Preparation method and application of graphene-coated vanadium tetrasulfide nano material
Preparing graphene-coated vanadium tetrasulfide nanoparticle materials through a one-step solvothermal method solves the problems of insufficient cycle stability and rate performance of sodium-ion battery anode materials, and achieves an electrode material with high capacity and good cycle performance, which is suitable for sodium ion batteries. Battery negative terminal.
Patent Information
- Application Number
- CN202410836920.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing anode materials for sodium-ion batteries have deficiencies in cycle stability and rate performance. In particular, commercial graphite and embedded anode materials exhibit low capacity and poor cycle stability. There is an urgent need for an anode material with excellent electrochemical properties.
A one-step solvothermal method is used to prepare graphene-coated vanadium tetrasulfide nanoparticle materials. The composite structure of graphene and VS4 nanoparticles improves the conductivity and specific surface area of the electrode material and provides excellent electrochemical performance.
The graphene-coated vanadium tetrasulfide nanomaterial shows excellent rate performance and cycle stability. The discharge and charge capacities in the first cycle are 450 and 338 mAh/g respectively. The capacity remains stable after the 15th cycle, and under high current density There is still a discharge specific capacity of 192mAh/g, proving its potential application in sodium-ion batteries.
Smart Images

Figure CN118867162A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanomaterials and electrochemical technology, and adopts a simple one-step solvent thermal method to construct a preparation method and application of a graphene-coated vanadium tetrasulfide nanocomposite material, and the material exhibits good cycle and rate performance. Background Art
[0002] Although lithium-ion batteries meet the daunting challenge of sustainable energy development, their feasibility must be reconsidered for the growing electric vehicle market. Lithium is widely distributed in the earth's crust, but it is not an abundant element. The relative content of lithium in the earth's crust is only 20ppm. In fact, the cost of lithium materials (Li2CO3 price) has risen sharply in the first decade of this century. Compared with lithium, sodium resources are ubiquitous and sodium is one of the most abundant elements on the surface. There are also unlimited sodium resources in the ocean. In addition, sodium is the second lightest and smallest alkali metal element relative to lithium. Therefore, sodium-ion batteries have the potential to replace lithium-ion batteries.
[0003] For sodium-ion batteries, most research focuses on their positive electrode materials, which already have excellent electrochemical properties. However, for their negative electrode materials, commercial graphite exhibits very low capacity (35mAh / g), and embedded negative electrodes exhibit low specific capacity. Alloying reaction (Sn, P, SnO2, etc.) and conversion reaction (ZnS, CoS, etc.) type negative electrode materials exhibit high capacity, but their cycle stability and rate performance are poor. Therefore, there is an urgent need to find negative electrode materials with excellent cycle stability, long life and high rate performance. Transition metal sulfides (TMDs) have attracted widespread attention due to their unique physicochemical properties. As battery negative electrode materials, they have high theoretical specific capacity, the required elements are abundant in the earth's crust, and the price is low. A non-layered transition metal sulfide NiS2 with a cubic phase structure is used as a sodium battery negative electrode material, which has excellent electrochemical properties. The present invention introduces a S2 2- Application of monomeric chain transition metal sulfides as electrode materials in sodium ion storage.
[0004] VS4 is one of these compounds. It was discovered in 1960 and its crystal structure was established in 1964. VS4 is a linear chain polymer with V connecting two adjacent S2 2- Monomer, namely V 4+ (S2 2-)2, the chains are connected by weak van der Waals forces to form a loosely stacked structure, with an interchain distance of 0.583nm, much larger than the radius of sodium ions (0.196nm). The large channels within and between chains provide potential sites for the diffusion and storage of alkali metals. In addition to its low price and abundant vanadium and sulfur resources, vanadium tetrasulfide has great advantages in practical energy storage applications. However, due to the complexity of the vanadium-sulfide system and the difficulty in synthesizing the pure VS4 phase in real experiments, there are few reports on this material. Summary of the invention
[0005] The technical problem to be solved by the present invention is to propose a one-step solvothermal method to prepare a graphene-coated VS4 nanoparticle composite in view of the above-mentioned prior art. The process is simple, and the resulting embedded graphene sheets greatly improve the conductivity and specific surface area of the electrode material, and provide a substrate for the nucleation and growth of VS4. The graphene-coated vanadium tetrasulfide nanocomposite material has very good electrochemical properties.
[0006] The technical solution adopted by the present invention to solve the above technical problems is:
[0007] 1. A graphene-coated vanadium tetrasulfide nanoparticle material, prepared by a one-step solvothermal method using graphene as a carbon source. The size of the VS4 nanoparticles is 100-200 nm, and the material is prepared by the following method, comprising the following steps:
[0008] 1) Measure a certain amount of graphite flakes and a certain amount of concentrated sulfuric acid in a conical flask, mix them evenly, and stir at room temperature;
[0009] 2) placing the conical flask in step 1) in a water bath, first adding a certain amount of oxidant until it is completely dissolved, and then slowly adding a certain amount of oxidant with stirring;
[0010] 3) Slowly adding deionized water to the solution obtained in step 2), then adding deionized water and stirring for 15 minutes, then taking it out of the water bath and diluting it with deionized water, and finally adding a certain amount of 30% H2O2 to remove the unreacted oxidant;
[0011] 4) The suspension obtained in step 3) is centrifuged and washed several times to remove unreacted acid and salt, and the pure GO is dispersed in an appropriate amount of deionized water and ultrasonicated for 1 hour. The obtained GO dispersion is centrifuged to remove unexfoliated graphite, and finally a brown GO solution is obtained;
[0012] 5) dissolving a certain amount of vanadium source obtained in step 4) and a certain amount of sodium hydroxide (NaOH) in 30 mL of GO (1.5 mg / mL), which is referred to as solution A;
[0013] 6) dissolving a certain amount of sulfur source obtained in step 5) in 10 mL of GO, recorded as solution B, and mixing solutions A and B and stirring for 1 h;
[0014] 7) transferring the solution obtained in step 6) to a high temperature reactor for hydrothermal reaction and placing it in an oven at 160° C. for 24 h;
[0015] 8) The product obtained in step 7) was washed several times in deionized water and alcohol, centrifuged and dried in a vacuum drying oven for 10 hours to finally obtain a graphene-modified VS4 composite nano-anode material.
[0016] 2. According to the above scheme, the weight of the graphite sheet in step 1) is 0.5g to 1.5g, and the concentrated sulfuric acid is 18 to 28mL;
[0017] 3. According to the above scheme, the temperature of the water bath process in step 2) is 35-45°C, the oxidant is one or more of KMnO4, K2MnO4, and NaClO, the first addition of the oxidant is 0.1-0.4g, and the second addition of the oxidant is 1-2.5g;
[0018] 4. According to the above scheme, 3-8 mL of deionized water was first added to the solution obtained in step 3), 35-55 mL of deionized water was added for the second time, 120-150 mL of deionized water was removed from the water bath, and finally 5-15 mL of 30% H2O2 was added to remove unreacted KMnO4;
[0019] 5. According to the above scheme, the vanadium source in step 5) is 1-5 mmol of sodium vanadate (NaVO3) and 3-9 mmol of sodium hydroxide (NaOH)
[0020] 6. According to the above scheme, the sulfur source in step 6) is 10-20 mmol thioacetamide (TAA);
[0021] 7. According to the above scheme, the temperature during the hydrothermal reaction in step 7) is 140-180°C;
[0022] 8. According to the above scheme, the temperature of the vacuum drying oven in step 8) is 50-70°C;
[0023] The excellent electrochemical performance of the graphene-coated vanadium tetrasulfide nanomaterial of the present invention is mainly attributed to the nanostructure and the continuous graphene sheet skeleton. The nanostructure can effectively shorten the transmission path of ions, increase the contact area between the electrolyte and the electrode material, and improve the ionic conductivity of the material. The graphene further improves the electronic conductivity of the material. The synergistic effect of the two makes the material have good electrochemical performance. The obtained graphene-modified vanadium tetrasulfide nanomaterial has excellent rate performance and cycle stability, and is one of the optional negative electrode materials for sodium ion batteries.
[0024] The beneficial effects of the present invention are as follows: using graphene as a carbon source, a graphene-coated vanadium tetrasulfide nanoparticle material is prepared by a one-step solvothermal method, the size of the VS4 nanoparticles is 100-200nm, these vanadium tetrasulfide small particles are uniformly loaded on the graphene layer, and are interconnected by a continuous graphene network, and the VS4 / graphene electrode in the present invention shows good electrochemical performance in cycle and rate tests. At a current density of 100mA / g, the first cycle discharge and charge capacities are 450 and 338mAh / g, respectively, and the electrode specific capacity decays to 288mAh / g when the 15th cycle is cycled, and the capacity remains at a relatively stable value in subsequent cycles. This composite material electrode also has good cycle performance at a relatively large current density of 500mA / g. At a large current rate of 800mA / g, there is still a discharge specific capacity of 192mAh / g. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the structure of the VS4 material of the present invention. (a) is the repeating unit of the one-dimensional chain VS4 observed from the top, and (b) is the monoclinic VS4 observed from the side. The green balls are V atoms, and the yellow-green balls are S atoms; Figure 2 (a) is a schematic diagram of the synthesis of the graphene-coated vanadium tetrasulfide nanomaterial of the present invention, (b) is the XRD spectrum of the graphene-coated vanadium tetrasulfide nanomaterial of the present invention; (c) is the Raman spectrum of the graphene-coated vanadium tetrasulfide nanomaterial of the present invention and the corresponding peaks of the C element in GO and VS4 / graphene (inset). Among them, Theta represents the diffraction angle in the XRD test, Raman shift represents the Raman shift in the Raman test, and Intensity represents the intensity. Hydrothermal in the figure represents solvent heat;
[0026] Figure 3 The (a) SEM and (b) TEM images, (c) and (d) HRTEM images of the graphene-coated vanadium tetrasulfide nanomaterial of the present invention, the interplanar spacing of 0.56 and 0.59 nm respectively corresponds to the (110
[0027] ) and (002) crystal planes. Inset: FFT graph of VS4. Graphene stands for graphene;
[0028] Figure 4The electrochemical performance diagram of the sodium ion battery assembled in Example 1 of the present invention. (a) Charge and discharge curve of graphene-coated vanadium tetrasulfide nanomaterial electrode at 100mA / g, (b) Cyclic voltammetry curve of graphene-coated vanadium tetrasulfide nanomaterial at 0.1mV / s, (c) Cyclic performance at a current density of 100mA / g, (d) Rate performance of graphene-coated vanadium tetrasulfide nanomaterial electrode. Among them, Specific Capacity represents capacity, Potential represents voltage, Current represents current, Cycle Number represents the number of cycles, and Coulombic Efficiency represents coulombic efficiency;
[0029] Figure 5 It is the cycle performance of VS4 / graphene assembled into a sodium ion battery at a current density of 500 mA / g in Example 1 of the present invention. Wherein, Specific Capacity represents capacity, Cycle Number represents the number of cycles, and Coulombic Efficiency represents coulombic efficiency;
[0030] Figure 6 It is the cycle performance of the sodium ion battery composed of comparative example 1 of the present invention at a current density of 100 mA / g. Wherein, Specific Capacity represents capacity, Cycle Number represents the number of cycles, and Coulombic Efficiency represents coulombic efficiency;
[0031] Figure 7 It is the non-in-situ XRD test spectrum of the VS4 / graphene electrode of Example 1 of the present invention at different potentials. Point a is the initial VS4 / graphene electrode sheet, bf are the first discharge to 1.75, 1.55, 1.45, 0.55 and 0.01V respectively, and point g is the first charge to 2.2V. Among them, Theta represents the diffraction angle in the non-in-situ XRD test, Intensity represents the diffraction intensity, Potential represents the voltage, and Specific Capacity represents the capacity;
[0032] Figure 8 TEM and HRTEM images of the VS4 / graphene electrode of Example 1 of the present invention at a current density of 100 mA / g (a, b) in a fully discharged state (inset: the enlarged HRTEM corresponding to the V presence region,) (c, d) in a fully charged state (inset: EDS spectrum, showing the presence of element S). Wherein, Acetylene black represents acetylene black;
[0033] Fig. 91 is an EIS graph of the VS4 / graphene assembled into a sodium ion battery before and after cycling in Example 1 of the present invention. Wherein, Before cycling represents before cycling, and After cycling represents after cycling. DETAILED DESCRIPTION
[0034] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0035] Embodiment 1:
[0036] The preparation of graphene-coated vanadium tetrasulfide nanomaterials includes the following two parts:
[0037] Part 1: Preparation of graphene (GO)
[0038] 1) Mix 1g of graphite flakes and 23mL of concentrated sulfuric acid in a 250mL conical flask and stir at room temperature for 24h;
[0039] 2) Place the conical flask in step 1) in a 40°C water bath, first add 0.1g NaNO3 until it is completely dissolved, then slowly add 1.5g KMnO4 and stir at 45°C for 30min;
[0040] 3) Slowly add 5 mL of deionized water to the solution obtained in step 2), then add 40 mL of deionized water and stir for 15 min, then take it out of the water bath and dilute it with 140 mL of deionized water, and finally add 10 mL of 30% H2O2 to remove unreacted KMnO4;
[0041] 4) The suspension obtained in step 3) was centrifuged and washed several times to remove unreacted acid and salt, and the pure GO was dispersed in an appropriate amount of deionized water and ultrasonicated for 1 hour. The obtained GO dispersion was centrifuged to remove unexfoliated graphite, and finally a brown GO solution was obtained.
[0042] Part II: Preparation of graphene-coated vanadium tetrasulfide nanomaterials
[0043] Preparation of graphene-coated vanadium tetrasulfide nanomaterials
[0044] 1) 3mmol sodium vanadate (NaVO3) and 6mmol sodium hydroxide (NaOH) were dissolved in 30mL GO (1.5mg / mL), which was recorded as solution A;
[0045] 2) Dissolve 15 mmol of thioacetamide (TAA) in 10 mL of GO, referred to as solution B, and mix solutions A and B and stir for 1 h;
[0046] 3) Transfer the suspension obtained in step 2) to a 50 mL reaction kettle and place it in an oven at 160° C. for 24 h;
[0047] 4) After cooling step 3) to room temperature, the obtained product was washed several times in deionized water and alcohol, centrifuged and dried in a vacuum drying oven at 60° C. for 10 h, and finally a graphene-modified VS4 composite nano-anode material was obtained.
[0048] The VS4 material of the present invention is a linear chain polymer, V connects two adjacent S22-monomers, that is, V 4+ ( S2 2-) 2. The chains are connected by weak van der Waals forces to form a loosely stacked structure with a distance of 0.583 nm, which is much larger than the radius of sodium ions (0.196nm). Figure 1 As shown in Figure 2, the large intra-chain and inter-chain channels provide potential sites for the diffusion and storage of alkali metals. This example reveals the formation process of VS4 / graphene composites. Figure 2 As shown in a, C2H5NS (TAA), one of the raw materials, not only acts as a reducing agent but also a sulfur source in the entire reaction process. In the solvothermal process, under alkaline conditions, C2H5NS hydrolyzes to produce S 2- V and O in solution are V x O yn- In the reaction process, V x O yn- Slowly transforming into VS4, GO was partially reduced to reduced graphene (rGO).
[0049] The crystal structure and crystallinity of VS4 / graphene nanocomposites were characterized. Figure 2 b) The product is a pure face-centered cubic monoclinic phase VS4 (space group: I2 / c). (JCPDS No.87-0603). At the same time, the XRD peaks obtained from the test are very sharp, indicating that the final product has a high degree of crystallinity. Raman spectrum of VS4 / graphene ( Figure 2 c) shows two main peaks at 190 and 279 cm -1 The two peaks correspond to the stretching and bending vibrations of VS. In order to explore the properties of graphene in the sample, Raman spectroscopy tests were performed on VS4 / graphene nanocomposites and pure graphene ( Figure 2 c inner inset). Characteristic peaks are located at 1330 and 1590 cm -1 , corresponding to the D peak and G peak of graphene respectively. The D peak represents the defects and dislocations of carbon atoms, and the G peak is caused by the sp 2The ID / IG ratio shows the degree of defects in graphitized carbon materials. Compared with the initial graphene, the ID / IG value of VS4 / graphene composites is relatively high, and the ratio increases from 1.11 to 1.16, proving that GO is partially reduced to rGO during the solvothermal process, forming more defects and vacancies, which are mainly due to the deoxidation process of GO.
[0050] The morphology of graphene-coated vanadium tetrasulfide nanoparticles in this example. SEM ( Figure 3 a) and TEM( Figure 3 b) shows that VS4 nanoparticles grow on the wrinkled graphene surface. The graphene sheets not only improve the electronic conductivity of the material, but also provide a substrate for the nucleation and growth of VS4. The size of VS4 nanoparticles is 100-200nm. From TEM ( Figure 3 b, c) Thin wrinkled graphene can be clearly observed. The presence of graphene effectively limits the agglomeration of VS4 nanoparticles. HRTEM ( Figure 3 d) shows that the interplanar spacing of the material is 0.56 and 0.59 nm, which corresponds to the (110) and (002) planes of VS4, respectively. Fast Fourier transform image ( Figure 3 d illustration) also corresponds to the monoclinic phase VS4. Elemental analysis (CHNS) is used to detect the carbon content of graphene-coated vanadium tetrasulfide nanomaterials, and the test results show that the carbon content of the material is about 9.8%.
[0051] The electrochemical performance of button cells (CR2016) was tested by using self-made sodium metal sheets as counter electrodes and graphene-coated vanadium tetrasulfide nanomaterials as electrode materials. The electrode voltage test range was 0.01-2.2Vvs.Na+ / Na. Figure 4 a shows the charge and discharge curves of the first three cycles of graphene-coated vanadium tetrasulfide nanomaterials. It can be seen from the figure that the first cycle discharge and charge capacities are 450.4 and 338.4 mAh / g, respectively. The first cycle coulomb efficiency is 75%, and the lower coulomb efficiency is due to irreversible electrolyte decomposition and the formation of solid electrolyte interface (SEI). We tested the cyclic voltammetry (CV) curve of graphene-coated vanadium tetrasulfide nanomaterials with a scan rate of 0.1 mV / s ( Figure 4b). The curve of the first cycle is different from the subsequent curves. During the first discharge process, a strong reduction peak appeared at 1.6V but disappeared in the subsequent cycles. This pattern is similar to other transition metal sulfides, such as MoS2, FeS2, SnS2, SnS, etc. In the second and subsequent cycles, the VS4 / graphene electrode has three reduction peaks, located at 0.65, 1.10, and 1.30V, respectively. There are also two oxidation peaks at 1.50 and 1.95V. The two reduction peaks at 0.65 and 1.10V represent the conversion reaction between the electrode and Na. In addition, there is only one strong oxidation peak at 1.50V corresponding to a reversible oxidation reaction. The redox couple 1.30 / 1.95V corresponds to the conversion reaction of sulfur atoms in the complex. The characteristic peak position of CV corresponds well to the position of the electrode charge and discharge platform. At a current density of 100mA / g, the cycling performance of the VS4 graphene electrode is as follows. Figure 4 c. In the second cycle, the coulombic efficiency of the battery reached 91.8%, and after several cycles, the coulombic efficiency was close to 100%. The discharge capacity of the electrode decayed to 288 mAh / g at the 15th cycle, and the capacity remained relatively stable in the subsequent cycles. After 50 cycles, the discharge and charge capacities of the VS4 / graphene composite electrode were 241 and 237 mAh / g, respectively. Subsequently, we studied the rate performance of the material ( Figure 4 d). The battery was first cycled 4 times at increasing current densities of 100, 300, 500 and 800 mA / g, and the discharge capacity at each current density was 342, 267, 220 and 192 mAh / g, respectively. Then the current density was reduced to 100 mA / g, and the capacity recovered to 93.9% of the initial capacity. The rate test further shows that the material can maintain a relatively stable capacity at each rate under the rapid change of current density, and has excellent rate performance and cycle stability.
[0052] The sodium ion storage performance of the VS4 / graphene composite electrode was investigated by ex situ XRD testing of the electrode sheet and its XRD under different charge and discharge conditions. Figure 7 As shown, the initial electrode sheet is pure phase, with two strong diffraction peaks located at 15.8° and 17.0° ( Figure 7 -a point). When discharged to 1.75V, the electrode sheet does not have obvious structural changes ( Figure 7 - point b). When the discharge continues to 1.55V ( Figure 7 -c), the main peak intensity of VS4 weakens. During this process, sodium is embedded into the active material. The electrochemical reaction equation is: VS4+xNa + +xe - →NaxVS4
[154] When the material is discharged to 1.45V, the two main peaks disappear ( Figure 7 -d point). Continue to discharge deeply to 0.55V ( Figure 7 -e point), the main diffraction peak of VS4 completely disappears. At the same time, a diffraction peak appears at 48.0°, which corresponds to the (200) diffraction peak of metal V (JCPDS No.01-088-2322). This process corresponds to the conversion reaction of VS4 during the discharge process, generating metal V and Na2S phase. The corresponding electrochemical reaction is: Na x VS4+(8-x)Na + +(8-x)e - →4Na2S+V. When fully discharged to 0.01V, the intensity of the newly appeared diffraction peak increases ( Figure 7 -f point). When fully charged back to 2.2V ( Figure 7 -g point), the diffraction peak of VS4 no longer appears, which indicates that an irreversible conversion reaction occurred in the first cycle, but the peak of metal V still exists. The broadened peak at 16-21° is generated by the test sample substrate. In order to further explore the mechanism of sodium ion storage, we tested the TEM and EDS spectra of the VS4 / graphene composite electrode in fully discharged and fully charged states. Figure 8 a shows the TEM image of VS4 when it is fully discharged to 0.01V, and the corresponding HRTEM ( Figure 8 b) shows that the lattice fringe spacing is 0.190nm and 0.309nm, which correspond to the (200) crystal plane of metal V and the crystal plane of Na2S, respectively. When the electrode is fully charged to 2.2V, HRTEM ( Figure 8 d) shows that the interplanar spacing is 0.190 and 0.219 nm, corresponding to the (200) and (111) planes of metal V, respectively, further confirming that metal V still exists in the electrode after the first cycle of charge and discharge and remains inert during subsequent cycles. TEM image and EDS spectrum ( Figure 8 c and the corresponding inset) show a S aggregation area, which is consistent with the electrochemical reaction mechanism obtained from the ex situ XRD test, that is, after the first cycle, the subsequent electrochemical reaction may be a reversible reaction between S and Na2S.
[0053] Metal V is produced in the continuous electrochemical reaction, which greatly reduces the charge transfer resistance of the electrode material. To confirm this, we tested the electrochemical impedance spectroscopy (EIS) of the VS4 / graphene electrode before and after cycling. Fig. 9 ). Before cycling, the spectrum shows two semicircles with larger diameters that are not completely separated in the high-frequency range, indicating high interfacial resistance. After cycling, the semicircle in the high-frequency range becomes one and the diameter becomes smaller, and the charge transfer resistance of the electrode material decreases. The vanadium produced after the first discharge greatly improves the conductivity of the material. This phenomenon has also appeared in reports on MoS2 negative electrode materials.
[0054] In summary, the electrochemical reaction mechanism during the charge and discharge process of VS4 was explored with the help of ex-situ XRD testing, ex-situ TEM testing and EDS spectroscopy. The first cycle of sodiumization of V VS4 / graphene composite electrode undergoes three independent electrochemical reaction processes. The initial discharge undergoes a sodium insertion reaction, followed by a conversion reaction, and NaxVS4 decomposes into new phases V and Na2S. The subsequent cycle process may be a reversible electrochemical reaction between Na2S and S. The metal V produced during the entire reaction process does not participate in the subsequent electrochemical reaction but greatly improves the conductivity of the electrode material.
[0055] Embodiment 2:
[0056] The preparation of graphene-coated vanadium tetrasulfide nanomaterials includes the following two parts:
[0057] Part I: Preparation of graphene (GO)
[0058] 1) Mix 0.5 g of graphite flakes and 23 mL of concentrated sulfuric acid in a 250 mL conical flask and stir at room temperature for 24 h;
[0059] 2) Place the conical flask in step 1) in a 37°C water bath, first add 0.2g NaNO3 until it is completely dissolved, then slowly add 1.7g KMnO4 and stir at 45°C for 30min;
[0060] 3) Slowly add 7 mL of deionized water to the solution obtained in step 2), then add 42 mL of deionized water and stir for 15 min, then take it out of the water bath and dilute it with 147 mL of deionized water, and finally add 9 mL of 30% H2O2 to remove unreacted KMnO4;
[0061] 4) The suspension obtained in step 3) was centrifuged and washed several times to remove unreacted acid and salt, and the pure GO was dispersed in an appropriate amount of deionized water and ultrasonicated for 1 hour. The obtained GO dispersion was centrifuged to remove unexfoliated graphite, and finally a brown GO solution was obtained.
[0062] Part II: Preparation of graphene-coated vanadium tetrasulfide nanomaterials
[0063] 1) 1mmol sodium vanadate (NaVO3) and 5mmol sodium hydroxide (NaOH) were dissolved in 30mL GO (1.5mg / mL), which was recorded as solution A;
[0064] 2) Dissolve 13 mmol of thioacetamide (TAA) in 10 mL of GO, referred to as solution B, and mix solutions A and B and stir for 1 h;
[0065] 3) Transfer the suspension obtained in step 2) to a 50 mL reaction kettle and place it in an oven at 145°C for 24 hours;
[0066] 4) After cooling step 3) to room temperature, the obtained product was washed several times in deionized water and alcohol, centrifuged and dried in a vacuum drying oven at 67° C. for 10 h, and finally a graphene-modified VS4 composite nano-anode material was obtained.
[0067] Taking the VS4 / rGO material obtained in this example as an example, the metal sodium sheet was used as the counter electrode, and the graphene-coated vanadium tetrasulfide nanomaterial was used as the electrode material to assemble a button cell (CR2016) to test its electrochemical performance. The electrode voltage test range was 0.01-2.2V vs. Na + / Na. At a current density of 100mA / g, after 50 cycles, the discharge and charge capacities of the VS4 / graphene composite electrode were 249 and 235mAh / g, respectively. The battery was first cycled 4 times at increasing current densities of 100, 300, 500 and 800mA / g, and the discharge specific capacity at each current density was 342, 267, 220 and 192mAh / g, respectively. Then the current density was reduced to 100mA / g, and the capacity could be restored to 93.9% of the initial capacity. The rate test further illustrates that the material can maintain a relatively stable capacity at each rate under the rapid change of current density, and has excellent rate performance and cycle stability. In addition, at a high current density of 500mA / g, the initial discharge capacity of the electrode was 286mAh / g, and the capacity retention rate was 81.5% after 100 cycles.
[0068] Embodiment 3:
[0069] The preparation of graphene-coated vanadium tetrasulfide nanomaterials includes the following two parts:
[0070] Part I: Preparation of graphene (GO)
[0071] 1) Mix 1.1 g of graphite flakes and 19 mL of concentrated sulfuric acid in a 250 mL conical flask and stir at room temperature for 24 h;
[0072] 2) Place the conical flask in step 1) in a 42°C water bath, first add 0.3g NaNO3 until it is completely dissolved, then slowly add 2.1g KMnO4 and stir at 45°C for 30min;
[0073] 3) 8 mL of deionized water was slowly added dropwise to the solution obtained in step 2), and then 38 mL of deionized water was added and stirred for 15 min, after which it was taken out of the water bath and diluted with 138 mL of deionized water, and finally 11 mL of 30% H2O2 was added to remove unreacted KMnO4;
[0074] 4) The suspension obtained in step 3) was centrifuged and washed several times to remove unreacted acid and salt, and the pure GO was dispersed in an appropriate amount of deionized water and ultrasonicated for 1 hour. The obtained GO dispersion was centrifuged to remove unexfoliated graphite, and finally a brown GO solution was obtained.
[0075] Part II: Preparation of graphene-coated vanadium tetrasulfide nanomaterials
[0076] Preparation of graphene-coated vanadium tetrasulfide nanomaterials
[0077] 1) 4mmol sodium vanadate (NaVO3) and 4mmol sodium hydroxide (NaOH) were dissolved in 30mL GO (1.5mg / mL), which was recorded as solution A;
[0078] 2) Dissolve 17 mmol of thioacetamide (TAA) in 10 mL of GO, referred to as solution B, mix solutions A and B and stir for 1 h;
[0079] 3) Transfer the suspension obtained in step 2) to a 50 mL reaction kettle and place it in an oven at 167° C. for 24 h;
[0080] 4) After cooling step 3) to room temperature, the obtained product was washed several times in deionized water and alcohol, centrifuged and dried in a vacuum drying oven at 69° C. for 10 h, and finally a graphene-modified VS4 composite nano-anode material was obtained.
[0081] Taking the VS4 / rGO material obtained in this example as an example, the metal sodium sheet was used as the counter electrode, and the graphene-coated vanadium tetrasulfide nanomaterial was used as the electrode material to assemble a button cell (CR2016) to test its electrochemical performance. The electrode voltage test range was 0.01-2.2V vs. Na + / Na. At a current density of 100mA / g, after 50 cycles, the discharge and charge capacities of the VS4 / graphene composite electrode were 247 and 232mAh / g, respectively. The battery was first cycled 4 times at increasing current densities of 100, 300, 500 and 800mA / g, and the discharge specific capacity at each current density was 347, 261, 228 and 196mAh / g, respectively. Then the current density was reduced to 100mA / g, and the capacity could be restored to 96.1% of the initial capacity. The rate test further illustrates that the material can maintain a relatively stable capacity at each rate under the rapid change of current density, and has excellent rate performance and cycle stability. In addition, at a high current density of 500mA / g, the initial discharge capacity of the electrode was 282mAh / g, and the capacity retention rate was 88.5% after 100 cycles.
[0082] Embodiment 4:
[0083] The preparation of graphene-coated vanadium tetrasulfide nanomaterials includes the following two parts:
[0084] Part 1: Preparation of graphene (GO)
[0085] 1) 0.8 g of graphite flakes and 22 mL of concentrated sulfuric acid were mixed evenly in a 250 mL conical flask and stirred at room temperature for 24 h;
[0086] 2) Place the conical flask in step 1) in a 38°C water bath, first add 0.4g NaNO3 until it is completely dissolved, then slowly add 1.7g KMnO4 and stir at 45°C for 30min;
[0087] 3) Slowly add 5 mL of deionized water to the solution obtained in step 2), then add 46 mL of deionized water and stir for 15 min, then take it out of the water bath and dilute it with 125 mL of deionized water, and finally add 11 mL of 30% H2O2 to remove unreacted KMnO4;
[0088] 4) The suspension obtained in step 3) was centrifuged and washed several times to remove unreacted acid and salt, and the pure GO was dispersed in an appropriate amount of deionized water and ultrasonicated for 1 hour. The obtained GO dispersion was centrifuged to remove unexfoliated graphite, and finally a brown GO solution was obtained.
[0089] Part II: Preparation of graphene-coated vanadium tetrasulfide nanomaterials
[0090] Preparation of graphene-coated vanadium tetrasulfide nanomaterials
[0091] 1) 3mmol sodium vanadate (NaVO3) and 7mmol sodium hydroxide (NaOH) were dissolved in 30mL GO (1.5mg / mL), which was recorded as solution A;
[0092] 2) Dissolve 17 mmol of thioacetamide (TAA) in 10 mL of GO, referred to as solution B, and mix solutions A and B and stir for 1 h;
[0093] 3) Transfer the suspension obtained in step 2) to a 50 mL reaction kettle and place it in an oven at 162° C. for 24 h;
[0094] 4) After cooling step 3) to room temperature, the obtained product was washed several times in deionized water and alcohol, centrifuged and dried in a vacuum drying oven at 64° C. for 10 h, and finally a graphene-modified VS4 composite nano-anode material was obtained.
[0095] Taking the VS4 / rGO material obtained in this example as an example, the metal sodium sheet was used as the counter electrode, and the graphene-coated vanadium tetrasulfide nanomaterial was used as the electrode material to assemble a button cell (CR2016) to test its electrochemical performance. The electrode voltage test range was 0.01-2.2V vs. Na+ / Na. At a current density of 100mA / g, after 50 cycles, the discharge and charge capacities of the VS4 / graphene composite electrode were 234 and 249mAh / g, respectively. The battery was first cycled 4 times at increasing current densities of 100, 300, 500 and 800mA / g, and the discharge specific capacity at each current density was 353, 291, 234 and 192mAh / g, respectively. Then the current density was reduced to 100mA / g, and the capacity could be restored to 86.1% of the initial capacity. The rate test further illustrates that the material can maintain a relatively stable capacity at each rate under the rapid change of current density, and has excellent rate performance and cycle stability. In addition, at a high current density of 500mA / g, the initial discharge capacity of the electrode was 236mAh / g, and the capacity retention rate was 89.5% after 100 cycles.
[0096] Embodiment 5:
[0097] The preparation of graphene-coated vanadium tetrasulfide nanomaterials includes the following two parts:
[0098] Part I: Preparation of graphene (GO)
[0099] 1) Mix 1.2 g of graphite flakes and 24 mL of concentrated sulfuric acid in a 250 mL conical flask and stir at room temperature for 24 h;
[0100] 2) Place the conical flask in step 1) in a 37°C water bath, first add 0.3g NaNO3 until it is completely dissolved, then slowly add 1.7g KMnO4 and stir at 45°C for 30min;
[0101] 3) Slowly add 4 mL of deionized water to the solution obtained in step 2), then add 40 mL of deionized water and stir for 15 min, then take it out of the water bath and dilute it with 122 mL of deionized water, and finally add 13 mL of 30% H2O2 to remove unreacted KMnO4;
[0102] 4) The suspension obtained in step 3) was centrifuged and washed several times to remove unreacted acid and salt, and the pure GO was dispersed in an appropriate amount of deionized water and ultrasonicated for 1 hour. The obtained GO dispersion was centrifuged to remove unexfoliated graphite, and finally a brown GO solution was obtained.
[0103] Part II: Preparation of graphene-coated vanadium tetrasulfide nanomaterials
[0104] Preparation of graphene-coated vanadium tetrasulfide nanomaterials
[0105] 1) 3mmol sodium vanadate (NaVO3) and 5mmol sodium hydroxide (NaOH) were dissolved in 30mL GO (1.5mg / mL), which was recorded as solution A;
[0106] 2) Dissolve 14 mmol of thioacetamide (TAA) in 10 mL of GO, referred to as solution B, and mix solutions A and B and stir for 1 h;
[0107] 3) Transfer the suspension obtained in step 2) to a 50 mL reaction kettle and place it in an oven at 151°C for 24 hours;
[0108] 4) After cooling step 3) to room temperature, the obtained product was washed several times in deionized water and alcohol, centrifuged and dried in a vacuum drying oven at 56° C. for 10 h, and finally a graphene-modified VS4 composite nano-anode material was obtained.
[0109] Taking the VS4 / rGO material obtained in this example as an example, the metal sodium sheet was used as the counter electrode, and the graphene-coated vanadium tetrasulfide nanomaterial was used as the electrode material to assemble a button cell (CR2016) to test its electrochemical performance. The electrode voltage test range was 0.01-2.2V vs. Na + / Na. At a current density of 100mA / g, after 50 cycles, the discharge and charge capacities of the VS4 / graphene composite electrode were 237 and 220mAh / g, respectively. The battery was first cycled 4 times at increasing current densities of 100, 300, 500 and 800mA / g, and the discharge specific capacity at each current density was 387, 265, 238 and 296mAh / g, respectively. Then the current density was reduced to 100mA / g, and the capacity could be restored to 93.1% of the initial capacity. The rate test further illustrates that the material can maintain a relatively stable capacity at each rate under the rapid change of current density, and has excellent rate performance and cycle stability. In addition, at a high current density of 500mA / g, the initial discharge capacity of the electrode was 284mAh / g, and the capacity retention rate was 87.5% after 100 cycles.
[0110] Embodiment 6:
[0111] The preparation of graphene-coated vanadium tetrasulfide nanomaterials includes the following two parts:
[0112] Part I: Preparation of graphene (GO)
[0113] 1) 0.7 g of graphite flakes and 23 mL of concentrated sulfuric acid were mixed evenly in a 250 mL conical flask and stirred at room temperature for 24 h;
[0114] 2) Place the conical flask in step 1) in a 37°C water bath, first add 0.2g NaNO3 until it is completely dissolved, then slowly add 1.4g KMnO4 and stir at 45°C for 30min;
[0115] 3) Slowly add 3 mL of deionized water to the solution obtained in step 2), then add 44 mL of deionized water and stir for 15 min, then take it out of the water bath and dilute it with 134 mL of deionized water, and finally add 7 mL of 30% H2O2 to remove unreacted KMnO4;
[0116] 4) The suspension obtained in step 3) was centrifuged and washed several times to remove unreacted acid and salt, and the pure GO was dispersed in an appropriate amount of deionized water and ultrasonicated for 1 hour. The obtained GO dispersion was centrifuged to remove unexfoliated graphite, and finally a brown GO solution was obtained.
[0117] Part II: Preparation of graphene-coated vanadium tetrasulfide nanomaterials
[0118] Preparation of graphene-coated vanadium tetrasulfide nanomaterials
[0119] 1) 3mmol sodium vanadate (NaVO3) and 7mmol sodium hydroxide (NaOH) were dissolved in 30mL GO (1.5mg / mL), which was recorded as solution A;
[0120] 2) Dissolve 15 mmol of thioacetamide (TAA) in 10 mL of GO, referred to as solution B, and mix solutions A and B and stir for 1 h;
[0121] 3) Transfer the suspension obtained in step 2) to a 50 mL reaction kettle and place it in an oven at 151°C for 24 hours;
[0122] 4) After cooling step 3) to room temperature, the obtained product was washed several times in deionized water and alcohol, centrifuged and dried in a vacuum drying oven at 59° C. for 10 h, and finally a graphene-modified VS4 composite nano-anode material was obtained.
[0123] Taking the VS4 / rGO material obtained in this example as an example, the metal sodium sheet was used as the counter electrode, and the graphene-coated vanadium tetrasulfide nanomaterial was used as the electrode material to assemble a button cell (CR2016) to test its electrochemical performance. The electrode voltage test range was 0.01-2.2V vs. Na + / Na. At a current density of 100mA / g, after 50 cycles, the discharge and charge capacities of the VS4 / graphene composite electrode were 251 and 292mAh / g, respectively. The battery was first cycled 4 times at increasing current densities of 100, 300, 500 and 800mA / g, and the discharge specific capacity at each current density was 361, 291, 268 and 236mAh / g, respectively. Then the current density was reduced to 100mA / g, and the capacity could be restored to 86.1% of the initial capacity. The rate test further illustrates that the material can maintain a relatively stable capacity at each rate under the rapid change of current density, and has excellent rate performance and cycle stability. In addition, at a high current density of 500mA / g, the initial discharge capacity of the electrode was 275mAh / g, and the capacity retention rate was 86.1% after 100 cycles.
[0124] Embodiment 7:
[0125] The preparation of graphene-coated vanadium tetrasulfide nanomaterials includes the following two parts:
[0126] Part I: Preparation of graphene (GO)
[0127] 1) Mix 1.5 g of graphite flakes and 28 mL of concentrated sulfuric acid in a 250 mL conical flask and stir at room temperature for 24 h;
[0128] 2) Place the conical flask in step 1) in a 37°C water bath, first add 0.2g NaNO3 until it is completely dissolved, then slowly add 1.8g KMnO4 and stir at 45°C for 30min;
[0129] 3) Slowly add 4 mL of deionized water to the solution obtained in step 2), then add 43 mL of deionized water and stir for 15 min, then take it out of the water bath and dilute it with 132 mL of deionized water, and finally add 8 mL of 30% H2O2 to remove unreacted KMnO4;
[0130] 4) The suspension obtained in step 3) was centrifuged and washed several times to remove unreacted acid and salt, and the pure GO was dispersed in an appropriate amount of deionized water and ultrasonicated for 1 hour. The obtained GO dispersion was centrifuged to remove unexfoliated graphite, and finally a brown GO solution was obtained.
[0131] Part II: Preparation of graphene-coated vanadium tetrasulfide nanomaterials
[0132] Preparation of graphene-coated vanadium tetrasulfide nanomaterials
[0133] 1) 3mmol sodium vanadate (NaVO3) and 9mmol sodium hydroxide (NaOH) were dissolved in 30mL GO (1.5mg / mL), which was recorded as solution A;
[0134] 2) Dissolve 19 mmol of thioacetamide (TAA) in 10 mL of GO, referred to as solution B, and mix solutions A and B and stir for 1 h;
[0135] 3) Transfer the suspension obtained in step 2) to a 50 mL reaction kettle and place it in an oven at 179°C for 24 hours;
[0136] 4) After cooling step 3) to room temperature, the obtained product was washed several times in deionized water and alcohol, centrifuged and dried in a vacuum drying oven at 69° C. for 10 h, and finally a graphene-modified VS4 composite nano-anode material was obtained.
[0137] Taking the VS4 / rGO material obtained in this example as an example, the metal sodium sheet was used as the counter electrode, and the graphene-coated vanadium tetrasulfide nanomaterial was used as the electrode material to assemble a button cell (CR2016) to test its electrochemical performance. The electrode voltage test range was 0.01-2.2V vs. Na + / Na. At a current density of 100mA / g, after 50 cycles, the discharge and charge capacities of the VS4 / graphene composite electrode were 292 and 242mAh / g, respectively. The battery was first cycled 4 times at increasing current densities of 100, 300, 500 and 800mA / g, and the discharge specific capacity at each current density was 317, 255, 328 and 416mAh / g, respectively. Then the current density was reduced to 100mA / g, and the capacity could be restored to 89.7% of the initial capacity. The rate test further illustrates that the material can maintain a relatively stable capacity at each rate under the rapid change of current density, and has excellent rate performance and cycle stability. In addition, at a high current density of 500mA / g, the initial discharge capacity of the electrode was 422mAh / g, and the capacity retention rate was 91.5% after 100 cycles.
[0138] Comparative Example 1
[0139] 1) Mix 1.1 g of graphite flakes and 23 mL of concentrated sulfuric acid in a 250 mL conical flask and stir at room temperature for 24 h;
[0140] 2) Place the conical flask in step 1) in a 47°C water bath, first add 0.4g NaNO3 until it is completely dissolved, then slowly add 1.8g KMnO4 and stir at 45°C for 30min;
[0141] 3) Slowly add 7 mL of deionized water to the solution obtained in step 2), then add 53 mL of deionized water and stir for 15 min, then take it out of the water bath and dilute it with 146 mL of deionized water, and finally add 14 mL of 30% H2O2 to remove unreacted KMnO4;
[0142] 4) The suspension obtained in step 3) was centrifuged and washed several times to remove unreacted acid and salt, and the pure GO was dispersed in an appropriate amount of deionized water and ultrasonicated for 1 hour. The obtained GO dispersion was centrifuged to remove unexfoliated graphite, and finally a brown GO solution was obtained.
[0143] The electrochemical performance of the button cell (CR2016) was tested by using the metal sodium sheet as the counter electrode and the graphene material as the electrode material. The electrode voltage test range was 0.01-2.2V vs.Na + / Na. Figure 6 The graph of graphene cycle performance shows that graphene provides almost no capacity during battery cycling. Figure 5 The comparison of the electrochemical performance of the graphene-coated vanadium tetrasulfide nanomaterials in Example 1 shows that in the entire electrode material, the main capacity contribution is VS4 in the composite material. The good rate performance of the entire electrode material during the cycle is mainly attributed to the graphene between the VS4 nanoparticles, which greatly improves the conductivity of the material while limiting the agglomeration of nanoparticles. The small particle size also accelerates the diffusion rate of sodium ions.
Claims
1. A graphene-coated vanadium tetrasulfide nanoparticle material, prepared by a one-step solvothermal method using graphene as a carbon source. The size of the VS4 nanoparticles is 100-200 nm, and the material is prepared by the following method, comprising the following steps: 1) Measure a certain amount of graphite flakes and a certain amount of concentrated sulfuric acid in a conical flask, mix them evenly, and stir at room temperature; 2) placing the conical flask in step 1) in a water bath, first adding a certain amount of oxidant until it is completely dissolved, and then slowly adding a certain amount of oxidant with stirring; 3) Slowly adding deionized water to the solution obtained in step 2), then adding deionized water and stirring for 15 minutes, then taking it out of the water bath and diluting it with deionized water, and finally adding a certain amount of 30% H2O2 to remove the unreacted oxidant; 4) The suspension obtained in step 3) is centrifuged and washed several times to remove unreacted acid and salt, and the pure GO is dispersed in an appropriate amount of deionized water and ultrasonicated for 1 hour. The obtained graphene oxide (GO) dispersion is centrifuged to remove unexfoliated graphite, and finally a brown GO solution is obtained; 5) dissolving a certain amount of vanadium source obtained in step 4) and a certain amount of sodium hydroxide (NaOH) in 30 mL of GO (1.5 mg / mL), which is referred to as solution A; 6) dissolving a certain amount of sulfur source obtained in step 5) in 10 mL of GO, recorded as solution B, and mixing solutions A and B and stirring for 1 h; 7) transferring the solution obtained in step 6) to a high temperature reactor for hydrothermal reaction and placing it in an oven at 160° C. for 24 h; 8) The product obtained in step 7) was washed several times in deionized water and alcohol, centrifuged and dried in a vacuum drying oven for 10 hours to finally obtain a graphene-modified VS4 composite nano-anode material.
2. The preparation of the graphene-coated vanadium tetrasulfide nanoparticle material according to claim 1 is characterized in that the weight of the graphite sheet in step 1) is 0.5g to 1.5g, and the concentrated sulfuric acid is 18 to 28mL.
3. The preparation of the graphene-coated vanadium tetrasulfide nanoparticle material according to claim 1 is characterized in that the temperature in the water bath process in step 2) is 35-45°C, and the oxidant is KMnO 4 , K2MnO4, NaClO or more thereof. The first addition of oxidant is 0.1-0.4g, and the second addition of oxidant is 1-2.5g.
4. The preparation of the graphene-coated vanadium tetrasulfide nanoparticle material according to claim 1 is characterized in that 3 to 8 mL of deionized water is first added to the solution obtained in step 3), 35 to 55 mL of deionized water is added for the second time, 120 to 150 mL of deionized water is removed from the water bath, and finally 5 to 15 mL of 30% H2O2 is added to remove unreacted KMnO 4。 5. The preparation of the graphene-coated vanadium tetrasulfide nanoparticle material according to claim 1 is characterized in that the vanadium source in step 5) is 1 to 5 mmol of sodium vanadate (NaVO3) and 3 to 9 mmol of sodium hydroxide (NaOH).
6. The preparation of the graphene-coated vanadium tetrasulfide nanoparticle material according to claim 1 is characterized in that the sulfur source in step 6) is 10 to 20 mmol of thioacetamide (TAA).
7. The preparation of the graphene-coated vanadium tetrasulfide nanoparticle material according to claim 1 is characterized in that the temperature during the hydrothermal reaction in step 7) is 140-180°C.
8. The preparation of graphene-coated vanadium tetrasulfide nanoparticle material according to claim 1 is characterized in that the temperature of the vacuum drying oven in step 8) is 50-70°C.
Citation Information
Cited By
Graphite-phase carbon nitride / vanadium disulfide / carbon nanotube ternary heterojunction composite material as well as preparation method and application thereof
CN121244263A