mmol / L; the time of the ultrasonic treatment is 1 h.
5. The method for preparing a dopamine carbon-coated P2-type sodium ion battery layered oxide positive electrode material according to claim 1, characterized in that: In step (3), the mass ratio of dopamine hydrochloride to the positive electrode material in the dispersion is 0.01-0.05:1; the ultrasonic treatment time is 1 hour; the drying temperature of the drying treatment is 60°C-80°C, and the drying time is 18h-24h.
6. A dopamine carbon-coated P2-type sodium ion battery layered oxide positive electrode material prepared by the preparation method according to any one of claims 1 to 5.
7. Use of the dopamine carbon-coated P2-type sodium ion battery layered oxide positive electrode material according to claim 6 in the preparation of a sodium ion battery positive electrode.
Citation Information
Patent Citations
Electrode materials comprising a lamellar oxide of sodium and of metal, electrodes comprising same and use of same in electrochemistry
CN112913052A
Preparation method of Ca-doped sodium ion battery layered oxide positive electrode material
CN116789183A
Cited By
Multi-element doped P2 type layered oxide and preparation method thereof
CN121172124A