Preparation method of TC4 titanium alloy seamless tube
Through the improved extrusion-rolling process, including high vacuum melting and hot hydrogen treatment, the problems of difficult production and low yield of TC4 titanium alloy seamless pipes are solved, and the batch preparation and excellent mechanical properties of titanium alloy seamless pipes are achieved .
Patent Information
- Application Number
- CN202410818228.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-24
AI Technical Summary
TC4 titanium alloy seamless pipes have high deformation resistance and strong work hardening, which makes production difficult and batch preparation difficult. It also has high equipment requirements, high losses, and low yield.
An improved extrusion-rolling process is adopted, including high-vacuum non-consumable electric arc furnace melting, double-layer cladding extrusion, thermal hydrogen treatment, alternating cold and hot rolling processes, controlling the melting method and rolling parameters, and optimizing the annealing treatment. Realize the batch preparation of titanium alloy seamless tubes.
Through this method, the titanium alloy forming temperature is reduced, the plasticity is improved, equipment requirements and losses are reduced, the yield is improved, and a uniform structure and excellent mechanical properties are obtained.
Smart Images

Figure CN118847747A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of titanium alloy seamless pipes and preparation methods thereof, and specifically relates to a preparation method of a TC4 titanium alloy seamless pipe. Background Art
[0002] TC4 (Ti-6Al-4V) is a typical α-type two-phase titanium alloy with the advantages of high specific strength, low density, good thermal stability and corrosion resistance. It can be made into titanium alloy seamless pipes, which have broad application prospects in many fields such as marine engineering, shipbuilding, aerospace, chemical industry, automobile and electric power.
[0003] There are many methods for manufacturing titanium and titanium alloy tubes, mainly including: hot extrusion, hot rolling, cold deformation and welding or a combination of multiple methods.
[0004] TC4 titanium alloy has high deformation resistance, strong work hardening, and is easy to crack, which makes it difficult to produce seamless pipes. In addition, the batch preparation of TC4 titanium alloy seamless pipes is difficult, and the equipment requirements are high, the loss is large, and the yield rate is low.
[0005] Based on the above, it is necessary to develop a preparation method for TC4 titanium alloy seamless pipe that is simple to produce, can be mass-produced and has good performance. Summary of the invention
[0006] Based on this, in view of the above-mentioned deficiencies in the prior art, a method for preparing a TC4 titanium alloy seamless tube is provided, which improves the TC4 alloy tube extrusion-rolling process and aims to provide a feasible preparation process for the industrial production of TC4 titanium alloy seamless tube.
[0007] In order to achieve the above purpose, the following technical solutions are adopted: The present invention provides a method for preparing a TC4 titanium alloy seamless pipe, comprising the following steps: S101. Raw materials for preparing TC4 titanium alloy: 0A grade small particles of titanium sponge, AlV55 alloy and aluminum particles; S102. The raw materials 0A grade small particles of titanium sponge, AlV55 alloy and aluminum particles are placed in a high vacuum non-consumable arc furnace and evacuated; S103. A high vacuum non-consumable arc furnace is first filled with hydrogen and then with argon to start smelting to obtain a TC4 titanium alloy ingot; S104. The TC4 titanium alloy ingot is forged to obtain an extrusion billet raw material; the extrusion billet raw material billet surface is double-clad with copper and iron, extruded, and the billet is air-cooled to room temperature after extrusion; and then the billet is annealed; S105. The tube is hot rolled; S106. The tube is cold rolled; S107. Repeat S105 to S106 until a TC4 titanium alloy seamless tube that meets the size requirements is obtained, and then perform annealing to obtain a finished TC4 titanium alloy seamless tube.
[0008] In some embodiments, the annealing treatment in S104 is: heating to 850-900° C. at 10° C. / min in a horizontal vacuum annealing furnace for 2-3 hours, then cooling the furnace to 500° C. and then air cooling to room temperature.
[0009] In some embodiments, the annealing treatment in S107 is: heating the TC4 titanium alloy seamless tube to 550-580° C. at a rate of 7-10° C. / min in a horizontal vacuum annealing furnace, annealing for 1-1.5 hours, and then cooling the furnace to room temperature.
[0010] In some embodiments, in S101, 880-920 kg of 0A grade small particle titanium sponge is fed, 50-70 kg of AlV55 alloy is fed, and 30-50 kg of aluminum particles are fed.
[0011] In some embodiments, the extrusion process in S104 includes: heating the double-layer-encased extrusion blank raw material to 860-920° C. and keeping it warm for 1-2 hours before extruding, with an extrusion ratio of 6-9 and an extrusion speed controlled at 60-80 mm / s.
[0012] In some embodiments, S102 of “placing raw materials of 0A grade small-particle titanium sponge, AlV55 alloy and aluminum particles into a high vacuum non-consumable arc furnace and evacuating the furnace” includes: Put the raw materials of 0A grade small-particle titanium sponge, AlV55 alloy and aluminum particles into the copper crucible of a high vacuum non-consumable arc furnace, close the furnace door, start the mechanical pump, turn on the digital vacuum gauge, open the pre-evacuation valve, and wait until the vacuum degree in the furnace drops to 5×10 -3 When the speed reaches 0, close the main pumping valve, the stop valve, and the digital vacuum gauge. When the speed of the molecular pump reaches zero, turn off the power supply of the molecular pump. In some embodiments, S103 of “first charging hydrogen into a high vacuum non-consumable arc furnace, and then charging argon, and starting smelting to obtain a TC4 titanium alloy ingot” includes: Open the charging valve and keep the mechanical pump on to prevent air from entering the charging pipe. Wait until the vacuum in the furnace reaches 5x10 -4 Pa, close the charging valve, turn off the mechanical pump, open the hydrogen bottle and the charging valve, when the total gas pressure in the furnace is -0.05MPa, fill in 0.01Mpa hydrogen, then open the argon bottle and fill in 0.04MPa argon.
[0013] In some embodiments, the volume ratio of hydrogen to the total volume of the gas in the furnace is 20%.
[0014] In some embodiments, in S104, the TC4 titanium alloy ingot is forged six times to obtain an extrusion billet raw material.
[0015] In some embodiments, the hot rolling parameters of S105 include: hot rolling temperature of 900-950°C, deformation of each pass controlled at 30-50%, final rolling temperature requirement ≥800°C, feed amount of each pass 3-5mm / time, and rolling speed 80-100 times / minute.
[0016] In some embodiments, the cold rolling parameters of S106 include: the deformation of each cold rolling pass is controlled at 20-30%, the rolling speed is 40-60 times / minute, the intermediate annealing temperature is 800-850°C, and the annealing time is 1.5-2.5h.
[0017] The present invention has the following beneficial technical effects: The preparation method of the TC4 titanium alloy seamless tube disclosed in the present invention realizes batch preparation of the TC4 titanium alloy seamless tube by controlling the process paths such as smelting mode, extrusion and rolling, thereby solving the problems of the tube being difficult to produce and easy to crack due to its large deformation resistance and strong work hardening.
[0018] The preparation method of the TC4 titanium alloy seamless tube disclosed in the present invention adopts a high vacuum non-consumable smelting method to obtain a more uniform ingot, with a short smelting time, and is suitable for the smelting of refractory metals such as titanium; The preparation method of the TC4 titanium alloy seamless pipe disclosed in the invention reduces the forming temperature of the titanium alloy through a thermal hydrogen treatment process and improves the plasticity of the titanium alloy.
[0019] The preparation method of the TC4 titanium alloy seamless tube disclosed in the present invention adopts a cold and hot rolling alternating rolling method, which reduces the cost of the pure hot rolling process and optimizes the structure and performance of the tube during the cold rolling annealing process.
[0020] The preparation method of the TC4 titanium alloy seamless pipe disclosed in the invention comprises the following steps: subjecting a titanium alloy extruded billet to double-layer sheathing, heating and extruding, so as to realize batch preparation of the titanium alloy seamless pipe. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 It is a flow chart of the method for preparing the TC4 titanium alloy seamless pipe of the present invention; Figure 2The microstructure diagram of the finished tube of the titanium alloy seamless tube of Example 1 of the present invention; wherein (a) is a colored microstructure diagram of the finished tube; (b) is a grayscale microstructure diagram of the finished tube; Figure 3 The microstructure diagram of the finished tube of the titanium alloy seamless tube of Example 2 of the present invention; wherein (a) is a colored microstructure diagram of the finished tube; (b) is a grayscale microstructure diagram of the finished tube; Figure 4 The microstructure diagram of the finished tube of the titanium alloy seamless tube of the comparative example of the present invention; wherein (a) is a colored microstructure diagram of the finished tube; and (b) is a grayscale microstructure diagram of the finished tube. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in combination with specific embodiments and with reference to the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0024] like Figure 1 The method for preparing the TC4 titanium alloy seamless pipe shown comprises the following steps: S101, preparing raw materials for preparing TC4 titanium alloy: 0A grade small particle titanium sponge, AlV55 alloy and aluminum particles; S102, placing raw materials of 0A grade small-particle titanium sponge, AlV55 alloy and aluminum particles into a high vacuum non-consumable arc furnace and evacuating the furnace; S103, first filling hydrogen into a high vacuum non-consumable arc furnace, and then filling argon into the furnace, and starting smelting to obtain a TC4 titanium alloy ingot; S104, forging the TC4 titanium alloy ingot to obtain an extrusion billet raw material; after the billet surface of the extrusion billet raw material is double-clad with copper and iron, extrusion is performed, and the tube billet after extrusion is air-cooled to room temperature; and then the tube billet is annealed; S105, hot rolling the tube blank; S106, cold rolling the tube blank; S107, repeating steps S105 to S106 until a TC4 titanium alloy seamless tube that meets the size requirements is obtained, and then performing annealing treatment to obtain a finished TC4 titanium alloy seamless tube.
[0025] The alternating hot and cold rolling method is adopted to reduce the cost of pure hot rolling process, and at the same time optimize the structure and performance of the pipe during the cold rolling annealing process.
[0026] Furthermore, the annealing treatment in step S104 is: heating to 850-900° C. at 10° C. / min in a horizontal vacuum annealing furnace for 2-3 hours, then cooling the furnace to 500° C. and then air cooling to room temperature.
[0027] Furthermore, the annealing treatment in step S107 is: heating the TC4 titanium alloy seamless tube to 550-580° C. at a rate of 7-10° C. / min in a horizontal vacuum annealing furnace, annealing for 1-1.5 hours, and then cooling the furnace to room temperature.
[0028] Further, in step S104, the TC4 titanium alloy ingot is forged for 6 times to obtain an extrusion blank raw material. The extrusion process in step S104 includes: heating the extrusion blank raw material after the double-layer sheathing to 860-920°C and keeping it for 1-2 hours before extrusion, the extrusion ratio is 6-9, and the extrusion speed is controlled at 60-80 mm / s.
[0029] The titanium alloy extruded billet is double-jacketed, heated and extruded. The batch preparation of titanium alloy seamless pipes is achieved by controlling the heating method, heating temperature, insulation time, extrusion ratio, pressurization speed and other process parameters of the extruded billet. The jacketing process reduces the extrusion force required during extrusion, reduces the requirements for equipment, has low loss and high yield rate.
[0030] Further, step S102 of "placing the raw materials of 0A grade small-particle titanium sponge, AlV55 alloy and aluminum particles into a high vacuum non-consumable arc furnace and evacuating the furnace" includes: Put the raw materials of 0A grade small-particle titanium sponge, AlV55 alloy and aluminum particles into the copper crucible of a high vacuum non-consumable arc furnace, close the furnace door, start the mechanical pump, turn on the digital vacuum gauge, open the pre-evacuation valve, and wait until the vacuum degree in the furnace drops to 5×10 -3 When the speed reaches 0, close the main pumping valve, the stop valve, and the digital vacuum gauge. When the speed of the molecular pump reaches zero, turn off the power supply of the molecular pump. Further, step S103 of "first filling hydrogen into the high vacuum non-consumable arc furnace, and then filling argon, starting smelting to obtain a TC4 titanium alloy ingot" includes: Open the charging valve and keep the mechanical pump on to prevent air from entering the charging pipe. Wait until the vacuum in the furnace reaches 5x10 -4 Pa, close the charging valve, turn off the mechanical pump, turn on the gas analysis system, open the hydrogen bottle and the charging valve, and when the total gas pressure in the furnace is -0.05MPa, fill in 0.01Mpa hydrogen and then open the argon bottle to fill in 0.04MPa argon. The volume ratio of hydrogen to the total volume of the gas in the furnace is 20%. During the whole process, the ratio of hydrogen to argon is controlled by the gas analysis system.
[0031] Hydrogen has always been regarded as a harmful element in metal structural materials because it can cause hydrogen embrittlement in materials. However, hydrogen can also be used as a temporary alloying element to improve the processing properties of alloys. The thermal hydrogen treatment process can reduce the forming temperature of titanium alloys and improve the plasticity of titanium alloys.
[0032] Furthermore, in step S104, the TC4 titanium alloy ingot is subjected to six-time forging to obtain an extrusion billet raw material.
[0033] Furthermore, the hot rolling parameters of step S105 include: hot rolling is carried out by a hot rolling mill, the hot rolling temperature is 900-950°C, the deformation amount of each pass is controlled at 30-50%, the final rolling temperature is required to be ≥800°C, the feed amount of each pass is 3-5mm / time, and the rolling speed is 80-100 times / minute.
[0034] Furthermore, the cold rolling parameters of step S106 include: the deformation amount of each cold rolling pass is controlled at 20-30%, the rolling speed is 40-60 times / minute, the intermediate annealing temperature is 800-850°C, and the annealing time is 1.5-2.5h.
[0035] Further, step S102 includes: smelting is performed using a high vacuum non-consumable arc furnace. First, the circulating water is started, the power supply of the equipment is started, the furnace door is opened, and after the smelting furnace is cleaned, the raw materials of 0A grade small particles of sponge titanium, AlV55 alloy, and aluminum particles are placed in a copper crucible.
[0036] The high vacuum non-consumable melting method can obtain a more uniform ingot with a short melting time, which is suitable for the melting of refractory metals such as titanium.
[0037] The present invention is further illustrated by the following examples.
[0038] Example 1 A method for preparing a TC4 titanium alloy seamless tube, the specific implementation steps are as follows: (1) Smelting is carried out in a high vacuum non-consumable arc furnace. First, start the circulating water, start the equipment power, open the furnace door, clean the smelting furnace, and place the raw materials 910kg 0A grade small particle sponge titanium, 50kg AlV55 alloy and 40kg aluminum particles in a copper crucible.
[0039] (2) After placing all the raw materials according to step (1), close the furnace door, start the mechanical pump, turn on the digital vacuum gauge, open the pre-vacuum valve, and wait until the vacuum drops to 5×10 -3 When the speed of the molecular pump reaches zero, turn off the power supply of the molecular pump.
[0040] (3) Open the charging valve and keep the mechanical pump in the open state to prevent air from entering the charging pipe. Wait until the vacuum degree in the furnace reaches 5×10-4 Pa, close the charging valve, turn off the mechanical pump, turn on the gas analysis system, open the hydrogen bottle and the charging valve. When the total gas pressure in the furnace is -0.05MPa, fill in 0.01Mpa hydrogen and then open the argon bottle to flush in 0.04MPa argon. The hydrogen accounts for 20% of the total volume.
[0041] (4) The ingot is forged for 6 times and then machined to obtain the extrusion billet material of 120×40mm. The billet is copper-clad and iron-clad, heated to 880℃ and kept for 1.5h before extrusion. The extrusion speed is controlled at 70-80mm / s. The extrusion size is 90×20mm. After extrusion, it is air-cooled to room temperature. After extrusion, the temperature is raised to 900℃ at 10℃ / min and annealed in a horizontal vacuum annealing furnace for 2h, then furnace-cooled to 500℃ and air-cooled to room temperature.
[0042] (5) Hot rolling: Hot rolling is carried out on a hot rolling mill. The hot rolling temperature is 900°C, the deformation per pass is controlled at 30-50%, the final rolling temperature is required to be ≥800°C, the feed per pass is 5mm / pass, and the rolling speed is 90 times / minute.
[0043] (6) Cold rolling: The deformation of each cold rolling pass is controlled at 20-30%, the rolling speed is 50 times / min, and the intermediate annealing temperature parameter is 850℃ / 2h.
[0044] (7) Repeat steps (5) to (6) until a TC4 titanium alloy tube with a size of 72 × 8 mm is rolled; wherein, after step (6), the temperature is increased at a rate of 10 °C / min, annealing is performed at 580 °C for 1 h, and the furnace is cooled to room temperature to obtain a TC4 titanium alloy seamless tube.
[0045] After testing, the microstructure of the TC4 titanium alloy seamless tube prepared in this embodiment is as follows Figure 2 As shown, the structure is uniform and there are no coarse deformed grains. Its room temperature mechanical properties meet the following requirements: tensile strength Rm = 952MPa, Rp0.2 = 878MPa, elongation after fracture A = 13.5%, indicating that the TC4 titanium alloy seamless tube prepared by the preparation method of this embodiment has excellent comprehensive mechanical properties.
[0046] Example 2 A method for preparing a TC4 titanium alloy seamless tube, the specific implementation steps are as follows: (1) Smelting is carried out in a high vacuum non-consumable arc furnace. First, start the circulating water, start the equipment power, open the furnace door, clean the smelting furnace, and then place the raw materials 900kg 0A grade small particle sponge titanium, 70kg AlV55 alloy and 30kg aluminum particles in a copper crucible.
[0047] (2) After placing all the raw materials according to step (1), close the furnace door, start the mechanical pump, turn on the digital vacuum gauge, open the pre-vacuum valve, and wait until the vacuum drops to 5×10 -3 When the speed of the molecular pump reaches zero, turn off the power of the molecular pump.
[0048] (3) Open the charging valve and keep the mechanical pump in the open state to prevent air from entering the charging pipe. Wait until the vacuum degree in the furnace reaches 5×10 -4 Pa, close the charging valve, turn off the mechanical pump, turn on the gas analysis system, open the hydrogen bottle and the charging valve, when the total gas pressure in the furnace is -0.05MPa, fill in 0.01Mpa hydrogen and then open the argon bottle to flush in 0.04MPa argon, and the hydrogen accounts for 20% of the total volume. During the whole process, the ratio of hydrogen and argon is controlled by the gas analysis system.
[0049] (4) After smelting, the TC4 titanium alloy ingot is forged for 6 times and then machined to obtain the 150×40mm extrusion billet raw material. After the billet surface is double-clad with copper and iron, it is heated to 900℃ and kept warm for 1.5h before extrusion. The extrusion speed is controlled at 60-80mm / s. The tube billet with a size of 96×12mm is extruded and air-cooled to room temperature. After extrusion, the temperature is raised to 900℃ at 10℃ / min and annealed in a horizontal vacuum annealing furnace for 3h, then furnace cooled to 500℃ and air-cooled to room temperature.
[0050] (5) Hot rolling: The hot rolling is carried out by a hot rolling mill, the hot rolling temperature is 950°C, the deformation amount per pass is controlled to be 30-50%, the final rolling temperature is required to be ≥800°C, the feed amount per pass is 4 mm / pass, and the rolling speed is 80 times / minute.
[0051] (6) Cold rolling: The deformation of each cold rolling pass is controlled at 20-30%, the rolling speed is 40 times / min, the intermediate annealing temperature is 850℃, and the annealing time is 2.5h.
[0052] (7) Repeat steps (5) to (6) until a Ф71×9 mm TC4 titanium alloy tube is obtained; wherein, after step (6), a heating rate of 10°C / min, stress relief annealing at 550°C for 1.5 h, and furnace cooling to room temperature are performed to obtain a TC4 titanium alloy seamless tube.
[0053] After testing, the microstructure of the TC4 titanium alloy seamless tube prepared in this embodiment is as follows Figure 3 As shown, the structure is uniform and there are no coarse deformed grains. Its room temperature mechanical properties meet the following requirements: tensile strength Rm = 964MPa, Rp0.2 = 882MPa, elongation after fracture A = 14.6%, indicating that the TC4 titanium alloy seamless tube prepared by the preparation method of this embodiment has excellent comprehensive mechanical properties.
[0054] Comparative Example A method for preparing a TC4 titanium alloy seamless tube, the specific implementation steps are as follows: (1) Smelting is carried out in a high vacuum non-consumable arc furnace. First, start the circulating water, start the equipment power, open the furnace door, clean the smelting furnace, and then place the raw materials 900kg 0A grade small particle sponge titanium, 70kg AlV55 alloy and 30kg aluminum particles in a copper crucible.
[0055] (2) After placing all the raw materials according to step (1), close the furnace door, start the mechanical pump, turn on the digital vacuum gauge, open the pre-vacuum valve, and wait until the vacuum drops to 5×10 -3 When the speed of the molecular pump reaches zero, turn off the power of the molecular pump.
[0056] (3) Open the charging valve and keep the mechanical pump turned on until the vacuum in the furnace reaches 5×10 -4 Pa, close the charging valve, turn off the mechanical pump, turn on the gas analysis system, open the charging valve, and when the total gas pressure in the furnace is -0.05MPa, fill in argon.
[0057] (4) After smelting, the TC4 titanium alloy ingot is forged three times and then machined to obtain the 150×40mm extrusion billet raw material. After the billet surface is double-clad with copper and iron, it is heated to 900℃ and kept for 1.5h before extrusion. The extrusion speed is controlled at 100mm / s. The tube billet with a size of 96×12mm is extruded and air-cooled to room temperature. After extrusion, the temperature is raised to 900℃ at 10℃ / min and annealed in a horizontal vacuum annealing furnace for 3h, then furnace cooled to 500℃ and air-cooled to room temperature.
[0058] (5) Warm rolling: After heating to 400-500°C by an induction heating device, rolling is performed, with the deformation amount of each pass controlled at 10-20%, the feed amount of each pass at 5 mm / pass, and the rolling speed at 60 times / minute. Until a Ф71×9mm TC4 titanium alloy tube is obtained. After step (5), the heating rate is 10°C / min, and the stress relief annealing is maintained at 550°C for 2h, and the furnace is cooled to room temperature to obtain a TC4 titanium alloy seamless tube.
[0059] After testing, the microstructure of the TC4 titanium alloy seamless tube prepared in this embodiment is as follows Figure 4 As shown, the size of the structure is very uneven, and there are many deformed grains. Its room temperature mechanical properties meet the following requirements: tensile strength Rm = 867MPa, Rp0.2 = 830MPa, elongation after fracture A = 9.7%.
[0060] The above are exemplary embodiments disclosed in the present invention, but it should be noted that various changes and modifications may be made without departing from the scope of the embodiments disclosed in the claims. Although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.
[0061] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the above embodiments of the present invention, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.
Claims
1. A method for preparing a TC4 titanium alloy seamless tube, characterized in that: The following steps are involved: S101. Raw materials for preparing TC4 titanium alloy: 0A grade small particles of titanium sponge, AlV55 alloy and aluminum particles; S102. The raw materials 0A grade small particles of titanium sponge, AlV55 alloy and aluminum particles are placed in a high vacuum non-consumable arc furnace and evacuated; S103. A high vacuum non-consumable arc furnace is first filled with hydrogen and then with argon to start smelting to obtain a TC4 titanium alloy ingot; S104. The TC4 titanium alloy ingot is forged to obtain an extrusion billet raw material; the extrusion billet raw material billet surface is double-clad with copper and iron, extruded, and the billet is air-cooled to room temperature after extrusion; and then the billet is annealed; S105. The tube is hot rolled; S106. The tube is cold rolled; S107. Repeat S105 to S106 until a TC4 titanium alloy seamless tube that meets the size requirements is obtained, and then perform annealing to obtain a finished TC4 titanium alloy seamless tube.
2. The method for preparing the TC4 titanium alloy seamless pipe according to claim 1, characterized in that: The annealing treatment in S104 is: heating to 850-900°C at 10°C / min in a horizontal vacuum annealing furnace for 2-3h, then cooling the furnace to 500°C and then air cooling to room temperature; The annealing treatment in S107 is as follows: heating the TC4 titanium alloy seamless pipe to 550-580° C. at a rate of 7-10° C. / min in a horizontal vacuum annealing furnace, annealing for 1-1.5 hours, and then cooling the furnace to room temperature.
3. The method for preparing the TC4 titanium alloy seamless pipe according to claim 1, characterized in that: In the S101, 880-920 kg of 0A grade small particle titanium sponge, 50-70 kg of AlV55 alloy and 30-50 kg of aluminum particles are added.
4. The method for preparing the TC4 titanium alloy seamless pipe according to claim 1, characterized in that: The extrusion process in S104 includes: heating the extrusion blank raw material after double-layer sheathing to 860-920° C. and keeping it warm for 1-2 hours before extruding, with an extrusion ratio of 6-9 and an extrusion speed controlled at 60-80 mm / s.
5. The method for preparing the TC4 titanium alloy seamless pipe according to claim 1, characterized in that: The step S102 of "placing the raw materials of 0A grade small-particle titanium sponge, AlV55 alloy and aluminum particles into a high vacuum non-consumable arc furnace and evacuating the furnace" includes: Put the raw materials of 0A grade small-particle titanium sponge, AlV55 alloy and aluminum particles into the copper crucible of a high vacuum non-consumable arc furnace, close the furnace door, start the mechanical pump, turn on the digital vacuum gauge, open the pre-evacuation valve, and wait until the vacuum degree in the furnace drops to 5×10 -3 When the speed of the molecular pump reaches zero, turn off the power of the molecular pump.
6. The method for preparing the TC4 titanium alloy seamless pipe according to claim 1, characterized in that: The step S103 of "first filling hydrogen into a high vacuum non-consumable arc furnace, and then filling argon into the furnace, and starting smelting to obtain a TC4 titanium alloy ingot" includes: Open the charging valve and keep the mechanical pump on to prevent air from entering the charging pipe. Wait until the vacuum degree in the furnace is ≤5x10 -4 Pa, close the charging valve, turn off the mechanical pump, open the hydrogen bottle and the charging valve, when the total gas pressure in the furnace is -0.05MPa, fill in 0.01Mpa hydrogen, then open the argon bottle and fill in 0.04MPa argon.
7. The method for preparing the TC4 titanium alloy seamless pipe according to claim 6, characterized in that: The volume ratio of hydrogen to the total volume of gas in the furnace is 20%.
8. The method for preparing a TC4 titanium alloy seamless pipe according to claim 1, characterized in that: In S104, the TC4 titanium alloy ingot is forged six times to obtain an extrusion billet raw material.
9. The method for preparing a TC4 titanium alloy seamless pipe according to claim 1, characterized in that: The hot rolling parameters of S105 include: hot rolling temperature of 900-950°C, deformation of each pass controlled at 30-50%, final rolling temperature requirement ≥800°C, feed amount of each pass 3-5mm / pass, and rolling speed of 80-100 times / minute.
10. The method for preparing a TC4 titanium alloy seamless pipe according to claim 1, characterized in that: The cold rolling parameters of S106 include: the deformation of each cold rolling pass is controlled at 20-30%, the rolling speed is 40-60 times / minute, the intermediate annealing temperature is 800-850° C., and the annealing time is 1.5-2.5 hours.
Citation Information
Patent Citations
Titanium alloy seamless tube and manufacturing method thereof
CN104831120A
High-processability titanium alloy and preparation method thereof
CN112210680A
Method for preparing magnesium alloy plate through hot-cold alternate rolling
CN113913660A
Preparation method of near-alpha titanium alloy seamless tube
CN117086125A
High-strength TA18 seamless titanium alloy and production method of large-diameter thin tube of high-strength TA18 seamless titanium alloy
CN117867308A
Cited By
Short-process preparation method of TC4 titanium alloy sheet
CN121911838A